Negative electrode material and preparation method thereof, and lithium ion battery

By preparing highly uniform porous carbonaceous materials through a two-stage activation process, the problem of uneven distribution of silicon materials within the pores was solved, thereby improving the performance of the anode material, especially its expansion performance, cycle performance, and capacity.

CN117766745BActive Publication Date: 2026-11-24BTR NEW MATERIAL GRP CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311591084.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-24
Publication Date
2026-11-24
Estimated Expiration
2043-11-24

AI Technical Summary

Technical Problem

The existing biomass process for preparing porous carbonaceous materials results in uneven activation, leading to fewer or no pores in the silicon material during deposition, causing expansion, cycle and rate performance degradation of the anode material.

Method used

By employing a two-stage activation process and adjusting the activation dosage and time, porous carbonaceous materials with a uniformity N≥80% were prepared, ensuring that silicon material is mainly distributed within the pores, forming a stable SEI film and improving structural stability.

Benefits of technology

It improves the expansion performance, cycle performance and capacity of the anode material, suppresses the volume effect of silicon material during lithium insertion/deintercalation, and reduces particle pulverization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117766745B_ABST
    Figure CN117766745B_ABST
Patent Text Reader

Abstract

This application relates to an anode material and its preparation method, and a lithium-ion battery. The anode material includes a porous carbon material, in which silicon material is distributed. The anode material has a uniformity N, where N ≥ 80%. In the backscattered electron image obtained by scanning the anode material using a scanning electron microscope in BSE automatic brightness and contrast mode, the number of anode material particles with a first brightness in any 100μm*100μm region is denoted as C1, where the first brightness represents anode material with a gray value greater than or equal to 5500 in the backscattered electron image. The number of anode material particles with a second brightness is denoted as C2, where the second brightness represents anode material with a gray value less than 5500 in the backscattered electron image. The uniformity N' of the anode material in the above region is N' = C2 / (C2+C1)*100%, and the uniformity N of the anode material is the arithmetic mean of at least 10 N's.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of negative electrode material technology, specifically, it relates to negative electrode materials and their preparation methods, and lithium-ion batteries. Background Technology

[0002] Silicon-based anode materials possess advantages such as high specific capacity, low voltage plateau, environmental friendliness, and abundant resources, making them a promising replacement for graphite anodes in next-generation high-energy-density lithium-ion batteries. However, silicon undergoes significant volume changes during the insertion / extraction process, which can easily lead to particle pulverization and subsequent detachment from the current collector. Furthermore, the repeated volume changes of silicon materials during electrochemical cycling cause the SEI film formed on the silicon surface to continuously break down and regenerate, resulting in continuous lithium-ion consumption and ultimately rapid capacity decay.

[0003] Improving the processes of silicon anode materials through nano-sizing, carbon coating, and polymer coating can suppress the volume expansion of silicon to some extent. Typically, silicon is deposited in porous carbon to suppress volume expansion. Biomass methods are currently the mainstream preparation method for porous carbon materials. However, existing biomass-based porous carbon preparation processes generally suffer from uneven activation, with more or less particles lacking pores (or not being activated). During silicon deposition, these particles, lacking activation, result in few or no pores, making it easy for silicon to deposit on the particle surface, thus degrading the expansion performance, cycle performance, and rate performance of the anode material.

[0004] Therefore, there is an urgent need to provide a silicon anode material with low expansion, high cycling performance, and high rate capability. Summary of the Invention

[0005] This application provides an anode material and its preparation method, as well as a lithium-ion battery, which can improve the expansion performance, cycle performance, and rate performance of the anode material.

[0006] To achieve the above objectives, the first technical solution of this application is as follows: This application provides a negative electrode material comprising a porous carbonaceous material, wherein silicon material is distributed within the porous carbonaceous material, and the negative electrode material has a uniformity N, where N ≥ 80%. In the backscattered electron image obtained by scanning electron microscopy (SEM) of the anode material in BSE automatic brightness and contrast mode, at any 100 μm... Within a 100μm region, the number of particles of the negative electrode material with a first brightness is denoted as C1. Particles of the negative electrode material with the first brightness represent negative electrode materials with a grayscale value greater than or equal to 5500 in the backscattered electron image. The number of particles of the negative electrode material with a second brightness is denoted as C2. Particles of the negative electrode material with the second brightness represent negative electrode materials with a grayscale value less than 5500 in the backscattered electron image. The uniformity of the negative electrode material within the aforementioned region is N' = C2 / (C2 + C1). 100%, the uniformity N of the negative electrode material is the arithmetic mean of the uniformity N' of at least 10 of the aforementioned regions.

[0007] In some embodiments, the negative electrode material includes at least one of the following features (1) to (7): (1) The silicon material is also distributed on at least a portion of the surface of the porous carbonaceous material; (2) The porous carbonaceous material includes at least one of hard carbon, soft carbon, graphite, mesophase carbon microspheres, activated carbon and carbon gel; (3) The porous carbonaceous material includes micropores, and with the total number of pores in the porous carbonaceous material being 100%, the pore volume of the porous carbonaceous material and the proportion of the number of micropores in the porous carbonaceous material are greater than or equal to 80%; (4) The average pore diameter of the porous carbonaceous material is less than or equal to 5 nm; (5) The silicon material includes crystalline silicon and silicide SiO2. x At least one of amorphous silicon and silicon alloys, wherein 0 < x ≤ 2; (6) The silicon material accounts for 30% to 80% of the mass of the negative electrode material; (7) The median particle size of the silicon material is 0.1 nm to 500 nm.

[0008] In some embodiments, the negative electrode material further includes a coating layer covering at least a portion of the surface of the porous carbonaceous material, and the negative electrode material includes at least one of the following features (1) to (4): (1) The coating layer includes a carbon layer, and the material of the carbon layer includes at least one of graphene, soft carbon, hard carbon and conductive polymer; (2) The coating layer includes a metal oxide layer, and the material of the metal oxide layer includes at least one of titanium oxide, aluminum oxide, lithium oxide, cobalt oxide and vanadium oxide; (3) The coating layer includes a nitride layer, and the material of the nitride layer includes at least one of titanium nitride, vanadium nitride, cobalt nitride, nickel nitride and carbon nitride; (4) The thickness of the coating layer is 0.1 nm ~ 100 nm.

[0009] In some embodiments, the negative electrode material includes at least one of the following features (1) to (4): (1) The pore volume of the porous carbonaceous material is greater than or equal to 0.4 cm³. 3 / g; (2) The median particle size of the negative electrode material is less than or equal to 10 μm; (3) The specific surface area of ​​the negative electrode material is less than 5 m². 2 / g; (4) The conductivity of the negative electrode material is greater than or equal to 10. -1 S / m.

[0010] The second technical solution of this application is as follows: This application provides a method for preparing a negative electrode material, including the following steps: The carbon-based carbonized material is mixed with a first activator and subjected to a first activation treatment to obtain the activated material. The activating material is mixed with the second activator for a second activation treatment to obtain a porous carbonaceous material. The amount of the first activator added is 4 to 10 times that of the second activator added, and the time of the first activation treatment is longer than that of the second activation treatment. The porous carbonaceous material and silicon source are mixed and heat-treated to obtain the negative electrode material.

[0011] In some embodiments, the preparation method includes at least one of the following features (1) to (10): (1) The first activator includes an alkaline substance, and the mass ratio of the carbon-based carbonized material to the first activator is 1:(0.5~30). (2) The second activator includes an alkaline substance, and the mass ratio of the carbon-based carbonized material to the second activator is 1:(0.1~10). (3) The first activator includes at least one of water vapor, oxygen and air, and the concentration of the first activator is 3% to 20%; (4) The second activator includes at least one of water vapor, oxygen and air, and the concentration of the second activator is 0.1% to 5%; (5) The first activator includes an alkaline substance, which includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide and rubidium hydroxide; (6) The second activator includes an alkaline substance, which includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide and rubidium hydroxide; (7) The activation time for the first activation treatment is 5h~20h; (8) The second activation treatment time is 3h~10h; (9) The temperature of the first activation treatment is 900℃~1200℃; (10) The temperature of the second activation treatment is 800℃~1000℃.

[0012] In some embodiments, the preparation method includes at least one of the following features (1) to (5): (1) The carbon-based carbonized material is obtained by carbonizing carbon-based raw materials, wherein the carbon-based raw materials include at least one of lignin, coconut shell, fruit shell, peanut shell, rice shell, coal-derived biomass and resin; (2) The carbon-based carbonized material is obtained by carbonizing carbon-based raw materials, and the carbonization temperature is 400℃~900℃; (3) The carbon-based carbonized material is obtained by carbonizing carbon-based raw materials, and the carbonization time is 1h~20h; (4) The carbon-based carbonized material is obtained by carbonizing carbon-based raw materials. The carbonization is carried out under a protective gas atmosphere, and the protective gas includes at least one of nitrogen, helium, neon, argon, krypton and xenon. (5) Before the first activation treatment of mixing the carbon-based carbon material with the first activator, the method further includes the step of acid washing the carbon-based carbon material.

[0013] In some embodiments, the preparation method includes at least one of the following features (1) to (4): (1) The silicon source includes silane; (2) The flow rate of the silicon source is 0.1 L / min ~ 1000 L / min; (3) The temperature of the heat treatment is 300℃~800℃; (4) The heat treatment time is 2h~25h.

[0014] In some embodiments, after heat treatment of the porous carbonaceous material and silicon source, the mixture is further heat-treated by mixing the heat-treated material with the coating material. The preparation method includes at least one of the following features (1) to (10): (1) The coating material includes at least one of carbon source, metal oxide and nitride; (2) The coating material includes at least one of carbon source, metal oxide and nitride, wherein the carbon source includes at least one of gaseous carbon source and solid carbon source; (3) The coating material includes at least one of carbon source, metal oxide and nitride, wherein the carbon source includes at least one of gaseous carbon source and solid carbon source, and the gaseous carbon source includes at least one of acetylene, methane, propylene, benzene, ethanol, methanol, ethylene, propane and butane; (4) The coating material includes at least one of carbon source, metal oxide and nitride, wherein the carbon source includes at least one of gaseous carbon source and solid carbon source, and the flow rate of the gaseous carbon source is 0.1 L / min ~ 1000 L / min; (5) The coating material includes at least one of carbon source, metal oxide and nitride, wherein the carbon source includes at least one of gaseous carbon source and solid carbon source, and the solid carbon source includes at least one of sucrose, fructose, glucose, asphalt, phenolic resin, polyimide, citric acid, epoxy resin, amino resin, polystyrene, polyacrylic acid, carboxymethyl cellulose and cellulose acetate butyrate. (6) The coating material includes at least one of carbon source, metal oxide and nitride, the carbon source includes at least one of gas carbon source and solid carbon source, and the mass ratio of solid carbon source to negative electrode material is (1~100):100; (7) The coating material includes at least one of carbon source, metal oxide and nitride, wherein the metal oxide includes at least one of iron oxide, zinc oxide, tin oxide, copper oxide and titanium oxide; (8) The coating material includes at least one of a carbon source, a metal oxide, and a nitride, wherein the nitride includes at least one of titanium nitride, vanadium nitride, cobalt nitride, nickel nitride, and carbon nitride; (9) The temperature of the heat treatment is 600℃~1100℃; (10) The heat treatment holding time is 2h~10h.

[0015] The third technical solution of this application is as follows: This application provides a lithium-ion battery, which includes the negative electrode material described in the first aspect or the negative electrode material prepared by the preparation method described in the second aspect.

[0016] The technical solution of this application has at least the following beneficial effects: The negative electrode material of this application comprises porous carbonaceous material and silicon material, and the negative electrode material has a uniformity N, where N ≥ 80%. This indicates that the negative electrode material of this application mainly exists in the form of particles with a gray value less than 5500 in the backscattered electron image. Particles with a gray value less than 5500 in the backscattered electron image indicate that the silicon material in the negative electrode material particles is mainly distributed within the pores of the porous carbonaceous material, and the distribution is uniform. In other words, in this application, taking the total number of negative electrode material particles as 100%, the proportion of silicon particles uniformly distributed within the pores of the porous carbonaceous material is greater than or equal to 80%. This indicates that the porous carbonaceous material of this application has uniformly distributed activation pores, and the number of activation pores is appropriate, allowing the silicon material to be mainly distributed within the pores of the porous carbonaceous material, resulting in a high silicon deposition rate. Furthermore, this application is based on any 100μm... The negative electrode materials obtained from testing within a 100μm region show that the number and distribution of activated pores in the porous carbonaceous material of each negative electrode material particle in this application are highly similar. That is, the negative electrode material in this application has a porous carbonaceous material with good consistency. The porous carbonaceous material with good consistency can improve the dispersion of silicon material in the negative electrode material, suppress the volume effect caused by the agglomeration of silicon material during lithium insertion / deintercalation, and reduce the pulverization of negative electrode material particles. At the same time, during the lithium insertion / deintercalation process, the SEI film is formed in a limited space, which is conducive to the formation of a stable SEI film, improves the structural stability of the negative electrode material, and thus improves the expansion performance, cycle performance and capacity of the negative electrode material. Attached Figure Description

[0017] The present application will be further described below with reference to the accompanying drawings and embodiments.

[0018] Figure 1 This is a flowchart illustrating the preparation process of the negative electrode material in this application; Figure 2 This is a SEM image of the negative electrode material prepared in Example 1 of this application; Figure 3 The image shows the XRD pattern of the negative electrode material prepared in Example 1 of this application. Figure 4 The first charge-discharge curve of the negative electrode material prepared in Example 1 of this application; Figure 5 The cycling performance curve of the negative electrode material prepared in Example 1 of this application. Detailed Implementation

[0019] To better understand the technical solution of this application, the embodiments of this application will be described in detail below with reference to the accompanying drawings.

[0020] It should be understood that the described embodiments are merely some, not all, of the embodiments in this application. All other embodiments obtained by those skilled in the art based on the embodiments in this application without inventive effort are within the scope of protection of this application.

[0021] The terminology used in the embodiments of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of this application. The singular forms “a,” “the,” and “the” used in the embodiments of this application and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise.

[0022] It should be understood that the term "and / or" used in this article is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this article generally indicates that the preceding and following related objects have an "or" relationship.

[0023] Biomass is currently the mainstream method for preparing porous carbonaceous materials. However, existing biomass processes generally result in uneven activation of porous carbonaceous materials, with some particles lacking pores (and thus not being activated). These particles, due to their lack of activation during silicon deposition, result in few or no pores, leading to less or almost no silicon deposition and deterioration of the anode material's performance.

[0024] This application provides a negative electrode material, including a porous carbonaceous material, in which silicon material is distributed internally, and the negative electrode material has a uniformity N, where N ≥ 80%; In the backscattered electron image obtained by scanning the anode material using a Hitachi S4800 SEM in BSE automatic brightness and contrast mode, at any 100 μm... Within a 100μm region, the number of negative electrode material particles with the first brightness is denoted as C1. Negative electrode material with the first brightness represents negative electrode material with a grayscale value greater than or equal to 5500 in the backscattered electron image. The number of negative electrode material particles with the second brightness is denoted as C2. Negative electrode material with the second brightness represents negative electrode material with a grayscale value less than 5500 in the backscattered electron image. The uniformity of the negative electrode material within the above region is N' = C2 / (C2 + C1). 100%, the uniformity N of the negative electrode material is the arithmetic mean of the uniformity N' of at least 10 of the above regions.

[0025] In the above scheme, the negative electrode material of this application includes porous carbonaceous material and silicon material, and the negative electrode material has a uniformity N, where N≥80%. This indicates that the negative electrode material of this application mainly exists in the form of particles with a gray value less than 5500 in the backscattered electron image. Particles with a gray value less than 5500 in the backscattered electron image indicate that the silicon material in the negative electrode material particles is mainly distributed within the pores of the porous carbonaceous material, and the distribution is uniform. In other words, in this application, taking the total number of negative electrode material particles as 100%, the proportion of silicon particles uniformly distributed within the pores of the porous carbonaceous material is greater than or equal to 80%. This indicates that the porous carbonaceous material of this application has uniformly distributed activation pores, and the number of activation pores is appropriate, allowing the silicon material to be mainly distributed within the pores of the porous carbonaceous material, resulting in a high silicon deposition rate. Furthermore, this application is based on any 100μm... The negative electrode materials obtained from testing within a 100μm region show that the number and distribution of activated pores in the porous carbonaceous material of each negative electrode material particle in this application are highly similar. That is, the negative electrode material in this application has a porous carbonaceous material with good consistency. The porous carbonaceous material with good consistency can improve the dispersion of silicon material in the negative electrode material, suppress the volume effect caused by the agglomeration of silicon material during lithium insertion / deintercalation, and reduce the pulverization of negative electrode material particles. At the same time, during the lithium insertion / deintercalation process, the SEI film is formed in a limited space, which is conducive to the formation of a stable SEI film, improves the structural stability of the negative electrode material, and thus improves the expansion performance, cycle performance and capacity of the negative electrode material.

[0026] Due to the significant difference in electrical conductivity between carbon and silicon, under scanning electron microscopy (SEM) with backscattered electrons (BSE) in automatic brightness and contrast mode, anode material particles with higher conductivity are typically darker in color. This indicates that the silicon deposition in the porous carbonaceous material is less, or there is no silicon deposition at all, resulting in darker-colored particles. Conversely, anode material particles with lower conductivity are typically brighter in color. This indicates that the silicon material is mainly deposited in porous silicon-carbonaceous materials with uniform pore distribution, resulting in brighter-colored particles, often appearing bright white. This application uses a grayscale value of 5500 as the criterion for determining whether the material particle color is dark or bright. Anode materials with a grayscale value greater than or equal to 5500 indicate a darker surface, meaning the material particles have a first level of brightness. Material particles with this first level of brightness indicate that less silicon material is deposited inside the anode material particles, meaning the amount of silicon deposited is relatively small. A negative electrode material with a gray value less than 5500 indicates that the material surface is relatively bright, that is, the material particles have a second brightness. Material particles with a second brightness indicate that the silicon material is mainly deposited in the porous silicon-carbon material with uniform pore distribution, and the amount of silicon deposited is relatively large, that is, a large amount of silicon is deposited inside the negative electrode material particles.

[0027] In this application, the uniformity N was tested and calculated using a Hitachi S4800 SEM scanning electron microscope. Specifically, the negative electrode material particles were scanned using the scanning electron microscope (SEM) in BSE automatic brightness and contrast mode, and the scanned image was converted into a grayscale image. The grayscale image was then processed using ImageJ image processing software. Specifically, the grayscale image was opened using ImageJ image processing software, and the particle area for which the grayscale value needed to be calculated was selected using the "selection box" tool. The selected area was any 100 μm. A 100μm area is formed. Then, press Ctrl+1 and Ctrl+3 sequentially to obtain the grayscale variation curves of all particles. Next, use the line tool (rectangular or rounded rectangular selection) to draw perpendicular lines to the horizontal axis at each trough point, forming multiple closed shapes below the grayscale variation curves. Finally, use the wand (tracing) tool to select each closed shape except for the beginning and end, obtaining the total grayscale value of each shape, which is considered the grayscale value of the multiple particles in the selected area. Repeat the above steps to obtain the uniformity N' of at least 10 selected areas. Then, calculate the uniformity N by averaging the uniformity N' of all selected areas.

[0028] In some embodiments, N can be, for example, 80%, 86%, 88%, 90%, 93%, 95%, 97%, 99%, and 100%, etc., and of course, other values ​​within the above range are also possible, which are not limited herein. Within the above-defined range, it indicates that the porous carbonaceous material has a suitable number and uniformly distributed activation pores, allowing silicon material to be mainly distributed within the pores of the porous carbonaceous material, resulting in a higher silicon content in the negative electrode material. The negative electrode material is also brighter in the automatic brightness and contrast mode of scanning electron microscopy (SEM-backscattered electrons (BSE)). If N is less than 80%, it indicates poor uniformity of activation pore distribution in the porous carbonaceous material, with a certain number of particles having few or no activation pores, leading to less or almost no silicon material deposition inside the porous carbonaceous material, thereby causing deterioration of the negative electrode material performance. Preferably, the uniformity is 86% ≤ N ≤ 99%.

[0029] In some embodiments, silicon material is also distributed on at least a portion of the surface of the porous carbonaceous material.

[0030] In some embodiments, the porous carbonaceous material includes at least one of hard carbon, soft carbon, graphite, mesophase carbon microspheres, activated carbon, and carbon gel.

[0031] In some embodiments, the porous carbonaceous material includes micropores, which are pores with a diameter of less than 2 nm. Micropores are activated pores, which are beneficial for the filling of silicon material. The silicon material filling the micropores can ensure the structural compactness of the porous carbonaceous material, so that the structure of the negative electrode material will not collapse during the compaction process of electrode preparation.

[0032] In some embodiments, taking the total number of pores in the porous carbonaceous material as 100%, the proportion of micropores is greater than or equal to 80%, specifically 80%, 85%, 90%, 92%, 95%, 97%, or 99%, etc., and of course, other values ​​within the above range are also possible, which are not limited herein. Within the above-defined range, it indicates that there is a relatively large number of activated pores in this application. Activated pores have an energy storage function, which can reduce the diffusion resistance of the electrolyte and improve the capacity performance and rate performance of the negative electrode material. Preferably, the proportion of micropores in the porous carbonaceous material is greater than or equal to 90%, more preferably, the proportion of micropores in the porous carbonaceous material is greater than or equal to 92%. In this application, the number of micropores is determined by nitrogen desorption. If the number of micropores in the porous carbonaceous material is less than 80%, it indicates that the number of micropores in the porous carbon is small, the silicon material filling amount is small, which is not conducive to improving the capacity performance of the negative electrode material.

[0033] In some embodiments, the average pore size of the porous carbonaceous material is less than or equal to 5 nm, for example, it can be 1 nm, 1.3 nm, 1.8 nm, 2 nm, 3 nm, 4 nm, or 5 nm, etc., and of course, it can be other values ​​within the above range, which are not limited herein. Preferably, the average pore size of the porous carbonaceous material is less than or equal to 2 nm, and more preferably, the average pore size of the porous carbonaceous material is less than or equal to 1.8 nm.

[0034] In some embodiments, the silicon material includes crystalline silicon and silicon-oxygen material SiO2. x At least one of amorphous silicon and silicon alloys, wherein the silicon oxide material includes silicon oxide (SiO2). x Where 0 < x ≤ 2, silicon oxide is a silicon-oxygen complex containing oxygen atoms and silicon atoms, with a molar ratio of oxygen atoms to silicon atoms of 0 to 2, excluding 0. It can be Si, SiO₂, etc. 0.2 SiO 0.5 SiO 0.8 SiO, SiO 1.2 SiO 1.5 SiO 1.8 It may be a substance composed of two or more of the following: SiO2, or a substance with the chemical formula SiO2. x The compounds can, of course, be other values ​​within the above range, and this application does not impose any restrictions on them.

[0035] In some embodiments, the mass percentage of silicon material in the anode material is 30% to 80%, specifically 30%, 40%, 50%, 60%, 70%, and 80%, etc., and of course, other values ​​within the above range are also possible. This application does not impose any restrictions on this. Within the above-defined range, the mass percentage of silicon material in the anode material is relatively high, which is beneficial to improving the capacity of the anode material.

[0036] In some embodiments, the median particle size of the silicon material is 0.1 nm to 500 nm, for example, it can be 0.1 nm, 1 nm, 5 nm, 10 nm, 30 nm, 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, or 500 nm, etc., and of course, it can also be other values ​​within the above range, which are not limited herein. Within the above-defined range, it is beneficial to buffer the stress and deformation generated in the silicon material during the lithium ion insertion and extraction process, thereby improving the capacity and cycle performance of the anode material. Preferably, the median particle size of the silicon material is 0.1 nm to 10 nm, more preferably, the median particle size of the silicon material is 0.1 nm to 5 nm.

[0037] In some embodiments, the negative electrode material further includes a coating layer distributed on at least a portion of the surface of the porous carbonaceous material. The coating layer can, on the one hand, reduce the risk of electrolyte entering the negative electrode material and causing side reactions that lead to a decrease in initial efficiency and capacity; on the other hand, the coating layer can work synergistically with the porous carbonaceous material to mitigate the volume expansion of silicon, thereby reducing the overall volume expansion of the negative electrode material and minimizing electrode sheet swelling.

[0038] In some embodiments, the coating layer is at least one of a carbon layer, a metal oxide layer, and a nitride layer.

[0039] In some embodiments, the carbon layer is made of at least one of graphene, soft carbon, hard carbon, and conductive polymers. Specifically, the conductive polymers include at least one of polyaniline, polyacetylene, polypyrrole, polythiophene, poly-3-hexylthiophene, poly(p-phenylenevinylene), polypyridine, and polyphenylenevinylene.

[0040] In some embodiments, the metal oxide layer includes at least one of titanium oxide, aluminum oxide, lithium oxide, cobalt oxide, and vanadium oxide.

[0041] In some embodiments, the nitride layer includes at least one of titanium nitride, vanadium nitride, cobalt nitride, nickel nitride, and carbon nitride.

[0042] In some embodiments, the thickness of the coating layer is 0.1 nm to 100 nm, specifically 0.1 nm, 1 nm, 10 nm, 30 nm, 50 nm, 70 nm, 90 nm and 100 nm, etc., and of course other values ​​within the above range are also possible, which are not limited here.

[0043] In some embodiments, the pore volume of the porous carbonaceous material is greater than or equal to 0.4 cm³. 3 / g, for example, could be 0.4 cm 3 / g, 0.5 cm 3 / g, 0.7 cm 3 / g, 1.0 cm 3 / g, 1.5 cm 3 / g, 2.0 cm 3 / g, 2.5 cm 3 / g、3 cm 3 / g, 3.5 cm 3 / g or 5.0 cm 3 / g, etc., can also be other values ​​within the above range, and this application does not impose any limitations on them. Within the above-defined range, it indicates that the porous carbonaceous material of this application has a large number of activated pores, which is beneficial for depositing more silicon material and improving the capacity performance of the anode material. Preferably, the pore volume of the porous carbonaceous material is greater than or equal to 0.5 cm³. 3 / g, more preferably, the pore volume of the porous carbonaceous material is greater than or equal to 0.7 cm³. 3 / g.

[0044] In some embodiments, the median particle size of the negative electrode material is less than or equal to 10 μm, for example, it can be 1 μm, 3 μm, 5 μm, 7 μm, 9 μm, or 10 μm, etc., and of course, it can be other values ​​within the above range, which are not limited herein. Controlling the median particle size of the negative electrode material within the above range is beneficial to improving the cycle performance of the negative electrode material.

[0045] In some implementations, the specific surface area of ​​the negative electrode material is less than 5 m². 2 / g, for example, could be 1 m 2 / g、2 m 2 / g、3 m 2 / g、4 m 2 / g or 4.5 m 2 / g, etc., can also be other values ​​within the above range, and this application does not impose any restrictions. Understandably, controlling the specific surface area of ​​the negative electrode material within the above range can suppress the volume expansion of the negative electrode material and is beneficial to improving the cycle performance of the negative electrode material.

[0046] In some embodiments, the conductivity of the negative electrode material is greater than or equal to 10. -1 S / m, for example, could be 10 -1 Within the ranges of S / m, 0.5S / m, 1 S / m, 2 S / m, 3 S / m, 4 S / m, 5 S / m, and 6 S / m, electron transport within the negative electrode material is beneficial, as is the rate performance of the negative electrode material during charge and discharge.

[0047] This application also provides a method for preparing the above-mentioned negative electrode material, such as... Figure 1 The diagram shown is a flowchart of the preparation process of the negative electrode material of this application, including the following steps: Step S100: Mix the carbon-based carbonized material with the first activator and perform a first activation treatment to obtain the activated material; Step S200: Mix the activating material with the second activator for a second activation treatment to obtain a porous carbonaceous material. The amount of the first activator added is 4 to 10 times that of the second activator added, and the time of the first activation treatment is longer than that of the second activation treatment.

[0048] Step S300: Mix the porous carbonaceous material and the silicon source and perform heat treatment to obtain the negative electrode material.

[0049] In the above-mentioned scheme, this application involves activating the carbon-based carbide material twice. In the first activation treatment, the amount of the first activator added is 4 to 10 times that of the second activator, and the activation time of the first activation treatment is longer than that of the second activation treatment. This indicates that the first activation treatment has a stronger activation ability for the carbon-based carbide material, which is beneficial for forming more activation pores inside the prepared activated material, and the pore size distribution range of the activation pores is larger. The second activation treatment has a weaker activation ability. The second activation treatment can further activate the unactivated areas in the activated material, forming activation pores with smaller pore sizes, and at the same time, it can enlarge the pores with excessively small pore sizes after the first activation treatment, so that the prepared porous carbonaceous material contains more and more uniformly distributed activation pores. This application utilizes a two-stage activation process to prepare a porous carbonaceous material with good uniformity. A silicon source is then deposited within this porous carbonaceous material, with the silicon primarily distributed within the activated pores. This improves the dispersion and deposition amount of silicon in the anode material, ensuring a uniformity N of ≥ 80%. This suppresses the volume effect caused by silicon agglomeration during lithium insertion / deintercalation, reducing particle pulverization. Simultaneously, the formation of the SEI film within a confined space during lithium insertion / deintercalation facilitates a stable SEI film formation, enhancing the structural stability of the anode material and thus improving its expansion performance, cycle performance, and capacity. This application, by controlling the different activation levels in the two activation processes, prepares a porous carbonaceous material with good uniformity. The process is simple, allows for mass production, and improves the electrochemical performance of the anode material as a battery.

[0050] The preparation method of this application is described in detail below with reference to the embodiments: Step S100: Mix the carbon-based carbonized material with the first activator to obtain the activated material.

[0051] In some embodiments, carbon-based carbonized materials are obtained by carbonizing carbon-based raw materials.

[0052] In some embodiments, the carbon-based raw material includes at least one of lignin, coconut shell, fruit shell, peanut shell, rice husk, coal-derived biomass, and resin.

[0053] In some embodiments, the carbonization temperature is 400℃~900℃, specifically 400℃, 500℃, 600℃, 650℃, 700℃, 750℃, 800℃, 850℃ or 900℃, etc., and of course other values ​​within the above range are also possible, which are not limited here.

[0054] In some embodiments, the carbonization time is 1h to 20h, specifically 1h, 3h, 5h, 10h, 12h, 15h, 18h and 20h, etc. Of course, it can also be other values ​​within the above range, which are not limited here.

[0055] In some embodiments, carbonization is carried out in a protective gas atmosphere, including at least one of nitrogen, helium, neon, argon, krypton, and xenon.

[0056] In some embodiments, after obtaining the carbon-based carbonized material, the process further includes: acid washing the carbon-based carbonized material, wherein the acid used for acid washing is at least one selected from hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, phosphoric acid, perchloric acid, acetic acid, and benzoic acid.

[0057] In some embodiments, the concentration of the pickling solution is 1 mol / L to 10 mol / L, for example, it can be 1 mol / L, 3 mol / L, 5 mol / L, 8 mol / L, or 10 mol / L, etc., and of course, other values ​​within the above range are also possible, without limitation. It is understood that the purpose of pickling is to remove impurities from the material. The carbon-based carbonized material is pickled and then washed with deionized water until the product is neutral.

[0058] In some implementations, the pickling time is 3h to 8h, for example, it can be 3h, 4h, 5h, 6h, 7h or 8h, etc., and of course it can be other values ​​within the above range, which are not limited here.

[0059] In some embodiments, the first activator includes an alkaline substance.

[0060] In some embodiments, the alkaline substance includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, and rubidium hydroxide.

[0061] In some embodiments, the mass ratio of carbon-based carbide to the first activator is 1:(0.5~30), specifically 1:0.5, 1:1, 1:5, 1:10, 1:20, and 1:30, etc., and other values ​​within the above range are also possible and are not limited here. Within the above-mentioned range, a larger amount of the first activator results in stronger activation ability, enabling the formation of more and more uniformly distributed activation pores in the carbon-based carbide, which is beneficial for the subsequent filling of silicon material into the activation pores. If too much of the first activator is added, the pore size of the pore structure in the activation material will be larger and the number of pores will be greater, which may easily lead to structural collapse of the anode material during the insertion / extraction process, resulting in a decrease in the cycle performance of the anode material. If too little of the first activator is added, it will be impossible to form a suitable number and uniformly distributed activation pores inside the carbon-based carbide, which is not conducive to the subsequent deposition of silicon source, and the anode material will have a large volume expansion, resulting in a decrease in the capacity and expansion performance of the anode material.

[0062] In some embodiments, the first activator includes at least one of water vapor, oxygen, and air. The gaseous first activator activates the carbon-based carbide by reacting with carbon at high temperature using gaseous water vapor, oxygen, and air to generate hydrogen and carbon monoxide, thereby etching the carbon-based carbide to obtain activated pores.

[0063] In some embodiments, the concentration of the first activator is 3% to 20%, specifically 3%, 5%, 7%, 9%, 10%, 12%, 15%, 18%, and 20%, etc., and of course, other values ​​within the above range are also possible, which are not limited herein. Within the above-defined range, the addition of a relatively large amount of the first activator results in a stronger activation ability, which can form more and more uniformly distributed activation pores in the carbon-based carbide, which is beneficial for the subsequent filling of silicon material into the activation pores.

[0064] It is understandable that when the first activator is water vapor, the concentration of water vapor can be considered as the humidity of water vapor.

[0065] In some embodiments, the first activation treatment time is 5h to 20h, for example, it can be 5h, 8h, 10h, 12h, 15h, 18h or 20h, etc. Of course, it can also be other values ​​within the above range, which are not limited here.

[0066] In some embodiments, the temperature of the first activation treatment is 900℃~1200℃, specifically 900℃, 930℃, 950℃, 1000℃, 1100℃ and 1200℃, etc., and of course other values ​​within the above range are also possible, which are not limited here.

[0067] Step S200: Mix the activating material with the second activator for a second activation treatment to obtain a porous carbonaceous material. The amount of the first activator added is 4 to 10 times that of the second activator added, and the time of the first activation treatment is longer than that of the second activation treatment.

[0068] In this application, by limiting the amount of the first activator to 4 to 10 times that of the second activator, and by making the first activation treatment time longer than the second activation treatment time, the carbon-based carbon material undergoes two activation treatments, resulting in a porous carbon material with a large number of activated pores and a uniform distribution.

[0069] In some embodiments, the amount of the first activator added is 4 to 10 times that of the second activator added, specifically 4, 5, 6, 7, 8, 9, and 10 times, etc., and of course, other values ​​within the above range are also possible, which are not limited herein. If the amount of the second activator added is too small, the activation ability of the second activation treatment is poor, and it cannot play the role of increasing the activation pores, resulting in fewer activation pores and poor distribution uniformity in the porous carbonaceous material; if the amount of the second activator added is too large, it is easy for the activation pores formed in the first activation treatment to undergo secondary pore expansion to form mesopores or macropores, which is not conducive to the dispersion uniformity of subsequent silicon source deposition, resulting in poor expansion performance of the material.

[0070] It is understood that the first activator and the second activator can be gaseous or solid. When they are gaseous activators, the amount added can represent the concentration of the gaseous activator introduced; when they are solid activators, the amount added can represent the mass of the solid activator added. If the first activator is a gaseous activator and the second activator is a solid activator, those skilled in the art can, based on experience, determine the activation differences between the gaseous and solid activators, thereby determining the concentration of the gaseous activator and the mass of the solid activator added.

[0071] In some embodiments, the second activator includes an alkaline substance.

[0072] In some embodiments, the alkaline substance includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, and rubidium hydroxide.

[0073] In some embodiments, the mass ratio of carbon-based carbide to the second activator is 1:(0.1~10), specifically 1:0.1, 1:0.5, 1:1.5, 1:3, 1:5, and 1:10, or other values ​​within the above range, which are not limited here. If the amount of the second activator added is too small, the activator prepared in step S100 cannot be effectively activated a second time; if the amount of the second activator added is too large, the pore size after secondary pore expansion will be too large, affecting the subsequent deposition of silicon material, causing the silicon material to easily agglomerate, resulting in a large volume effect in the negative electrode material, which is prone to cracking or even pulverization during use, which is not conducive to improving the expansion performance of the material. At the same time, the large pore size of the porous carbon makes the material prone to collapse and has poor structural stability. Preferably, the mass ratio of carbon-based carbide to the second activator is 1:(0.1~3).

[0074] In some embodiments, the second activator includes at least one of water vapor, oxygen, and air.

[0075] In some embodiments, the concentration of the second activator is 0.1% to 5%, specifically 0.1%, 0.3%, 0.8%, 1%, 2%, 3%, 4%, and 5%, etc., and of course, other values ​​within the above range are also possible, which are not limited herein. Within the above-defined range, the amount of the second activator added is relatively small. On the one hand, it can expand the activated pores obtained from the first activation treatment without making the pore size too large, which is beneficial for the subsequent filling of silicon material; on the other hand, the second activator can activate the unactivated areas in the activated material to obtain activated pores with smaller pore sizes, thereby making the prepared porous carbonaceous material have a large number of activated pores and a relatively uniform distribution of activated pores. If the concentration of the second activator is less than 0.1%, the activated material prepared in step S100 cannot be effectively activated a second time. If the concentration of the second activator is less than or greater than 5%, the pore size after secondary pore expansion will be too large, affecting the subsequent deposition of silicon material, causing the silicon material to easily agglomerate, resulting in a large volume effect of the anode material. The anode material is prone to cracking or even pulverization during use, which is not conducive to improving the expansion performance of the material. At the same time, the large pore size of the porous carbon makes the material prone to collapse and has poor structural stability.

[0076] In some embodiments, the second activation treatment time is 3h to 10h, for example, it can be 3h, 4h, 5h, 6h, 7h, 8h, 9h, or 10h, etc., and of course, other values ​​within the above range are also possible, which are not limited here. Within the above-defined range, it is beneficial for the prepared porous carbonaceous material to have a large number of uniformly distributed activation pores, which is conducive to the subsequent deposition of silicon material inside the porous carbonaceous material. If the second activation treatment time is too short, the activated material prepared in step S100 cannot be effectively activated a second time, resulting in a small amount of silicon material deposited inside the porous carbonaceous material, causing performance degradation; if the second activation treatment time is too long, the pore size after secondary pore expansion is too large, affecting the subsequent deposition of silicon material, resulting in a large volume effect of the negative electrode material, which is prone to cracking or even pulverization during use, which is not conducive to improving the expansion performance of the material. At the same time, the large pore size inside the porous carbon makes the material prone to collapse and has poor structural stability.

[0077] In some embodiments, the temperature of the second activation treatment is 800℃~1000℃, specifically 800℃, 830℃, 85℃, 900℃, 950℃, and 1000℃, etc., and of course, other values ​​within the above range are also possible, which are not limited herein. In some embodiments, by limiting the temperature of the first activation treatment to be greater than the temperature of the second activation treatment, the activation degrees of the two activation treatment processes are different and the differences are large, thereby preparing porous carbonaceous materials with good consistency.

[0078] In summary, this application prepares porous carbonaceous materials with a suitable number and uniform distribution of activated pores by controlling the amount of activator added, the activation temperature, and the activation time of the two activation treatments.

[0079] Step S300: Mix porous carbonaceous material and silicon source and perform heat treatment to obtain negative electrode material. In some implementations, the silicon source includes silane.

[0080] In some embodiments, the flow rate of the silicon source is 0.1 L / min to 1000 L / min, specifically 0.1 L / min, 1 L / min, 10 L / min, 100 L / min, 300 L / min, 600 L / min and 1000 L / min, etc., and of course other values ​​within the above range are also possible, which are not limited in this application.

[0081] In some embodiments, the heat treatment temperature is 300℃~800℃, specifically 300℃, 400℃, 500℃, 600℃, 700℃ and 800℃, etc., and of course other values ​​within the above range are also possible, which are not limited here.

[0082] In some embodiments, the heat treatment time is 2 h to 25 h, specifically 2 h, 5 h, 10 h, 15 h, 20 h and 25 h, etc., and of course other values ​​within the above range are also possible, which are not limited here.

[0083] In some embodiments, after heat treatment of the porous carbonaceous material and silicon source, the mixture further includes: mixing the heat-treated material and the coating material and then heat-treating them.

[0084] In some embodiments, the coating material includes one of a carbon source, a metal oxide, and a nitride.

[0085] In some embodiments, the nitride includes at least one of titanium nitride, vanadium nitride, cobalt nitride, nickel nitride, and carbon nitride.

[0086] In some embodiments, the metal oxide includes at least one selected from iron oxide, zinc oxide, tin oxide, copper oxide, and titanium oxide. In some embodiments, the carbon source includes at least one of a gaseous carbon source and a solid carbon source.

[0087] In some embodiments, the gaseous carbon source includes at least one selected from acetylene, methane, propylene, benzene, ethanol, methanol, ethylene, propane, and butane.

[0088] In some embodiments, the flow rate of the gaseous carbon source is 0.1 L / min to 1000 L / min, specifically 0.1 L / min, 1 L / min, 10 L / min, 100 L / min, 300 L / min, 600 L / min and 1000 L / min, etc., and of course other values ​​within the above range are also possible, which are not limited in this application.

[0089] In some embodiments, the solid carbon source includes at least one selected from sucrose, fructose, glucose, pitch, phenolic resin, polyimide, citric acid, epoxy resin, amino resin, polystyrene, polyacrylic acid, carboxymethyl cellulose, and cellulose acetate butyrate.

[0090] In some embodiments, the mass ratio of the solid carbon source to the heat-treated material is (1~100):100, specifically 1:100, 10:100, 30:100, 50:100, 80:100 and 100:100, etc. Of course, other values ​​within the above range are also possible, and this application does not limit them here.

[0091] In some embodiments, the heat treatment temperature is 600℃~1100℃. Specifically, the heat treatment temperature can be, for example, 600℃, 650℃, 700℃, 800℃, 900℃, 1000℃, and 1100℃, etc., and of course, other values ​​within the above range are also possible, which are not limited herein. If the heat treatment temperature is below 600℃, the coating material will not be completely carbonized, and a dense coating layer cannot be obtained. If the heat treatment temperature is above 1100℃, the silicon material will crystallize, resulting in poor cycle performance and expansion performance of the negative electrode material.

[0092] In some embodiments, the heat treatment holding time is 2h to 10h. Specifically, the heat treatment holding time can be, for example, 2h, 5h, 7h, 8h and 10h, etc. Of course, it can also be other values ​​within the above range, which are not limited here.

[0093] In some embodiments, after mixing the heat-treated material and the coating material and then performing heat treatment, the process further includes the steps of sieving and grading the resulting material.

[0094] Thirdly, this application provides a lithium-ion battery comprising the above-described negative electrode material or the negative electrode material prepared by the above-described preparation method.

[0095] Those skilled in the art will understand that the methods for preparing lithium-ion batteries described above are merely examples. Other methods commonly used in the art can be employed without departing from the disclosure of this application.

[0096] The embodiments of this application will be further described below with reference to several examples. However, the embodiments of this application are not limited to the specific embodiments described below. Appropriate modifications can be made within the scope of the main claims.

[0097] Example 1 (1) Place 10g of bamboo charcoal in a carbonization furnace for carbonization treatment. The carbonization temperature is 800℃ and the carbonization time is 7h. After carbonization, acid washing is performed. The concentration of hydrochloric acid for acid washing is 10mol / L and the acid washing time is 5h to obtain carbon-based carbonized material.

[0098] (2) After drying the carbon-based carbonized material, it is activated by steam. A mixture of steam and nitrogen is introduced, with a steam concentration of 9%, an activation time of 18 hours, and an activation temperature of 900°C to obtain the activated material.

[0099] (3) The activated material is subjected to secondary steam activation treatment. A mixture of steam and nitrogen is introduced, with a steam concentration of 2%, an activation time of 3 hours, and an activation temperature of 900℃ to obtain porous carbonaceous material.

[0100] (4) Place the porous carbonaceous material in the CVD equipment, then introduce silane into the CVD equipment, control the silane concentration to 25%, raise the temperature to 460℃, and react for 8 hours.

[0101] (5) Place the material obtained in step (4) in a reactor, introduce methane gas with a methane concentration of 12%, heat treat at 720°C for 2 hours, and then sieve and classify the obtained sample to obtain the negative electrode material.

[0102] The negative electrode material obtained in this embodiment includes a core and a carbon coating layer on the surface of the core. The core includes porous carbonaceous material and silicon particles distributed inside and on the surface of the porous carbonaceous material. The uniformity N of the negative electrode material, the median particle size, specific surface area and conductivity of the negative electrode material prepared in this embodiment, as well as the pore volume of the porous carbonaceous material, the proportion of micropores in the porous carbonaceous material, the average pore size and the mass proportion of silicon particles in the negative electrode material are shown in Table 1.

[0103] The scanning electron microscope (SEM) BSE image of the negative electrode material prepared in this embodiment is obtained from... Figure 2 It can be seen that in the negative electrode material prepared in this embodiment, typical particles with first brightness and particles with second brightness can be distinguished. In the batch of negative electrode materials, the number of negative electrode material particles with second brightness accounts for a large proportion, indicating that this application can obtain a negative electrode material in which silicon is deposited inside a porous carbonaceous material of appropriate quantity and uniform distribution.

[0104] The XRD pattern of the negative electrode material prepared in this embodiment is shown below. Figure 3 As shown, by Figure 3 It can be seen that the negative electrode material has no characteristic peaks at the 25°~30° position, which is a diffraction band. This indicates that there is amorphous silicon in the negative electrode material, that is, the silicon deposited in the porous carbonaceous material is amorphous silicon, which is beneficial to reducing the volume expansion of the negative electrode material.

[0105] The initial charge-discharge curve of the negative electrode material prepared in this embodiment is as follows: Figure 4 As shown, by Figure 4 It is evident that this negative electrode material exhibits high initial charge-discharge capacity and high initial efficiency.

[0106] The cycle performance curve of the negative electrode material prepared in this embodiment is as follows: Figure 5 As shown, by Figure 5 It is evident that this anode material exhibits excellent cycling performance, with a capacity retention rate of 92.2% after 50 cycles.

[0107] Example 2 (1) Place 10g of coconut shell in a carbonization furnace for carbonization treatment. The carbonization temperature is 800℃ and the carbonization time is 10h. After carbonization, acid washing is performed. The concentration of hydrochloric acid for acid washing is 10mol / L and the acid washing time is 5h to obtain carbon-based carbonized material.

[0108] (2) After drying the carbon-based carbonized material, it is activated by steam. A mixture of steam and nitrogen is introduced, with a steam concentration of 3.5%, an activation time of 12 hours, and an activation temperature of 950°C to obtain the activated material. (3) The activated material is subjected to secondary steam activation treatment. A mixture of steam and nitrogen is introduced, with a steam concentration of 0.5%, an activation time of 6 hours, and an activation temperature of 950°C to obtain porous carbonaceous material.

[0109] (4) Place the porous carbonaceous material in the CVD equipment, then introduce silane into the CVD equipment, control the silane concentration to 25%, raise the temperature to 460℃, and react for 8 hours.

[0110] (5) Place the material obtained in step (4) in a reactor, introduce methane gas with a methane concentration of 12%, heat treat at 720°C for 2 hours, and then sieve and classify the obtained sample to obtain the negative electrode material.

[0111] The negative electrode material obtained in this embodiment includes a core and a carbon coating layer on the surface of the core. The core includes porous carbonaceous material and silicon particles distributed inside and on the surface of the porous carbonaceous material. The uniformity N of the negative electrode material, the median particle size, specific surface area and conductivity of the negative electrode material prepared in this embodiment, as well as the pore volume of the porous carbonaceous material, the proportion of micropores in the porous carbonaceous material, the average pore size and the mass proportion of silicon particles in the negative electrode material are shown in Table 1.

[0112] Example 3 (1) Place 10g of fruit shell in a carbonization furnace for carbonization treatment. The carbonization temperature is 950℃ and the carbonization time is 5h. After carbonization, acid washing is performed. The concentration of hydrochloric acid for acid washing is 10mol / L and the acid washing time is 5h to obtain carbon-based carbonized material.

[0113] (2) After drying the carbon-based carbonized material, it is activated by steam. A mixture of steam and nitrogen is introduced, with a steam concentration of 5.7%, an activation time of 14 hours, and an activation temperature of 950°C to obtain the activated material. (3) The activated material is subjected to alkaline activation treatment. The alkali is sodium hydroxide, the amount of sodium hydroxide added is 3% of the mass of the fruit shell, the activation time is 9h, and the activation temperature is 950℃ to obtain porous carbonaceous material.

[0114] (4) Place the porous carbonaceous material in the CVD equipment, then introduce silane into the CVD equipment, control the silane concentration to 25%, raise the temperature to 460℃, and react for 8 hours.

[0115] (5) Place the material obtained in step (4) in a reactor, introduce methane gas with a methane concentration of 12%, heat treat at 720°C for 2 hours, and then sieve and classify the obtained sample to obtain the negative electrode material.

[0116] The negative electrode material obtained in this embodiment includes a core and a carbon coating layer on the surface of the core. The core includes porous carbonaceous material and silicon particles distributed inside and on the surface of the porous carbonaceous material. The uniformity N of the negative electrode material, the median particle size, specific surface area and conductivity of the negative electrode material prepared in this embodiment, as well as the pore volume of the porous carbonaceous material, the proportion of micropores in the porous carbonaceous material, the average pore size and the mass proportion of silicon particles in the negative electrode material are shown in Table 1.

[0117] Example 4 (1) Place 10g of fruit shell in a carbonization furnace for carbonization treatment. The carbonization temperature is 950℃ and the carbonization time is 5h. After carbonization, acid washing is performed. The concentration of hydrochloric acid for acid washing is 10mol / L and the acid washing time is 5h to obtain carbon-based carbonized material.

[0118] (2) After drying the carbon-based carbonized material, it is activated by steam. A mixture of steam and nitrogen is introduced, with a steam concentration of 14.5%, an activation time of 8 hours, and an activation temperature of 990°C to obtain the activated material. (3) The activated material is subjected to secondary steam activation treatment. A mixture of steam and nitrogen is introduced, with a steam concentration of 1.5%, an activation time of 5 hours, and an activation temperature of 850°C to obtain porous carbonaceous material.

[0119] (4) Place the porous carbonaceous material in the CVD equipment, then introduce silane into the CVD equipment, control the silane concentration to 25%, raise the temperature to 460℃, and react for 8 hours.

[0120] (5) Place the material obtained in step (4) in a reactor, introduce methane gas with a methane concentration of 12%, heat treat at 720°C for 2 hours, and then sieve and classify the obtained sample to obtain the negative electrode material.

[0121] The negative electrode material obtained in this embodiment includes a core and a carbon coating layer on the surface of the core. The core includes porous carbonaceous material and silicon particles distributed inside and on the surface of the porous carbonaceous material. The uniformity N of the negative electrode material, the median particle size, specific surface area and conductivity of the negative electrode material prepared in this embodiment, as well as the pore volume of the porous carbonaceous material, the proportion of micropores in the porous carbonaceous material, the average pore size and the mass proportion of silicon particles in the negative electrode material are shown in Table 1.

[0122] Example 5 (1) Place 10g of fruit shell in a carbonization furnace for carbonization treatment. The carbonization temperature is 950℃ and the carbonization time is 5h. After carbonization, acid washing is performed. The concentration of hydrochloric acid for acid washing is 10mol / L and the acid washing time is 5h to obtain carbon-based carbonized material.

[0123] (2) After drying the carbon-based carbonized material, it is activated by steam. A mixture of steam and nitrogen is introduced, with a steam concentration of 20%, an activation time of 5 hours, and an activation temperature of 1050℃ to obtain the activated material. (3) The activated material is subjected to secondary steam activation treatment. A mixture of steam and nitrogen is introduced, with a steam concentration of 5%, an activation time of 3 hours, and an activation temperature of 900℃ to obtain porous carbonaceous material.

[0124] (4) Place the porous carbonaceous material in the CVD equipment, then introduce silane into the CVD equipment, control the silane concentration to 25%, raise the temperature to 460℃, and react for 8 hours.

[0125] (5) Place the material obtained in step (4) in a reactor, introduce methane gas with a methane concentration of 12%, heat treat at 720°C for 2 hours, and then sieve and classify the obtained sample to obtain the negative electrode material.

[0126] The negative electrode material obtained in this embodiment includes a core and a carbon coating layer on the surface of the core. The core includes porous carbonaceous material and silicon particles distributed inside and on the surface of the porous carbonaceous material. The uniformity N of the negative electrode material, the median particle size, specific surface area and conductivity of the negative electrode material prepared in this embodiment, as well as the pore volume of the porous carbonaceous material, the proportion of micropores in the porous carbonaceous material, the average pore size and the mass proportion of silicon particles in the negative electrode material are shown in Table 1.

[0127] Example 6 (1) Place 10g of fruit shell in a carbonization furnace for carbonization treatment. The carbonization temperature is 950℃ and the carbonization time is 5h. After carbonization, acid washing is performed. The concentration of hydrochloric acid for acid washing is 10mol / L and the acid washing time is 5h to obtain carbon-based carbonized material.

[0128] (2) The carbon-based carbonized material is subjected to alkali activation treatment. The alkali is sodium hydroxide. The amount of sodium hydroxide added is 15% of the weight of the fruit shell. The activation time is 10h and the activation temperature is 950℃ to obtain activated material. (3) The activated material is subjected to a second alkaline activation treatment. The alkali is sodium hydroxide, the amount of sodium hydroxide added is 3% of the mass of the fruit shell, the activation time is 5h, and the activation temperature is 850℃ to obtain porous carbonaceous material.

[0129] (4) Place the porous carbonaceous material in the CVD equipment, then introduce silane into the CVD equipment, control the silane concentration to 25%, raise the temperature to 460℃, and react for 8 hours.

[0130] (5) Place the material obtained in step (4) in a reactor, introduce methane gas with a methane concentration of 12%, heat treat at 720°C for 2 hours, and then sieve and classify the obtained sample to obtain the negative electrode material.

[0131] The negative electrode material obtained in this embodiment includes a core and a carbon coating layer on the surface of the core. The core includes porous carbonaceous material and silicon particles distributed inside and on the surface of the porous carbonaceous material. The uniformity N of the negative electrode material, the median particle size, specific surface area and conductivity of the negative electrode material prepared in this embodiment, as well as the pore volume of the porous carbonaceous material, the proportion of micropores in the porous carbonaceous material, the average pore size and the mass proportion of silicon particles in the negative electrode material are shown in Table 1.

[0132] Example 7 (1) Place 10g of fruit shell in a carbonization furnace for carbonization treatment. The carbonization temperature is 950℃ and the carbonization time is 5h. After carbonization, acid washing is performed. The concentration of hydrochloric acid for acid washing is 10mol / L and the acid washing time is 5h to obtain carbon-based carbonized material.

[0133] (2) The carbon-based carbonized material is subjected to alkaline activation treatment. The alkali is sodium hydroxide. The amount of sodium hydroxide added is 10% of the mass of the fruit shell. The activation time is 12h and the activation temperature is 1000℃ to obtain activated material. (3) The activated material is subjected to a second alkaline activation treatment. The alkali is sodium hydroxide, the amount of sodium hydroxide added is 1% of the mass of the fruit shell, the activation time is 3h, and the activation temperature is 850℃ to obtain porous carbonaceous material.

[0134] (4) Place the porous carbonaceous material in the CVD equipment, then introduce silane into the CVD equipment, control the silane concentration to 25%, raise the temperature to 460℃, and react for 8 hours.

[0135] (5) Place the material obtained in step (4) in a reactor, introduce methane gas with a methane concentration of 12%, heat treat at 720°C for 2 hours, and then sieve and classify the obtained sample to obtain the negative electrode material.

[0136] The negative electrode material obtained in this embodiment includes a core and a carbon coating layer on the surface of the core. The core includes porous carbonaceous material and silicon particles distributed inside and on the surface of the porous carbonaceous material. The uniformity N of the negative electrode material, the median particle size, specific surface area and conductivity of the negative electrode material prepared in this embodiment, as well as the pore volume of the porous carbonaceous material, the proportion of micropores in the porous carbonaceous material, the average pore size and the mass proportion of silicon particles in the negative electrode material are shown in Table 1.

[0137] Comparative Example 1 (1) Bamboo charcoal is placed in a carbonization furnace for carbonization treatment. The carbonization temperature is 800℃ and the carbonization time is 7h. After carbonization, it is acid washed. The concentration of hydrochloric acid for acid washing is 10mol / L and the acid washing time is 5h to obtain carbon-based carbonized material.

[0138] (2) Place the carbon-based carbonized material in the CVD equipment, then introduce silane into the CVD equipment, control the silane concentration to 25%, raise the temperature to 460℃, and react for 8 hours.

[0139] (3) Place the material obtained in step (2) in a reactor, introduce methane gas with a methane concentration of 12%, heat treat at 720°C for 2 hours, and then sieve and classify the obtained sample to obtain the negative electrode material.

[0140] Comparative Example 2 Unlike Example 1, step (3) is skipped, and the activated material obtained in step (2) is directly subjected to step (4).

[0141] Comparative Example 3 Unlike Example 1, step (2) is omitted, and the carbon-based carbonized material obtained in step (1) is directly subjected to step (3).

[0142] Comparative Example 4 (1) Place 10g of fruit shell in a carbonization furnace for carbonization treatment. The carbonization temperature is 950℃ and the carbonization time is 5h. After carbonization, acid washing is performed. The concentration of hydrochloric acid for acid washing is 10mol / L and the acid washing time is 5h to obtain carbon-based carbonized material.

[0143] (2) After drying the carbon-based carbonized material, it is activated by steam. A mixture of steam and nitrogen is introduced, with a steam concentration of 9%, an activation time of 18 hours, and an activation temperature of 900°C to obtain the activated material. (3) The activated material is subjected to secondary steam activation treatment. A mixture of steam and nitrogen gas is introduced, with a steam concentration of 9%, an activation time of 16 hours, and an activation temperature of 900℃ to obtain porous carbonaceous material.

[0144] (4) Place the porous carbonaceous material in the CVD equipment, then introduce silane into the CVD equipment, control the silane concentration to 25%, raise the temperature to 460℃, and react for 8 hours.

[0145] (5) Place the material obtained in step (4) in a reactor, introduce methane gas with a methane concentration of 12%, heat treat at 720°C for 2 hours, and then sieve and classify the obtained sample to obtain the negative electrode material.

[0146] Comparative Example 5 (1) Place 10g of fruit shell in a carbonization furnace for carbonization treatment. The carbonization temperature is 950℃ and the carbonization time is 5h. After carbonization, acid washing is performed. The concentration of hydrochloric acid for acid washing is 10mol / L and the acid washing time is 5h to obtain carbon-based carbonized material.

[0147] (2) After drying the carbon-based carbonized material, it is activated by steam. A mixture of steam and nitrogen is introduced, with a steam concentration of 9%, an activation time of 2 hours, and an activation temperature of 900℃ to obtain the activated material. (3) The activated material is subjected to secondary steam activation treatment. A mixture of steam and nitrogen is introduced, with a steam concentration of 2%, an activation time of 12 hours, and an activation temperature of 900°C to obtain porous carbonaceous material.

[0148] (4) Place the porous carbonaceous material in the CVD equipment, then introduce silane into the CVD equipment, control the silane concentration to 25%, raise the temperature to 460℃, and react for 8 hours.

[0149] (5) Place the material obtained in step (4) in a reactor, introduce methane gas with a methane concentration of 12%, heat treat at 720°C for 2 hours, and then sieve and classify the obtained sample to obtain the negative electrode material.

[0150] Performance testing 1. The pore volume of porous carbonaceous materials is tested using BET pore distribution. Before testing the porosity, the silicon material in the negative electrode material needs to be etched away using HF.

[0151] 2. The number of micropores in porous carbonaceous materials was determined by nitrogen desorption.

[0152] 3. Before etching the silicon material in the negative electrode material, test the mass M1 of the negative electrode material. After etching the silicon material with HF, test the mass M2 of the negative electrode material. (M2-M1) / M2 is the mass ratio of silicon material in the negative electrode material.

[0153] 4. The median particle size of the negative electrode material was measured using a laser particle size analyzer.

[0154] 5. After etching the silicon material in the porous carbonaceous material using HF, the average pore diameter was measured using a Micromeritics ASAP 2460 fully automated surface area and porosity analyzer. The gas used for testing was either CO2 or N2. Etching method: The negative electrode material was soaked in a 1M nitric acid solution for 4 hours. Then, a 20% (w / w) HF acid solution was added dropwise to the negative electrode material, producing yellow fumes. This process was repeated until no more yellow fumes were produced in the solution. Finally, the residue was digested with a 1M nitric acid solution, followed by washing and drying to obtain the negative electrode material after removing the silicon material.

[0155] 6. Test method for median particle size of silicon materials: Perform mathematical statistics on the diameter of silicon materials in transmission electron microscopy images.

[0156] 7. The scanning electron microscope is a Hitachi S4800. The test conditions are: voltage 3 kV and current 10 μA.

[0157] 8. The following methods were used to test the electrochemical performance of the negative electrode material: The negative electrode material, conductive agent, and binder were dissolved and mixed in a solvent at a mass ratio of 94:1:5, with the solid content controlled at 50%. This mixture was then coated onto a copper foil current collector and vacuum dried to obtain the negative electrode sheet. Subsequently, a ternary positive electrode sheet prepared using conventional mature processes, a 1 mol / L LiPF6 / EC+DMC+EMC (v / v=1:1:1) electrolyte, a Celgard 2400 separator, and a casing were assembled into an 18650 cylindrical cell using conventional manufacturing processes. The charge-discharge tests of the cylindrical cells were conducted on the LAND battery testing system of Wuhan Jinno Electronics Co., Ltd., under normal temperature conditions, with a constant current charge-discharge of 0.2C and a charge-discharge voltage limited to 2.75~4.2V. The test results are shown in Tables 1 and 2.

[0158] Table 1. Uniformity test results of the negative electrode materials in each embodiment and comparative example.

[0159] Table 2. Performance test results of the anode materials in each embodiment and comparative example.

[0160] As shown in Tables 1 and 2, the negative electrode materials prepared in Examples 1-7 of this application include porous carbonaceous materials and silicon materials. The negative electrode materials have a uniformity N, where N ≥ 80%, indicating that the porous carbonaceous materials of this application have uniformly distributed activation pores, and the number of activation pores is appropriate, allowing the silicon material to be mainly distributed within the pores of the porous carbonaceous materials. Furthermore, this application uses materials with a diameter of 100 μm. The negative electrode materials obtained from testing within a 100μm region show that the number and distribution of activated pores in the porous carbonaceous material of each negative electrode material particle in this application are highly similar. That is, the negative electrode material in this application has a porous carbonaceous material with good consistency. The porous carbonaceous material with good consistency can improve the dispersion of silicon material in the negative electrode material, suppress the volume effect caused by the agglomeration of silicon material during lithium insertion / deintercalation, and reduce the pulverization of negative electrode material particles. At the same time, during the lithium insertion / deintercalation process, the SEI film is formed in a limited space, which is conducive to the formation of a stable SEI film, improves the structural stability of the negative electrode material, and thus improves the expansion performance, cycle performance and capacity of the negative electrode material.

[0161] In Comparative Example 1, the carbon-based carbide material was not activated and the silicon source was directly deposited, resulting in very little silicon deposition in the anode material. The uniformity N of the anode material was too small, leading to problems such as low capacity, large expansion, and poor cycle performance.

[0162] In Comparative Example 2, only the carbon-based carbon material was activated in step (2) without the activation in step (3), which resulted in the distribution uniformity of activated pores in the porous carbon material being inferior to that in Example 1. The deposition of silicon source on the porous carbon material resulted in poor distribution uniformity of silicon in the porous carbon material, and the uniformity N of the negative electrode material did not meet the limits of this application, leading to poor expansion and cycle performance of the negative electrode material.

[0163] In Comparative Example 3, only the carbon-based carbon material was activated in step (3), resulting in fewer activated pores in the porous carbon material and a less uniform distribution than in Example 1 and Comparative Example 2. The deposition of silicon source on the porous carbon material resulted in poor uniform distribution of silicon in the porous carbon material and a smaller amount of silicon deposited in the porous carbon material. The uniformity N of the negative electrode material did not meet the limits of this application, resulting in poor expansion performance and cycle performance of the negative electrode material.

[0164] In Comparative Example 4, two activation treatments were performed, and the degree of the two activation treatments was not significantly different. This resulted in a large number and size of pores in the prepared porous carbon material, which made it easy for silicon to agglomerate inside the porous carbon material. The uniformity N of the negative electrode material did not meet the limits of this application, resulting in poor expansion performance of the negative electrode material.

[0165] In Comparative Example 5, two activation treatments were performed, and the time of the first activation treatment was much shorter than that of the second activation treatment. As a result, the pore volume of the prepared porous carbonaceous material was small, which resulted in a smaller amount of silicon source deposited inside the negative electrode material. The uniformity N of the negative electrode material did not meet the limits of this application, leading to poor capacity performance and cycle performance of the negative electrode material.

[0166] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A negative electrode material, characterized in that, The negative electrode material comprises a porous carbonaceous material, wherein silicon material is distributed within the porous carbonaceous material, and the negative electrode material has a uniformity N, where N ≥ 80%. In the backscattered electron image obtained by scanning electron microscopy (SEM) of the anode material in BSE automatic brightness and contrast mode, at any 100 μm... Within a 100μm region, the number of particles of the negative electrode material with a first brightness is denoted as C1. Particles of the negative electrode material with the first brightness represent negative electrode materials with a grayscale value greater than or equal to 5500 in the backscattered electron image. The number of particles of the negative electrode material with a second brightness is denoted as C2. Particles of the negative electrode material with the second brightness represent negative electrode materials with a grayscale value less than 5500 in the backscattered electron image. The uniformity of the negative electrode material within the aforementioned region is N' = C2 / (C2 + C1). 100%, the uniformity N of the negative electrode material is the arithmetic mean of the uniformity N' of at least 10 of the aforementioned regions.

2. The negative electrode material according to claim 1, characterized in that, The negative electrode material includes at least one of the following features (1) to (7): (1) The silicon material is also distributed on at least a portion of the surface of the porous carbonaceous material; (2) The porous carbonaceous material includes at least one of hard carbon, soft carbon, graphite, mesophase carbon microspheres, activated carbon and carbon gel; (3) The porous carbonaceous material includes micropores, and the proportion of micropores is greater than or equal to 80%, based on the total number of pores in the porous carbonaceous material being 100%. (4) The average pore diameter of the porous carbonaceous material is less than or equal to 5 nm; (5) The silicon material includes crystalline silicon and silicide SiO2. x At least one of amorphous silicon and silicon alloys, wherein 0 < x ≤ 2; (6) The silicon material accounts for 30% to 80% of the mass of the negative electrode material; (7) The median particle size of the silicon material is 0.1 nm to 500 nm.

3. The negative electrode material according to claim 1, characterized in that, The negative electrode material further includes a coating layer distributed on at least a portion of the surface of the porous carbonaceous material, and the negative electrode material includes at least one of the following features (1) to (4): (1) The coating layer includes a carbon layer, and the material of the carbon layer includes at least one of graphene, soft carbon, hard carbon and conductive polymer; (2) The coating layer includes a metal oxide layer, and the material of the metal oxide layer includes at least one of titanium oxide, aluminum oxide, lithium oxide, cobalt oxide and vanadium oxide; (3) The coating layer includes a nitride layer, and the material of the nitride layer includes at least one of titanium nitride, vanadium nitride, cobalt nitride, nickel nitride and carbon nitride; (4) The thickness of the coating layer is 0.1 nm to 100 nm.

4. The negative electrode material according to claim 1, characterized in that, The negative electrode material includes at least one of the following features (1) to (4): (1) The pore volume of the porous carbonaceous material is greater than or equal to 0.4 cm³. 3 / g; (2) The median particle size of the negative electrode material is less than or equal to 10 μm; (3) The specific surface area of ​​the negative electrode material is less than 5 m². 2 / g; (4) The conductivity of the negative electrode material is greater than or equal to 10. -1 S / m.

5. A lithium-ion battery, characterized in that, The lithium-ion battery includes the negative electrode material as described in any one of claims 1 to 4.

Citation Information

Patent Citations

  • Composite carbon particles and use thereof

    CN115667136A