Cathode material, preparation method and application thereof

CN117766707BActive Publication Date: 2026-11-20JIANGSU PYLON BATTERY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311749369.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-18
Publication Date
2026-11-20
Estimated Expiration
2043-12-18

AI Technical Summary

Technical Problem

但该材料仅能实现2e-反应,容量不足且电压较低,能量密度还有待提高

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117766707B_ABST
    Figure CN117766707B_ABST
Patent Text Reader

Abstract

This invention provides a cathode material, its preparation method, and its application, relating to the field of battery technology. The cathode material provided by this invention is mainly composed of a phosphate material and carbon; the chemical formula of the phosphate material is Na. (3+y) Fe (x) Mn (y) Cr (2‑x‑y) (PO4)3, 0 < x, 0.5 ≤ y ≤ 1, x + y < 2; carbon is coated on the surface of the phosphate material. The phosphate material achieves ≥2.5e ‑ Reversible reaction, high material capacity; appropriate amounts of Mn and transition metal Fe help alleviate Mn contamination. 3+ Ginger-Taylor distortion and high potential Cr 3+ / 4+ The resulting cycle life issues; high potential Mn 3+ / Mn 4+ Cr 3+ / Cr 4+ It also compensated for Fe 2+ / Fe 3+ The lower potential, combined with other factors, endows the material with excellent cycle life and high operating voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and in particular to a cathode material, its preparation method, and its application. Background Technology

[0002] Sodium-ion batteries, with their abundant sodium reserves and low cost, are considered an ideal choice for low-speed electric vehicles and large-scale energy storage systems. Sodium fast ion conductor (NASICON) type phosphate cathode materials, with their open three-dimensional structure (lantern-shaped), high thermal stability, and structural diversity, have become a research hotspot. A typical NASICON type Na3V2(PO4)3 / C cathode is based on V... 3+ / V 4+ Redox couple, providing 110 mAh g -1 The specific capacitance is high, and the voltage plateau is 3.4V. However, this material can only achieve 2e... - The reaction has insufficient capacity and low voltage, and the energy density needs to be improved.

[0003] In view of this, the present invention is hereby proposed. Summary of the Invention

[0004] The first objective of this invention is to provide a cathode material to solve at least one of the above-mentioned problems.

[0005] A second objective of this invention is to provide a method for preparing the above-mentioned cathode material.

[0006] A third objective of this invention is to provide the application of the above-mentioned cathode material in the preparation of sodium-ion batteries.

[0007] The fourth objective of this invention is to provide a sodium-ion battery.

[0008] To achieve the above objectives, the following technical solution is proposed:

[0009] In a first aspect, the present invention provides a cathode material, which is mainly composed of phosphate material and carbon;

[0010] The chemical formula of the phosphate material is Na. (3+y) Fe (x) Mn (y) Cr (2-x-y) (PO4)3, 0<x, 0.5≤y≤1, x+y<2;

[0011] The carbon is coated on the surface of the phosphate material.

[0012] As a further technical solution, the chemical formula of the phosphate material is Na. 3.5 Fe 0.5 Mn 0.5 Cr(PO4)3.

[0013] As a further technical solution, the carbon content in the cathode material is 8%-16% by mass.

[0014] Secondly, the present invention provides a method for preparing the above-mentioned cathode material, comprising the following steps:

[0015] The carbon source complexing agent solution is mixed with iron, manganese and chromium sources to carry out a complexation reaction, and then mixed with sodium and phosphorus sources to form a gel. After drying and sintering under a protective atmosphere, the cathode material is prepared.

[0016] As a further technical solution, the carbon source complexing agent includes citric acid;

[0017] The total amount of iron, manganese and chromium in the iron source, manganese source and chromium source is in a molar ratio of 2:3 to 1:2 with citric acid.

[0018] As a further technical solution, the iron source includes at least one of ferric nitrate, ferric phosphate dihydrate, or ferric oxide;

[0019] And / or, the manganese source includes at least one of manganese acetate, manganese nitrate, or manganese acetylacetone;

[0020] And / or, the chromium source includes at least one of chromium nitrate, chromium acetate, or chromium trioxide;

[0021] And / or, the sodium source includes at least one of sodium acetate, sodium carbonate, sodium nitrate, sodium dihydrogen phosphate, or sodium hydroxide;

[0022] And / or, the phosphorus source includes at least one of phosphoric acid or ammonium dihydrogen phosphate.

[0023] As a further technical solution, the gel formation method includes stirring at 75-85°C.

[0024] As a further technical solution, the sintering temperature is 650-700℃;

[0025] The sintering time is 6-10 hours.

[0026] Thirdly, the present invention provides the application of the above-mentioned cathode material in the preparation of sodium-ion batteries.

[0027] Fourthly, the present invention provides a sodium-ion battery, wherein the sodium-ion battery uses the aforementioned positive electrode material as the positive electrode material.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The cathode material provided by this invention is mainly composed of phosphate material and carbon, wherein the phosphate material is produced by Fe...2+ / Fe 3+ Mn 2+ / Mn 3+ / Mn 4+ Cr 3+ / Cr 4+ The reaction couple achieves ≥2.5e - Reversible reactions increase material capacity; appropriate amounts of Mn and transition metal Fe help mitigate Mn contamination. 3+ Ginger-Tyler distortion and high potential Cr 3+ / 4+ The resulting cycle life issues; high potential Mn 3 + / Mn 4+ Cr 3+ / Cr 4+ It also compensated for Fe 2+ / Fe 3+ The relatively low potential, combined with other factors, endows the material with excellent cycle life and high operating voltage. Carbon coating on the phosphate material surface forms an excellent conductive network, which is beneficial to improving the material's electronic conductivity. Furthermore, the preparation process is simple, and most raw materials are inexpensive, supporting the future industrial application prospects of this material. This cathode material can achieve a capacity of 137.6 mAh g. -1 The operating voltage can reach 3.6V, and the capacity retention rate can reach 83.36% after 300 cycles. Attached Figure Description

[0030] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0031] Figure 1 for Na 3.5 Fe 0.5 Mn 0.5 XRD pattern of Cr(PO4)3 / C cathode material;

[0032] Figure 2 for Na 3.5 Fe 0.5 Mn 0.5 SEM and EDS mapping of Cr(PO4)3 / C cathode material;

[0033] Figure 3 for Na 3.5 Fe 0.5 Mn 0.5First-cycle charge-discharge curves of Cr(PO4)3 / C cathode material;

[0034] Figure 4 for Na 3.5 Fe 0.5 Mn 0.5 The dQ / dV curves of the first charge-discharge cycle of Cr(PO4)3 / C cathode material;

[0035] Figure 5 for Na 3.5 Fe 0.5 Mn 0.5 Cycle performance of Cr(PO4)3 / C cathode material. Detailed Implementation

[0036] The embodiments and examples of the present invention will be described in detail below. However, those skilled in the art will understand that the following embodiments and examples are for illustrative purposes only and should not be considered as limiting the scope of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention. Unless otherwise specified, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.

[0037] In a first aspect, the present invention provides a cathode material, which is mainly composed of phosphate material and carbon;

[0038] The chemical formula of the phosphate material is Na. (3+y) Fe (x) Mn (y) Cr (2-x-y) (PO4)3, 0<x, 0.5≤y≤1, x+y<2;

[0039] The carbon is coated on the surface of the phosphate material.

[0040] The cathode material provided by this invention is mainly composed of phosphate material and carbon, wherein the phosphate material is produced by Fe... 2+ / Fe 3+ Mn 2+ / Mn 3+ / Mn 4+ Cr 3+ / Cr 4+ The reaction couple achieves ≥2.5e - Reversible reactions increase material capacity; appropriate amounts of Mn and transition metal Fe help mitigate Mn contamination. 3+ Ginger-Tyler distortion and high potential Cr 3+ / 4+ The resulting cycle life issues; high potential Mn3 + / Mn 4+ Cr 3+ / Cr 4+ It also compensated for Fe 2+ / Fe 3+ The low potential, combined with the material's excellent cycle life and high operating voltage, contributes to its overall superior performance. The carbon coating on the phosphate material forms an excellent conductive network, which helps to improve the material's electronic conductivity. Furthermore, the preparation process is simple and the raw materials are mostly inexpensive, which supports the future industrial application prospects of this material.

[0041] It should be noted that in this invention, Fe has a +3 valence, Mn has a +2 valence, and Cr has a +3 valence.

[0042] In some optional embodiments, the phosphate material has the chemical formula Na. 3.5 Fe 0.5 Mn 0.5 Cr(PO4)3.

[0043] Further optimization and adjustment of the elemental composition of the phosphate material resulted in improved electrochemical performance. The inventors discovered that the optimized phosphate material achieved a capacity of 137.6 mAh g⁻¹. -1 The operating voltage can reach 3.6V, and the capacity retention rate can reach 83.36% after 300 cycles.

[0044] In some alternative embodiments, the carbon content in the cathode material may be, for example, but not limited to, 8%, 10%, 12%, 14%, or 16%.

[0045] In some alternative embodiments, the particle size of the cathode material is 400-600 nm.

[0046] Secondly, the present invention provides a method for preparing the above-mentioned cathode material, comprising the following steps:

[0047] The carbon source complexing agent solution is mixed with iron, manganese and chromium sources to carry out a complexation reaction, and then mixed with sodium and phosphorus sources to form a gel. After drying and sintering under a protective atmosphere, the cathode material is prepared.

[0048] It should be noted that carbon source complexing agents refer to complexing agents that can provide carbon sources. They can act as complexing agents to carry out complexation reactions and also provide carbon sources for the system.

[0049] The preparation method is simple and convenient, and the resulting cathode material has high capacity, high operating voltage, and long cycle life.

[0050] In some optional embodiments, the carbon source complexing agent includes, but is not limited to, citric acid; for example, oxalic acid and other carbon source complexing agents may also be used.

[0051] The total amount of iron, manganese and chromium in the iron source, manganese source and chromium source is in a molar ratio of 2:3 to 1:2 with citric acid.

[0052] By optimizing and adjusting the amounts of iron, manganese, chromium, and citric acid sources, the complexation reaction is made complete, the carbon content is appropriate, and the waste of raw materials is avoided.

[0053] In some alternative implementations, 40-60 mL of deionized water is used as a solvent for every 1 mol of cathode material synthesized.

[0054] In some alternative embodiments, the iron source includes, but is not limited to, at least one of ferric nitrate, ferric phosphate dihydrate, or ferric oxide.

[0055] In some alternative embodiments, the manganese source includes, but is not limited to, at least one of manganese acetate, manganese nitrate, or manganese acetylacetone.

[0056] In some alternative embodiments, the chromium source includes, but is not limited to, at least one of chromium nitrate, chromium acetate, or chromium trioxide.

[0057] In some alternative embodiments, the sodium source includes, but is not limited to, at least one of sodium acetate, sodium carbonate, sodium nitrate, sodium dihydrogen phosphate, or sodium hydroxide.

[0058] In some alternative embodiments, the phosphorus source includes, but is not limited to, at least one of phosphoric acid or ammonium dihydrogen phosphate.

[0059] In some alternative embodiments, the gel formation process includes stirring at 75-85°C. This condition helps to improve the efficiency of gel formation.

[0060] In some alternative embodiments, the sintering temperature may be, for example, but not limited to, 650°C, 660°C, 670°C, 680°C, 690°C, or 700°C;

[0061] The sintering time can be, for example, but not limited to, 6h, 7h, 8h, 9h or 10h.

[0062] Sintering can improve the crystallinity of the material and carbonize the carbon source complexing agent, coating it on the surface of the cathode material.

[0063] In some alternative embodiments, the protective atmosphere includes, but is not limited to, nitrogen, argon, or argon-hydrogen, and mixtures thereof.

[0064] In some preferred embodiments, grinding is also included separately before drying and sintering. Grinding is used to obtain cathode materials with suitable particle size.

[0065] Thirdly, the present invention provides the application of the above-mentioned cathode material in the preparation of sodium-ion batteries.

[0066] The cathode material provided by this invention has high capacity, high operating voltage, and long cycle life, and can be used to prepare battery cathode sheets, thereby preparing sodium-ion batteries.

[0067] Fourthly, the present invention provides a sodium-ion battery, wherein the sodium-ion battery uses the aforementioned positive electrode material as the positive electrode material.

[0068] For example, the positive electrode material, conductive agent SP (conductive carbon black), and binder PVDF (polyvinylidene fluoride) provided by this invention are mixed in a weight ratio of 8:1:1 to form a positive electrode slurry, which is then uniformly coated onto the surface of aluminum foil to prepare a positive electrode sheet. The negative electrode sheet can be a commercially available sodium sheet, combined with a 1M NaClO4 / PC electrolyte. A CR2032 battery can be assembled by matching the following components in the order of negative electrode shell, sodium sheet, separator, electrolyte, positive electrode sheet, gasket, spring, and positive electrode shell.

[0069] The present invention will be further illustrated below with specific embodiments and comparative examples. However, it should be understood that these embodiments are merely for the purpose of more detailed illustration and should not be construed as limiting the present invention in any way.

[0070] Example 1

[0071] A type of Na 3.5 Fe 0.5 Mn 0.5 The preparation method of Cr(PO4)3 / C cathode material is as follows:

[0072] Citric acid, used as a complexing agent and carbon source, was added to an appropriate amount of deionized water (40-60 mL of deionized water corresponds to the synthesis of 1 mol of the target cathode material) and stirred until homogeneous. Then, iron, manganese, and chromium sources were added to the citric acid solution according to their stoichiometric ratio, and the mixture was stirred for 1 hour to allow for a complete complexation reaction. The stoichiometric ratio of citric acid to transition metal elements was 3:2. Subsequently, sodium and phosphorus sources were added, and stirring continued for 30 minutes before being transferred to an 80°C hot water bath for further stirring until a gel was formed. After homogeneous grinding, the mixture was dried in a forced-air drying oven at 110°C for 8 hours. Following grinding, it was sintered in a tube furnace under N2 at 670°C for 8 hours, with a heating rate of 5°C / min. -1 Na 3.5 Fe 0.5 Mn 0.5 Cr(PO4)3 / C.

[0073] The iron source is ferric nitrate; the manganese source is manganese acetate; the chromium source is chromium nitrate; the sodium source is sodium acetate; and the phosphorus source is phosphoric acid.

[0074] Example 2

[0075] A Na4Fe 0.1 MnCr 0.9 The (PO4)3 / C cathode material differs from that in Example 1 in that the phosphate material is Na4Fe. 0.1 MnCr 0.9 (PO4)3.

[0076] Example 3

[0077] A type of Na 3.5 FeMn 0.5 Cr 0.5 The (PO4)3 / C cathode material differs from that in Example 1 in that the phosphate material is Na. 3.5 FeMn 0.5 Cr 0.5 (PO4)3.

[0078] Comparative Example 1

[0079] A type of Na 3.5 Mn 0.5 Cr 1.5 The (PO4)3 / C cathode material differs from that in Example 1 in that the phosphate material is Na. 3.5 Mn 0.5 Cr 1.5 (PO4)3.

[0080] Comparative Example 2

[0081] A Na3Fe 0.5 Cr 1.5 The (PO4)3 / C cathode material differs from that in Example 1 in that the phosphate material is Na3Fe. 0.5 Cr 1.5 (PO4)3.

[0082] Comparative Example 3

[0083] A type of Na 3.3 Fe 1.7 Mn 0.3 The (PO4)3 / C cathode material differs from that in Example 1 in that the phosphate material is Na. 3.3 Fe 1.7 Mn 0.3 (PO4)3.

[0084] Comparative Example 4

[0085] A Na3Fe2(PO4)3 / C cathode material differs from Example 1 in that the phosphate material is Na3Fe2(PO4)3.

[0086] Comparative Example 5

[0087] A Na3Cr2(PO4)3 / C cathode material differs from Example 1 in that the phosphate material is Na3Cr2(PO4)3.

[0088] Comparative Example 6

[0089] A Na4MnCr(PO4)3 / C cathode material differs from Example 1 in that the phosphate material is Na4MnCr(PO4)3.

[0090] Comparative Example 7

[0091] A Na3FeCr(PO4)3 / C cathode material differs from Example 1 in that the phosphate material is Na3FeCr(PO4)3.

[0092] Experimental Example 1

[0093] 1. XRD pattern analysis was performed on the cathode material of Example 1, such as... Figure 1 As shown, comparing the XRD pattern with the standard diffraction card reveals fewer impurity peaks, indicating that it is a pure phase and the material has good crystallinity.

[0094] 2. The cathode material provided in Example 1 was subjected to SEM morphology analysis, such as... Figure 2 As shown, the SEM morphology image indicates that the particle size of the material is approximately 400-600 nm, and the EDS mapping image shows that all elements are evenly distributed, indicating that the target material was successfully synthesized.

[0095] 3. The positive electrode materials provided in Examples 1-3 and Comparative Examples 1-8 were mixed with conductive agent SP and binder PVDF in a weight ratio of 8:1:1 to prepare a positive electrode slurry, which was then uniformly coated onto the surface of aluminum foil to prepare a positive electrode sheet. A commercially available sodium sheet was used as the negative electrode sheet, along with a 1M NaClO4 / PC electrolyte. The CR2032 battery was assembled in the following order: negative electrode shell, sodium sheet, separator, electrolyte, positive electrode sheet, gasket, spring sheet, and positive electrode shell.

[0096] The performance of the above batteries was tested. For the positive electrode specific capacity test, the mass w of the positive electrode material was recorded before preparing the CR2032 battery. Then, the battery was charged at a constant current rate of 0.1C to the upper limit voltage (the upper limit voltage for Examples 1-3, Comparative Examples 1-2, and Comparative Examples 6-7 was set to 4.5V; for Comparative Example 3, it was set to 4.3V; for Comparative Example 4, it was set to 3.5V; and for Comparative Example 5, it was set to 4.7V), and then discharged at a constant current rate of 0.1C to 1.9V. The discharge capacity C1 was recorded. The calculation method was positive electrode specific capacity = C1 / w. For the cycle performance test, the prepared battery was charged at a constant current rate of 1C to the upper limit voltage, and then discharged at a constant current rate of 1C to 1.9V. The discharge capacity C2 was recorded. After 300 charge-discharge cycles, the discharge capacity C3 of the 300th discharge was recorded. The calculation method was cycle capacity retention = C3 / C2 × 100%. The results are shown in Table 1.

[0097] Table 1

[0098]

[0099] The results show that the battery prepared using the cathode material of Example 1 (test results are as follows) Figures 3-5 As shown), its charge-discharge curves show Na 3.5 Fe 0.5 Mn 0.5 The Cr(PO4)3 / C material exhibits a discharge capacity of 137.6 mAh g⁻¹ within an electrochemical window of 1.9–4.5 V. -1 The average operating voltage is 3.6V. The corresponding dQ / dV curve shows that the material successfully excited Mn during the first charge. 2+ / 3+ / 4+ Cr 3+ / 4+ Redox couple; Fe added during discharge 3+ / 2+ This will enable the material to subsequently possess 2.5e - Redox capability. After 300 cycles, the material retains 83.36% of its capacity.

[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A positive electrode material, characterized in that, It is mainly composed of phosphate materials and carbon; The chemical formula of the phosphate material is Na. 3.5 Fe 0.5 Mn 0.5 Cr(PO4)3; The carbon is coated on the surface of the phosphate material; The mass percentage of carbon in the cathode material is 8%-16%; The method for preparing the cathode material includes the following steps: The carbon source complexing agent solution is mixed with iron, manganese and chromium sources to carry out a complexation reaction, and then mixed with sodium and phosphorus sources to form a gel. After drying and sintering under a protective atmosphere, the cathode material is prepared. The carbon source complexing agent includes citric acid; The total amount of iron, manganese and chromium in the iron source, manganese source and chromium source is in a molar ratio of 2:3 to 1:2 with citric acid.

2. The cathode material according to claim 1, characterized in that, The iron source includes at least one of ferric nitrate, ferric phosphate dihydrate, or ferric oxide. And / or, the manganese source includes at least one of manganese acetate, manganese nitrate, or manganese acetylacetone; And / or, the chromium source includes at least one of chromium nitrate, chromium acetate, or chromium trioxide; And / or, the sodium source includes at least one of sodium acetate, sodium carbonate, sodium nitrate, sodium dihydrogen phosphate, or sodium hydroxide; And / or, the phosphorus source includes at least one of phosphoric acid or ammonium dihydrogen phosphate.

3. The cathode material according to claim 1, characterized in that, The gel is formed by stirring at 75-85°C.

4. The cathode material according to claim 1, characterized in that, The sintering temperature is 650-700℃; The sintering time is 6-10 hours.

Citation Information

Patent Citations

  • Positive electrode material for transition metal-doped sodium ion battery and preparation and application thereof

    CN109755565A

  • Transition metal doped titanium manganese sodium phosphate / carbon composite positive electrode material, preparation thereof and application in sodium ion battery

    CN110611080A