Electrolyte, magnesium-manganese dry battery and preparation method thereof
By using magnesium halide and sodium halide electrolytes of specific concentrations in magnesium-manganese dry batteries, combined with carbon rod current collectors, the voltage hysteresis problem of magnesium-manganese dry batteries was solved, achieving high discharge capacity and stable open-circuit voltage, thus improving discharge performance.
Patent Information
- Application Number
- CN202311687428.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-08
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-08
AI Technical Summary
Magnesium-manganese dry batteries exhibit a "voltage lag" effect in the initial stage of discharge, which affects their discharge performance. Existing electrolytes such as MgSO₄, Mg(NO₃)₂, or Mg(ClO₄)₂ result in poor discharge performance of magnesium-manganese dry batteries.
Using an electrolyte composed of magnesium halides and sodium halides of specific concentrations, such as magnesium bromide and sodium fluoride, combined with a carbon rod as a current collector, a magnesium-manganese dry cell is formed, which improves the voltage hysteresis effect.
The discharge capacity and open-circuit voltage of magnesium-manganese dry batteries have been improved, the voltage hysteresis phenomenon has been basically eliminated, and the discharge performance has been enhanced.
Smart Images

Figure CN117766792B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and more specifically, to an electrolyte, a magnesium-manganese dry cell, and a method for preparing the same. Background Technology
[0002] Magnesium and its alloys possess advantages such as low electrode potential, high theoretical specific capacity, low density, and abundant resources, gradually becoming a negative electrode material for new types of batteries. Magnesium-manganese dry batteries have three times the specific energy of zinc-manganese dry batteries and exhibit high and stable discharge voltage, making them a promising new energy storage device to replace zinc-manganese dry batteries.
[0003] As early as 1948, the Leclanche-type magnesium dry cell was proposed and its performance was studied. The magnesium-manganese dioxide primary cell has a similar structure to the zinc-manganese carbon battery, using magnesium metal or magnesium alloy as the negative electrode, manganese dioxide as the positive electrode material, magnesium-containing salt as the electrolyte, and carbon rod as the current collector.
[0004] However, magnesium or magnesium alloys are chemically very reactive. While undergoing electrochemical reactions in the electrolyte, they are also accompanied by strong self-corrosion reactions. At the same time, a dense oxide film is formed on the surface of the magnesium or magnesium alloy negative electrode. When the battery starts to discharge, it takes a certain amount of time to break down the passivation film before the discharge reaction can continue. This "voltage lag" effect affects the discharge performance of magnesium-manganese dry batteries. Summary of the Invention
[0005] Based on the above-mentioned shortcomings, this application provides an electrolyte, a magnesium-manganese dry cell and a method for preparing the same, in order to partially or completely improve the problem of poor discharge performance of magnesium-manganese dry cells in related technologies.
[0006] This application is implemented as follows:
[0007] In a first aspect, an example of this application provides an electrolyte for use in a magnesium-manganese dry cell battery. The electrolyte comprises magnesium halide, sodium halide, and a solvent; the concentration of magnesium halide is 0.1-1 mol / L, and the concentration of sodium halide is 0.01-0.1 mol / L.
[0008] In the above-mentioned process, the electrolyte of the magnesium-manganese dry cell includes magnesium halide, sodium halide and solvent. By utilizing the combined effect of magnesium halide and sodium halide at specific concentrations, the discharge capacity and open-circuit voltage of the magnesium-manganese dry cell can be improved, the "voltage hysteresis" effect can be mitigated, and the discharge performance of the magnesium-manganese dry cell can be enhanced.
[0009] Furthermore, magnesium halides and sodium halides are used as the main components of the electrolyte in magnesium-manganese dry batteries. Both magnesium halides and sodium halides are inorganic salts, with abundant raw material sources, low prices, and no danger or pollution. They can be uniformly mixed with various positive electrode materials, reducing the manufacturing cost of magnesium-manganese dry batteries.
[0010] In conjunction with the first aspect, in one possible implementation, the magnesium halide is selected from at least one of magnesium fluoride, magnesium chloride, magnesium bromide, or magnesium iodide.
[0011] In the above process, the discharge capacity of magnesium-manganese dry batteries can be improved by using magnesium fluoride, magnesium chloride, magnesium bromide or magnesium iodide.
[0012] In conjunction with the first aspect, in one possible implementation, the sodium halide is selected from at least one of sodium fluoride, sodium chloride, sodium bromide, or sodium iodide.
[0013] In the above process, sodium fluoride, sodium chloride, sodium bromide or sodium iodide can be used to increase the current density and open-circuit voltage of magnesium-manganese dry cell batteries.
[0014] In conjunction with the first aspect, in one possible implementation, the magnesium halide is selected from magnesium bromide, and the sodium halide is selected from sodium fluoride.
[0015] In the above process, the combination of magnesium bromide and sodium fluoride can improve the discharge capacity and open-circuit voltage of magnesium-manganese dry batteries, improve the "voltage hysteresis" effect, and enhance the discharge performance of magnesium-manganese dry batteries.
[0016] In conjunction with the first aspect, in one possible implementation, the concentration of magnesium bromide is 0.75 mol / L and the concentration of sodium fluoride is 0.01 mol / L.
[0017] In the above-mentioned process, the concentrations of magnesium bromide and sodium fluoride have a certain impact on the discharge voltage and discharge capacity of magnesium-manganese dry batteries. Magnesium-manganese dry batteries exhibit better discharge performance when the concentration of magnesium bromide is 0.75 mol / L and the concentration of sodium fluoride is 0.01 mol / L.
[0018] In conjunction with the first aspect, in one possible implementation, the solvent is selected from water.
[0019] Optionally, the solvent may be deionized water.
[0020] In a second aspect, this application provides a method for preparing a magnesium-manganese dry cell, comprising:
[0021] The electrolyte provided in the first aspect is injected into a magnesium cylinder filled with positive electrode material. A diaphragm is provided between the positive electrode material and the inner wall of the magnesium cylinder. A carbon rod is inserted into the positive electrode material. The magnesium cylinder is sealed, and a positive electrode cap is provided at the end of the carbon rod that extends out of the magnesium cylinder to obtain a magnesium-manganese dry cell.
[0022] In the above implementation process, a diaphragm is placed on the inner wall of the magnesium cylinder, and the positive electrode material is filled inside the magnesium cylinder to prevent the positive electrode material from contacting the magnesium cylinder. The electrolyte provided in the first aspect is injected into the positive electrode material, allowing the electrolyte to fully wet the positive electrode material and form a paste-like material. A carbon rod is inserted into the positive electrode material, the magnesium cylinder is sealed, and a positive electrode cap is placed at the end of the carbon rod extending outside the magnesium cylinder, enabling the carbon rod to act as a current collector to draw out current. By using the electrolyte provided in the first aspect to wet the positive electrode material, the discharge capacity and open-circuit voltage of the magnesium-manganese dry cell can be improved, the "voltage hysteresis" effect can be mitigated, and the discharge performance of the magnesium-manganese dry cell can be enhanced.
[0023] In conjunction with the second aspect, in one possible implementation, the positive electrode material includes manganese dioxide and conductive carbon black.
[0024] In conjunction with the second aspect, in one possible implementation, manganese dioxide accounts for 85-92% of the total mass of the cathode material.
[0025] In a third aspect, an example of this application provides a magnesium-manganese dry cell prepared according to the preparation method provided in the second aspect.
[0026] In the above implementation process, the electrolyte in the magnesium-manganese dry battery provided in this application embodiment includes magnesium halide, sodium halide and solvent. Due to the combined effect of specific concentrations of magnesium halide and sodium halide, the magnesium-manganese dry battery can have a high discharge capacity and open circuit voltage, and basically does not have a "voltage hysteresis" effect. The magnesium-manganese dry battery has good discharge performance. Attached Figure Description
[0027] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below.
[0028] Figure 1 The discharge test curve provided in Embodiment 4 of this application;
[0029] Figure 2 The discharge test curves provided in Examples 4-6 of this application;
[0030] Figure 3 The discharge test curve provided for Comparative Example 4 of this application;
[0031] Figure 4 The discharge test curves provided for Comparative Examples 5, 6 and Example 6 of this application. Detailed Implementation
[0032] The embodiments of this application will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are for illustrative purposes only and should not be considered as limiting the scope of this application. Unless otherwise specified in the examples, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.
[0033] Magnesium-manganese dry cell batteries have three times the specific energy of zinc-manganese dry cell batteries, and their discharge voltage is high and stable, making them a promising new type of energy storage device to replace zinc-manganese dry cell batteries.
[0034] Magnesium-manganese dry cell batteries have a similar structure to zinc-manganese carbon batteries. They typically use magnesium metal or magnesium alloy as the negative electrode, manganese dioxide as the positive electrode material, a magnesium-containing salt solution as the electrolyte, and a carbon rod as the current collector.
[0035] However, magnesium or magnesium alloys are chemically very reactive. During electrochemical reactions in the electrolyte, they also undergo strong self-corrosion, forming a dense oxide film on the surface of the magnesium or magnesium alloy negative electrode. Therefore, when the battery begins to discharge, it typically requires a certain amount of time for the passivation film to break down before the discharge reaction can continue; this phenomenon is called the "voltage hysteresis" effect. The voltage hysteresis effect affects the discharge performance of magnesium-manganese dry cell batteries.
[0036] Typically, the electrolytes in existing magnesium-manganese dry cell electrolytes are MgSO4, Mg(NO3)2, or Mg(ClO4)2.
[0037] The inventors discovered that the electrolyte affects the discharge performance of magnesium-manganese dry batteries. When using existing electrolytes such as MgSO4, Mg(NO3)2, or Mg(ClO4)2 as electrolytes for magnesium-manganese dry batteries, the discharge performance of the batteries is poor, exhibiting a "voltage hysteresis" effect.
[0038] Therefore, in order to improve the "voltage hysteresis" effect and enhance the discharge performance of magnesium-manganese dry batteries, the inventors attempted to improve the electrolyte.
[0039] The inventors experimented with magnesium halides as the electrolyte and found that, compared to existing technologies using MgSO4, Mg(NO3)2, or Mg(ClO4)2, using magnesium halides as the electrolyte could improve the current density and discharge capacity of magnesium-manganese dry batteries. Magnesium halides, for example, are magnesium bromides.
[0040] However, when magnesium halide is used alone as the electrolyte, magnesium-manganese dry cell batteries still exhibit a certain degree of voltage hysteresis, and the electrical performance of magnesium-manganese dry cell batteries needs further improvement.
[0041] Therefore, in order to further improve the discharge performance of magnesium-manganese dry batteries and improve the "voltage hysteresis" effect, the inventors tried to add slow-release additives to magnesium halide electrolyte.
[0042] The inventors experimented with using Na3PO4 or CH3COONa as slow-release additives. They discovered that adding Na3PO4 or CH3COONa slow-release additives to the electrolyte could increase the current density and open-circuit voltage of magnesium-manganese dry batteries, and that Na3PO4 was more effective than CH3COONa as a slow-release additive.
[0043] However, even when using Na3PO4 as a slow-release additive, there is still a certain "voltage hysteresis" effect, and the electrical performance of magnesium-manganese dry batteries still needs to be further improved.
[0044] Furthermore, the type of slow-release additive needs to be matched with the type of electrolyte in order to further improve the electrical performance of magnesium-manganese dry batteries and mitigate the "voltage hysteresis" effect.
[0045] Therefore, this application further improves the electrolyte of magnesium-manganese dry cell batteries, thereby improving the "voltage hysteresis" effect of magnesium-manganese dry cell batteries to a certain extent and enhancing their discharge performance.
[0046] The electrolyte provided in this application example includes magnesium halide, sodium halide, and a solvent. The concentration of magnesium halide is 0.1-1 mol / L, and the concentration of sodium halide is 0.01-0.1 mol / L.
[0047] By utilizing the combined effect of magnesium halide and sodium halide, the discharge capacity and open-circuit voltage of magnesium-manganese dry batteries can be improved, the "voltage hysteresis" effect can be mitigated, and the discharge performance of magnesium-manganese dry batteries can be enhanced.
[0048] This application does not limit the specific types of magnesium halides; relevant personnel can make appropriate selections as needed.
[0049] In one possible embodiment, magnesium halide may be selected from at least one of magnesium fluoride, magnesium chloride, magnesium bromide, or magnesium iodide.
[0050] For example, magnesium halide can be selected from magnesium bromide.
[0051] For example, magnesium halides can be selected from magnesium bromide and magnesium chloride.
[0052] For example, magnesium halides can be selected from magnesium fluoride, magnesium bromide, and magnesium chloride.
[0053] The content of magnesium halide in the electrolyte affects the discharge performance of magnesium-manganese dry batteries.
[0054] To further improve the discharge voltage and discharge capacity of magnesium-manganese dry batteries, in one possible embodiment, the concentration of magnesium halide can be 0.1-1.0 mol / L.
[0055] For example, the concentration of magnesium halide can be one of 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L or 1.0 mol / L or any combination thereof.
[0056] For example, when the magnesium halide is selected from magnesium bromide, the concentration of magnesium bromide in the electrolyte is 0.1 mol / L; or, the concentration of magnesium bromide is 0.25 mol / L; or, the concentration of magnesium bromide is 0.5 mol / L; or, the concentration of magnesium bromide is 0.75 mol / L; or, the concentration of magnesium bromide is 1 mol / L.
[0057] This application does not limit the specific type of sodium halide. In one possible embodiment, the sodium halide may be selected from at least one of sodium fluoride, sodium chloride, sodium bromide or sodium iodide.
[0058] For example, sodium halide may be selected from sodium fluoride.
[0059] For example, sodium halide can be selected from sodium fluoride and sodium chloride.
[0060] For example, sodium halides can be selected from sodium fluoride, sodium chloride, and sodium bromide.
[0061] The concentration of sodium halide has a certain impact on the discharge voltage and discharge capacity of magnesium-manganese batteries.
[0062] To further improve the discharge voltage and discharge capacity of magnesium-manganese dry batteries, in one possible embodiment, the concentration of sodium halide in the electrolyte can be 0.01-0.1 mol / L.
[0063] For example, the concentration of sodium halide can be one of 0.01 mol / L, 0.02 mol / L, 0.03 mol / L, 0.04 mol / L, 0.05 mol / L, 0.06 mol / L, 0.07 mol / L, 0.08 mol / L, 0.09 mol / L or 0.1 mol / L or any combination thereof.
[0064] For example, when the sodium halide is selected from sodium fluoride, the concentration of sodium fluoride in the electrolyte is 0.01 mol / L; or, the concentration of magnesium bromide is 0.05 mol / L; or, the concentration of magnesium bromide is 0.1 mol / L.
[0065] For example, the electrolyte comprises 0.75 mol / L magnesium bromide and 0.01 mol / L sodium fluoride.
[0066] Furthermore, this application does not limit the specific type of solvent; in one possible embodiment, the solvent may be selected from water.
[0067] Furthermore, deionized water can be used as a solvent for magnesium bromide and sodium fluoride in the electrolyte.
[0068] Furthermore, this application example also provides a magnesium-manganese dry cell battery, which includes the electrolyte provided in this application example.
[0069] This application does not limit how magnesium-manganese dry batteries containing the electrolyte provided in the examples of this application are prepared. In one possible embodiment, this application also provides a method for preparing a magnesium-manganese dry battery, comprising:
[0070] The electrolyte provided in this application example is injected into a magnesium cylinder filled with positive electrode material. A diaphragm is provided between the positive electrode material and the inner wall of the magnesium cylinder. A carbon rod is inserted into the positive electrode material. The magnesium cylinder is sealed, and a positive electrode cap is provided at the end of the carbon rod that extends out of the magnesium cylinder to obtain a magnesium-manganese dry cell.
[0071] This application does not limit the specific material of the magnesium cylinder. In one possible embodiment, the magnesium cylinder may be made of metallic magnesium or a magnesium alloy.
[0072] For example, the magnesium alloy can be selected from AZ31 magnesium alloy.
[0073] Furthermore, this application does not limit how the magnesium cylinder is manufactured. In one possible embodiment, the magnesium cylinder can be manufactured by stamping.
[0074] Furthermore, before wrapping the diaphragm around the magnesium cylinder obtained by stamping, the magnesium cylinder can be polished to remove the oxide layer on its surface.
[0075] This application does not limit the specific type of diaphragm. In one possible embodiment, the diaphragm may be selected from polymer membranes, ceramic membranes, or polymer-ceramic hybrid membranes.
[0076] This application does not limit the specific type of cathode material. In one possible embodiment, the cathode material includes manganese dioxide and conductive carbon black.
[0077] Furthermore, manganese dioxide accounts for 85-92% of the total mass of the cathode material.
[0078] For example, in the cathode material, the mass content of manganese dioxide can be one of 85%, 86%, 87%, 88%, 89%, 90%, 91% or 92% or any combination thereof.
[0079] Furthermore, before filling the magnesium cylinder with the positive electrode material, the manganese dioxide and conductive carbon black in the positive electrode material are stirred evenly.
[0080] The electrolyte provided in this application example is injected into the positive electrode material inside the magnesium cylinder, so that the positive electrode material is fully wetted and a paste-like positive electrode material layer is formed in the magnesium cylinder.
[0081] For example, 2 to 3 mL of electrolyte is injected into a magnesium cylinder.
[0082] Furthermore, after the electrolyte has completely wetted the positive electrode material, a sealing machine can be used to seal the upper end of the magnesium cylinder, allowing one end of the carbon rod to extend beyond the magnesium cylinder.
[0083] Furthermore, after sealing, a positive electrode cap can be installed at the end of the carbon rod.
[0084] Furthermore, a negative electrode base is installed at the bottom of the magnesium cylinder.
[0085] Furthermore, heat-shrink tubing is used for packaging to obtain magnesium-manganese dry batteries.
[0086] The magnesium-manganese dry cell prepared by the above method has high discharge capacity, open circuit voltage, and current density, and basically no voltage lag effect, exhibiting good discharge performance.
[0087] The electrolyte of this application will be further described in detail below with reference to the embodiments.
[0088] Example 1
[0089] Example 1 provides an electrolyte comprising magnesium bromide, sodium fluoride, and deionized water. The concentration of magnesium bromide is 0.75 mol / L, and the concentration of sodium fluoride is 0.01 mol / L.
[0090] The specific composition of the electrolyte provided in Example 1 is shown in Table 1.
[0091] Example 2
[0092] Example 2 provides an electrolyte that differs from Example 1 in that the concentration of sodium fluoride is 0.05 mol / L.
[0093] The specific composition of the electrolyte provided in Example 2 is shown in Table 1.
[0094] Example 3
[0095] Example 3 provides an electrolyte that differs from Example 1 in that the concentration of sodium fluoride is 0.1 mol / L.
[0096] The specific composition of the electrolyte provided in Example 3 is shown in Table 1.
[0097] Comparative Example 1
[0098] Comparative Example 1 provides five electrolytes, which differ from Example 1 in that they do not contain sodium fluoride. The concentrations of magnesium bromide in the five electrolytes are 0.1 mol / L, 0.25 mol / L, 0.5 mol / L, 0.75 mol / L, and 1.0 mol / L, respectively.
[0099] The specific composition of the electrolyte provided in Comparative Example 1 is shown in Table 1.
[0100] Comparative Example 2
[0101] Comparative Example 2 provides an electrolyte that differs from Example 1 in that it consists of magnesium bromide, sodium phosphate, and deionized water. The concentration of magnesium bromide is 0.75 mol / L, and the concentration of sodium phosphate is 0.1 mol / L.
[0102] The specific composition of the electrolyte provided in Comparative Example 2 is shown in Table 1.
[0103] Comparative Example 3
[0104] Comparative Example 3 provides an electrolyte that differs from Example 1 in that it consists of magnesium bromide, sodium acetate, and deionized water. The concentration of magnesium bromide is 0.75 mol / L, and the concentration of sodium acetate is 0.1 mol / L.
[0105] The specific composition of the electrolyte provided in Comparative Example 3 is shown in Table 1.
[0106] Table 1 Electrolyte Composition
[0107]
[0108] Example 4
[0109] Example 4 provides a magnesium-manganese dry cell, the preparation method of which is as follows:
[0110] (1) Stir electrolytic manganese dioxide and conductive carbon black in a certain proportion until they are evenly mixed, wherein the mass of electrolytic manganese dioxide accounts for 90%;
[0111] (2) Use sandpaper to sand off the oxide layer on the surface of the stamped magnesium cylinder;
[0112] (3) The conductive carbon rod and the positive electrode material obtained in step 1) are hot-pressed into shape, and then wrapped with a diaphragm and filled into the magnesium cylinder polished in step (2). The magnesium cylinder is made of solid solution AZ31 magnesium alloy.
[0113] (4) Inject the electrolyte provided in Example 1, with an addition amount of 3 mL;
[0114] (5) After the electrolyte has completely wetted the positive electrode material, use a sealing machine to seal the top of the magnesium cylinder;
[0115] (6) After adding the positive electrode cap and the negative electrode bottom, the magnesium-manganese dry cell is packaged using a heat shrink tubing.
[0116] Example 5
[0117] Example 5 provides a magnesium-manganese dry cell battery, which differs from Example 4 in that: in step (4), the electrolyte provided in Example 2 is injected.
[0118] Example 6
[0119] Example 6 provides a magnesium-manganese dry cell battery, which differs from Example 4 in that: in step (4), the electrolyte provided in Example 3 is injected.
[0120] Comparative Example 4
[0121] Comparative Example 4 provides five types of magnesium-manganese dry batteries, which differ from Example 4 in that: in step (4), the electrolyte provided by Comparative Example 1 is injected into each of them.
[0122] Comparative Example 5
[0123] Comparative Example 5 provides a magnesium-manganese dry cell battery, which differs from Example 4 in that: in step (4), the electrolyte provided by Comparative Example 2 is injected.
[0124] Comparative Example 6
[0125] Comparative Example 6 provides a magnesium-manganese dry cell battery, which differs from Example 4 in that: in step (4), the electrolyte provided by Comparative Example 3 is injected.
[0126] Test case
[0127] The magnesium-manganese dry batteries provided in Examples 4-6 and Comparative Examples 4-6, after being left to stand for one day, were subjected to discharge tests using a charge-discharge device. Test method: discharge current was 10mA, and termination voltage was 0.9V.
[0128] The test curve for Example 4 can be found here. Figure 1 and Figure 2 The test curves for Examples 5 and 6 are shown below. Figure 2 . Figure 2 In the examples, Example 4 is recorded as 0.01M NaF, Example 5 as 0.05M NaF, and Example 6 as 0.1M NaF.
[0129] The test curves provided in Comparative Example 4 are shown below. Figure 3 The test curves for Comparative Examples 5 and 6, as well as Example 6, are shown in the attached diagram. Figure 4 . Figure 4In the examples, Comparative Example 5 is denoted as 0.1M Na3PO4, Comparative Example 6 is denoted as 0.1M CH3COONa, and Example 6 is denoted as 0.1M NaF.
[0130] Results analysis:
[0131] Depend on Figure 1 As can be seen, the magnesium-manganese dry cell prepared with the electrolyte provided in Example 1 of this application has a very short voltage hysteresis time, with virtually no voltage hysteresis effect. Its initial discharge voltage can reach 2.15V, and the discharge time is nearly 90 hours. The magnesium-manganese dry cell prepared with the electrolyte provided in Example 1 has a discharge capacity as high as 870mAh.
[0132] Depend on Figure 2 It is known that the concentration of sodium fluoride has a certain impact on the discharge voltage and discharge capacity of magnesium-manganese dry cell batteries. The performance of magnesium-manganese dry cell batteries decreases with increasing sodium fluoride concentration. When the sodium fluoride concentration in the electrolyte is 0.01-0.1 mol / L, the discharge time of the magnesium-manganese dry cell battery is not less than 75 hours, and the initial discharge voltage is not less than 2.1V. When the electrolyte contains 0.01 mol / L NaF, the magnesium-manganese dry cell battery has the maximum discharge capacity and open-circuit voltage.
[0133] Combination Figure 2 and Figure 3 It can be seen that, compared with Comparative Example 1 without sodium fluoride, the electrolyte provided in this application, by utilizing the combination of sodium fluoride and magnesium bromide, enables the magnesium-manganese dry cell to have a discharge time of not less than 75 hours and an initial discharge voltage of not less than 2.1V. In Comparative Example 1, without the addition of sodium fluoride, even with adjustments to the concentration of magnesium bromide, the discharge time of the obtained magnesium-manganese dry cell is still lower than that of the magnesium-manganese dry cell obtained using the electrolytes provided in Examples 1-3 of this application.
[0134] Depend on Figure 4 It can be seen that, compared with Comparative Examples 2 and 3 which added sodium sulfate and sodium acetate to the electrolyte, this application utilizes sodium fluoride in combination with magnesium bromide to improve the discharge time and discharge performance of magnesium-manganese dry batteries.
[0135] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. An electrolyte for use in magnesium-manganese dry batteries, characterized in that, The electrolyte comprises magnesium halide, sodium halide, and a solvent; the concentration of magnesium halide is 0.1-1 mol / L, the concentration of sodium halide is 0.01-0.1 mol / L, and the solvent is selected from water.
2. The electrolyte according to claim 1, characterized in that, The magnesium halide is selected from at least one of magnesium fluoride, magnesium chloride, magnesium bromide or magnesium iodide.
3. The electrolyte according to claim 2, characterized in that, The sodium halide is selected from at least one of sodium fluoride, sodium chloride, sodium bromide, or sodium iodide.
4. The electrolyte according to claim 3, characterized in that, The magnesium halide is selected from magnesium bromide, and the sodium halide is selected from sodium fluoride.
5. The electrolyte according to claim 4, characterized in that, The concentration of magnesium bromide is 0.75 mol / L, and the concentration of sodium fluoride is 0.01 mol / L.
6. The electrolyte according to claim 1, characterized in that, The solvent is selected from deionized water.
7. A method for preparing a magnesium-manganese dry cell, characterized in that, The preparation method includes: The electrolyte according to any one of claims 1-6 is injected into a magnesium cylinder filled with positive electrode material, wherein a diaphragm is provided between the positive electrode material and the inner wall of the magnesium cylinder, and a carbon rod is inserted into the positive electrode material; the magnesium cylinder is sealed, and a positive electrode cap is provided at the end of the carbon rod extending out of the magnesium cylinder to obtain the magnesium-manganese dry cell.
8. The preparation method according to claim 7, characterized in that, The positive electrode material includes manganese dioxide and conductive carbon black.
9. The preparation method according to claim 8, characterized in that, The manganese dioxide accounts for 85-92% of the total mass of the cathode material.
10. A magnesium-manganese dry cell battery, characterized in that, The magnesium-manganese dry cell is prepared by the method of any one of claims 7-9.
Citation Information
Patent Citations
Novel composite electrolytic solution applicable to magnesium-manganese dry battery
CN106410231A
Magnesium battery
JP2015050180A