Method for recycling calcium oxide-digested solid residue
By converting the solid residue from calcium oxide digestion into calcium carbonate powder, the problem of recycling and utilizing the solid residue from calcium oxide digestion is solved, achieving efficient resource utilization and environmental purification, with significant economic and environmental benefits.
Patent Information
- Application Number
- CN202311804832.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-25
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-25
AI Technical Summary
Solid residues from calcium oxide digestion account for a large proportion of light calcium production and are difficult to recycle effectively, leading to resource waste and environmental pollution.
The solid residue from calcium oxide digestion is ground into a fine powder, water is added to make a slurry, and then reacted with carbon dioxide to produce calcium carbonate powder. High-whiteness calcium carbonate powder is obtained through ultrafine processing and spray drying.
This method enables the effective recycling and utilization of solid residues from calcium oxide digestion, producing high-whiteness calcium carbonate powder. It solves the problems of resource waste and environmental pollution, and has significant economic and environmental benefits.
Abstract
Description
Technical Field
[0001] This application relates to the field of calcium oxide digestion solid residue treatment technology, and in particular to a method for recycling calcium oxide digestion solid residue. Background Technology
[0002] Calcium oxide digestion solid residue refers to the solid waste generated during the production of light calcium carbonate. In the production of light calcium carbonate, limestone is first calcined to produce calcium oxide. During the digestion process, part of the calcium oxide becomes calcium hydroxide, while the other part is difficult to digest and becomes solid residue. This residue is treated as solid waste.
[0003] In the entire production process of light calcium oxide, solid residue accounts for approximately 10-15%, which represents a huge waste of resources and also pollutes the environment. How to effectively recycle and utilize the solid residue from calcium oxide digestion is a pressing problem to be solved in this field. Summary of the Invention
[0004] The purpose of this application is to provide a new method for recycling solid residues from calcium oxide digestion.
[0005] The following technical solution is adopted in this application:
[0006] One aspect of this application discloses a method for recycling calcium oxide digestion solid residue, which includes grinding the calcium oxide digestion solid residue into fine powder, adding water to make a calcium oxide digestion solid residue slurry, subjecting the calcium oxide digestion solid residue slurry to ultrafine treatment, and simultaneously adding carbon dioxide to react. After the ultrafine treatment is completed, an ultrafine slurry is obtained, and the ultrafine slurry is spray-dried to obtain ultrafine calcium carbonate powder.
[0007] It should be noted that this application's research found that the solid residue from calcium oxide digestion mainly contains calcium oxide and calcium carbonate, with calcium carbonate being the predominant component. Therefore, this application creatively proposes to convert calcium oxide into calcium carbonate through a chemical reaction, specifically, calcium oxide is converted into calcium hydroxide, which then reacts with carbon dioxide to produce calcium carbonate. This process transforms the solid residue from calcium oxide digestion into calcium carbonate powder for recycling. The calcium carbonate powder obtained by this method includes both light and heavy calcium carbonate, exhibiting high whiteness. In one implementation of this application, the whiteness of the calcium carbonate powder exceeds 95%, achieving effective recycling of the solid residue from calcium oxide digestion. This addresses the problem of millions of tons of calcium oxide digestion residue being discarded annually, transforming it into a high-value-added calcium carbonate product with significant economic benefits. Furthermore, it also compensates for the shortage of high-whiteness calcite resources, resulting in significant economic and environmental benefits.
[0008] In one implementation of this application, the fine powder of the calcium oxide digestion solid residue has a particle size of 20-150 mesh.
[0009] In one implementation of this application, the solid content of the calcium oxide digestion solid residue slurry is 30-68%.
[0010] It should be noted that grinding the calcium oxide digestion solids into a fine powder and controlling the solids content of the calcium oxide digestion solids slurry is primarily to ensure that the calcium oxide, after being converted into calcium hydroxide, can fully contact carbon dioxide, thus facilitating its complete conversion into calcium carbonate. It is understandable that, under relatively lower requirements, calcium oxide digestion solids particles of other sizes or calcium oxide digestion solids slurries with different solids contents can also be used.
[0011] In one implementation of this application, the ultrafine processing employs a stirred mill with a grinding media of 2-8 mm, a filling rate of 70% of the grinding chamber volume, and a rotation speed of 120-900 rpm.
[0012] In one implementation of this application, the particle size of the ultrafine slurry is D90 less than 1 micrometer, and the pH value of the ultrafine slurry is less than 8.5.
[0013] In one implementation of this application, the recycling method further includes adding a dispersant during ultrafine processing.
[0014] In one implementation of this application, the dispersant is at least one of sodium pyrophosphate, sodium acrylate, and sodium tripolyphosphate.
[0015] In one implementation of this application, the amount of dispersant used is 0.3% to 1% of the total weight.
[0016] It should be noted that the role of the dispersant in this application is to ensure that the solid residue particles of calcium oxide digestion are evenly dispersed and do not precipitate or agglomerate, so that the calcium oxide can come into more complete contact with water and react to transform into calcium hydroxide to participate in the reaction. It is understood that if the calcium oxide can be made to come into full contact with water and not precipitate or agglomerate through other means, the dispersant may not be used.
[0017] In one implementation of this application, the product of spray drying is further modified to obtain ultrafine calcium carbonate powder. The modification process includes adding 0.5-1.5% by weight of a coupling agent to the spray-dried product and stirring at 900-1100 rpm for 20-45 minutes at 90-105°C.
[0018] In one implementation of this application, the coupling agent is at least one of aluminate and titanate.
[0019] In one implementation of this application, the amount of carbon dioxide used is 0.1 mol to 1.5 mol / min.
[0020] Another aspect of this application discloses calcium carbonate powder obtained by the recycling method of this application.
[0021] It should be noted that, due to the recycling method employed in this application, the calcium carbonate powder produced has the advantage of high whiteness, which can alleviate the problem of insufficient high-whiteness calcite resources, resulting in significant economic and environmental benefits. It can be understood that the calcium carbonate powder obtained by the recycling method of this application comprises, in part, the calcium carbonate originally present in the solid waste, i.e., precipitated calcium carbonate; and in part, the calcium carbonate produced by the reaction of calcium oxide and carbon dioxide, i.e., light calcium carbonate.
[0022] It should also be noted that the calcium carbonate powder obtained by the recycling method of this application has a high whiteness, which is greater than 95%, because the solid residue of calcium oxide digestion itself is calcined at high temperature and the final calcium carbonate powder is composed of light calcium carbonate and heavy calcium carbonate.
[0023] Another aspect of this application discloses the application of the calcium carbonate powder of this application in the preparation of calcite replacement materials.
[0024] It should be noted that calcite is a natural calcium carbonate mineral; therefore, the calcium carbonate powder of this application can replace calcite, especially high-whiteness calcite, to make up for the shortage of high-whiteness calcite resources.
[0025] The beneficial effects of this application are as follows:
[0026] The method for recycling solid residues from calcium oxide digestion in this application creatively converts calcium oxide in the residues into calcium carbonate, thereby obtaining high-whiteness calcium carbonate powder composed of heavy calcium carbonate and light calcium carbonate. This not only achieves effective recycling of solid residues from calcium oxide digestion, but also makes up for the shortage of high-whiteness calcite resources, resulting in significant economic and environmental benefits. Detailed Implementation
[0027] Analysis of the solid residue from calcium oxide digestion revealed the presence of calcium oxide and calcium carbonate, with calcium carbonate being the predominant component. Given that annual light calcium production exceeds tens of millions of tons, effective utilization of this residue could transform millions of tons of waste into high-value-added products, while also supplementing the shortage of high-whiteness calcite resources. Therefore, it offers significant economic and environmental benefits.
[0028] Therefore, this application creatively proposes a method for recycling calcium oxide digestion solid residue, which includes grinding the calcium oxide digestion solid residue into fine powder, adding water to make calcium oxide digestion solid residue slurry, subjecting the calcium oxide digestion solid residue slurry to ultrafine treatment, and simultaneously adding carbon dioxide to react. After the ultrafine treatment is completed, an ultrafine slurry is obtained, and the ultrafine slurry is spray-dried to obtain ultrafine calcium carbonate powder.
[0029] One implementation of this application specifically includes: collecting calcium oxide digestion residue, processing it to 80 mesh using a roller mill, then adding water to prepare a slurry containing calcium hydroxide and calcium carbonate, with a solid content of 30-68%. The resulting slurry is then fed into a stirred mill for ultrafine processing, with 0.3-1% dispersant added, while carbon dioxide is simultaneously introduced to react with the calcium hydroxide, producing calcium carbonate. The calcium carbonate in the residue is further ultrafined until the particle size is reduced to D90 less than 1 micrometer and the pH value less than 8.5. The resulting ultrafine slurry is then placed in a storage tank. Subsequent spray drying and modification processes yield an ultrafine calcium carbonate product with a high whiteness greater than 95%.
[0030] This application discloses a method for recycling calcium oxide digestion solid residue. This residue can be fully utilized, resulting in a final calcium carbonate product comprising calcium carbonate particles (light calcium carbonate) formed by the reaction of calcium hydroxide and carbon dioxide, and particles directly obtained from ultrafine calcium carbonate (heavy calcium carbonate). Light and heavy calcium carbonate differ in morphology and particle size distribution. The calcium carbonate product obtained through this method has finer particles, which can function as a solid dispersant in plastic products. This is a characteristic not found in light or heavy calcium carbonate products alone. Furthermore, because the raw material calcium oxide digestion solid residue itself undergoes high-temperature calcination, it has high whiteness, a characteristic not found in natural heavy calcium carbonate. Therefore, the calcium carbonate product obtained through this recycling method has better performance and significant economic benefits. Simultaneously, it completely solves the long-standing environmental pollution problem and the issue of high-value utilization of calcium oxide residue.
[0031] The present application will be further described in detail below through specific embodiments. The following embodiments are only for further illustration of the present application and should not be construed as limiting the present application.
[0032] Example 1
[0033] Take 100 kg of calcined 3 cm block calcium oxide, add 400 kg of water to make calcium hydroxide slurry, filter out the residue, which is the calcium oxide digestion solid residue, weigh it, and the residue weighs 12 kg.
[0034] The above residue was processed to 80 mesh using a roller mill, then added to a stirred mill for ultrafine processing. 0.6% dispersant (sodium pyrophosphate) was added, and 100% carbon dioxide was simultaneously introduced. After 50 minutes, the slurry was discharged into a storage tank. D90 = 1 micrometer. The prepared ultrafine slurry was then placed in a storage tank. After spray drying, 0.8% by weight of coupling agent (aluminate) was added, and the mixture was stirred at high speed for 30 minutes at 95 degrees Celsius and 950 rpm to obtain the calcium carbonate product in this example.
[0035] To test the whiteness of the calcium carbonate product prepared in this example, the whiteness meter was first calibrated using a standard whiteness sample. Then, the sample to be tested was prepared by pressing the powder material into a flat, solid, smooth, texture-free, defect-free, and stain-free sample plate using a powder press. The sample plate preparation steps included:
[0036] 1. Place the clean glass slide with the frosted side facing up in the base and press it down with the sample tube.
[0037] 2. Fill the sample tube with the powder sample and tap the bottom of the sample tube on the table several times to ensure the powder is fully incorporated.
[0038] 3. After placing the briquette on the powder, screw on the constant pressure pressurizer.
[0039] 4. Turn the pressure regulator handle clockwise. When the constant pressure is reached, the handle will automatically slip, indicating that the pressure has stopped.
[0040] 5. After loosening the handle counterclockwise, remove the pressure device, take out the pressure block, and screw on the bottom cover. Continue until the powder is pressed down.
[0041] 6. Turn the sample tube over, unscrew the base, gently rotate and push the glass slide to remove it. The preparation of the powder standard sample plate is now complete.
[0042] After the sample plate was prepared, it was placed in a whiteness meter to test its whiteness, and the value was read. The result was 96.3%.
[0043] Furthermore, 1 kg of the calcium carbonate product prepared in this example was taken, 2 kg of HDPE was added, and granulation was carried out using a twin-screw granulator to make a sample. The tensile strength of the sample was tested and compared with the tensile strength of pure HDPE. At the same time, the sample was subjected to transmitted light detection.
[0044] Tensile strength was measured using a HY-0580 microcomputer-controlled electronic universal testing machine. The specific steps were as follows: Granulated masterbatch was used to prepare international standard test strips via an injection molding machine. The strips were then fixed to the testing machine using clamps. The machine was started to begin tensile testing, and the tensile strength value was displayed simultaneously. The data at which the strip broke was the tensile strength of the strip. For transmitted light testing, the sample was placed 20-30 cm in front of a 100-watt incandescent lamp, and the uniformity of the sample's interior was observed visually.
[0045] Test results show that the tensile strength of the HDPE sample with added calcium carbonate is 66.07 MPa, while the tensile strength of pure HDPE is 55.7 MPa. This result indicates that adding calcium carbonate prepared by the method of this invention can significantly improve the tensile strength of HDPE resin, providing a reinforcing effect. This further illustrates that, at the same particle size, the degree of dispersibility determines the quality of the mechanical properties in practical applications.
[0046] Transmitted light test results showed that the HDPE sample containing calcium carbonate was uniform inside, with no dark spots, indicating that calcium carbonate had good dispersibility.
[0047] Comparative Example 1
[0048] Take 1 kg of modified light calcium carbonate product (commercially available light calcium carbonate), D90 = 1 micrometer. Add 2 kg of HDPE, granulate using a twin-screw granulator, and prepare a sample. Test its tensile strength according to the method in Example 1. The tensile strength is 53.12 MPa, while the tensile strength of pure HDPE is 55.7 MPa. The results show that although the particle size of commercially available light calcium carbonate is also D90 = 1 micrometer, it does not have a reinforcing effect on the tensile strength of HDPE resin in practical applications. This further illustrates that, at the same particle size, the quality of dispersibility determines the quality of the mechanical properties in practical applications. Transmitted light detection was performed using the same method as in Example 1. The results showed that the sample contained many dark spots, indicating poor dispersibility of calcium carbonate.
[0049] Comparative Example 2
[0050] Take 1 kg of modified heavy calcium carbonate product (commercially available heavy calcium carbonate), D90 = 1 micrometer. Add 2 kg of HDPE, granulate using a twin-screw granulator, and prepare a sample. According to the test in Example 1, its tensile strength is 55.3 MPa, compared to 55.7 MPa for pure HDPE. The results show that adding commercially available heavy calcium carbonate, with a particle size of D90 = 1 micrometer, while not reinforcing the tensile strength of HDPE resin in practical applications, does not significantly reduce the loss of tensile strength. The overall effect is better than light calcium carbonate, but there is still a significant difference compared to the product prepared by this invention. This further illustrates that, at the same particle size, the quality of dispersibility determines the quality of the mechanical properties in practical applications. Transmitted light detection was performed using the same method as in Example 1. The results showed that some dark spots were distributed inside the sample, indicating poor dispersibility of calcium carbonate.
[0051] The above description, in conjunction with specific embodiments, provides a further detailed explanation of this application and should not be construed as limiting the specific implementation of this application to these descriptions. Those skilled in the art to which this application pertains can make several simple deductions or substitutions without departing from the concept of this application.
Claims
1. A method for recycling solid residue from calcium oxide digestion, characterized in that: The process includes grinding calcium oxide digestion solid residue into fine powder, adding water to make calcium oxide digestion solid residue slurry, subjecting the calcium oxide digestion solid residue slurry to ultrafine treatment, adding carbon dioxide at the same time to react, obtaining ultrafine slurry after ultrafine treatment, and spray drying the ultrafine slurry to obtain ultrafine calcium carbonate powder. The ultrafine calcium carbonate powder is composed of light calcium carbonate and heavy calcium carbonate, and has a whiteness greater than 95%. The ultrafine treatment uses a stirred mill with a grinding media of 2-8 mm, a filling rate of 70% of the grinding chamber volume, and a rotation speed of 120-900 rpm. The particle size of the ultrafine slurry is less than 1 micrometer (D90), and the pH value of the ultrafine slurry is less than 8.
5. This also includes adding dispersants during ultrafine processing; The dispersant is at least one of sodium pyrophosphate, sodium acrylate, and sodium tripolyphosphate; The amount of the dispersant used is 0.3-1% of the total weight.
2. The recycling method according to claim 1, characterized in that: The fine powder of the calcium oxide digestion solid residue has a particle size of 20-150 mesh.
3. The recycling method according to claim 1, characterized in that: The solid content of the calcium oxide digestion solid residue slurry is 30-68%.
4. The recycling method according to claim 1, characterized in that: It also includes modifying the spray-dried product to obtain ultrafine calcium carbonate powder. The modification process includes adding 0.5-1.5% by weight of a coupling agent to the spray-dried product and stirring at 900-1100 rpm for 20-45 minutes at 90-105°C.
5. The recycling method according to claim 4, characterized in that: The coupling agent is at least one of aluminate and titanate.
6. The recycling method according to any one of claims 1-5, characterized in that: The amount of carbon dioxide used is 0.1 mol to 1.5 mol / min.
Citation Information
Patent Citations
Recycling utilization method of digestion waste slag
CN105036583A
Preparation method of light calcium carbonate for cigarette paper
CN113104878A