Light guide film and method of manufacturing the same
By using a composite material of poly(4-methyl-1-pentene), styrene-acrylonitrile copolymer and polyethylene grafted with glycidyl methacrylate, the problems of scratch resistance and yellowing resistance of light guide films were solved, and a light guide film with high light transmittance and resistance to damp heat was prepared.
Patent Information
- Application Number
- CN202311731329.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-15
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-15
AI Technical Summary
Existing light guide film materials are insufficient in terms of scratch resistance and yellowing resistance, and the addition of anti-aging agents will reduce light transmittance. Styrene-acrylonitrile copolymers are not heat-resistant and are prone to moisture absorption, which affects optical transmittance.
A light guide film was prepared by extrusion molding using a composite material of poly(4-methyl-1-pentene), styrene-acrylonitrile copolymer and polyethylene grafted with glycidyl methacrylate, thereby improving the compatibility and stability of the material.
The prepared light guide film has high light transmittance, good scratch resistance and damp heat resistance, and is not prone to yellowing after long-term use, thus maintaining good light guiding performance.
Smart Images

Figure CN117777607B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of light guide film technology, and in particular to a light guide film and its preparation method. Background Technology
[0002] Light guide film is a material used in optical display devices. Its main function is to improve the brightness uniformity of the display device. It can effectively guide and diffuse light, and transmit light evenly to the entire area of the display.
[0003] Light guide films are commonly used in backlight modules, LCD displays, and light guide plates to improve light utilization efficiency and uniformity. For example, in some backlight modules, point light sources are typically mounted on the side or back of the light guide film. Incident light enters from the side or back of the light guide film, which effectively guides the light from the light source across the entire film area, allowing the light energy to propagate and scatter fully. Light exits from the front of the light guide film, meaning the point light source is converted into a surface light source through the light guide film.
[0004] The materials used for light guide films include poly(4-methyl-1-pentene) (TPX) and styrene-acrylonitrile copolymer (SAN), both of which have good light transmittance.
[0005] Poly(4-methyl-1-pentene) (TPX) has a visible light transmittance of up to 90%, is lightweight, has a water absorption rate of only 0.01%, is not prone to moisture absorption, has good heat resistance, and can be used for a long time at 150℃ without softening. However, it has poor scratch resistance and is prone to yellowing when exposed to light sources for a long time. Some methods of adding anti-aging agents to prevent yellowing will reduce its light transmittance and light guiding performance.
[0006] Styrene-acrylonitrile copolymer (SAN) has a visible light transmittance of up to 88%, is oil-resistant, acid and alkali-resistant, scratch-resistant, and light-resistant. However, its heat distortion temperature is 82-105℃, which makes it not heat-resistant. Furthermore, its water absorption rate is 0.66%, which makes it prone to moisture absorption and reduces its optical transmittance. Summary of the Invention
[0007] This application provides a light guide film made of a composite material of poly(4-methyl-1-pentene) and styrene-acrylonitrile copolymer, to improve the poor scratch resistance and yellowing of poly(4-methyl-1-pentene) material under long-term exposure to light sources, as well as the reduced light transmittance and light guiding performance of poly(4-methyl-1-pentene) material alone, and the poor heat resistance and moisture absorption of poly(4-methyl-1-pentene) styrene-acrylonitrile copolymer alone, which reduces its optical transmittance. Therefore, this application adopts the following solution.
[0008] In the first aspect, this application proposes a light guide film and adopts the following technical solution.
[0009] A light guide film, wherein the raw materials for preparing the light guide film include poly(4-methyl-1-pentene), styrene-acrylonitrile copolymer and polyethylene grafted glycidyl methacrylate.
[0010] By adopting the above technical solution, poly(4-methyl-1-pentene) has a branched structure with isobutyl groups grafted onto the alkane chain, and the polymer chains are wound into a helical shape, making it a semi-crystalline polymer where crystalline and amorphous forms coexist. The styrene monomer in the styrene-acrylonitrile copolymer imparts good mechanical properties, while the acrylonitrile monomer imparts good chemical corrosion resistance. Polyethylene grafted with glycidyl methacrylate has ester and epoxy groups linked to the alkane chain, which is beneficial for combining alkane chains and cyano groups, improving the compatibility of poly(4-methyl-1-pentene) and the styrene-acrylonitrile copolymer, and enhancing the stability of the three-dimensional structure. The light guide film made from this composite material has high light transmittance, good scratch resistance, and resistance to damp heat, and is not prone to yellowing after long-term use.
[0011] As a preferred embodiment of the light guide film, the raw materials of the light guide film, calculated by mass percentage, include 55-70% of the poly4-methyl-1-pentene, 28-44% of the styrene-acrylonitrile copolymer, and 1-2% of the polyethylene-grafted glycidyl methacrylate.
[0012] By adopting the above technical solution, the components of the material have good compatibility, and the resulting membrane has high light transmittance, good toughness, and weather resistance.
[0013] As a preferred embodiment of the light guide film, the grafting rate of the polyethylene grafted with glycidyl methacrylate is 0.5-0.6%.
[0014] By adopting the above technical solution, the polyethylene grafted glycidyl methacrylate has suitable viscosity and can better promote the compatibility of poly(4-methyl-1-pentene) and styrene-acrylonitrile copolymer.
[0015] As a preferred embodiment of the light guide film, the polyethylene used to prepare the polyethylene grafted with glycidyl methacrylate is high-density polyethylene.
[0016] By adopting the above technical solution, high-density polyethylene has stronger strength and adhesion than low-density polyethylene. In this light guide film material, it is more adaptable to improving the compatibility of poly(4-methyl-1-pentene) and styrene-acrylonitrile copolymer, thereby improving the material's impact resistance.
[0017] Secondly, this application also proposes a method for preparing a light guide film, and adopts the following technical solution.
[0018] A method for preparing a light guide film as described above involves feeding the poly(4-methyl-1-pentene), the styrene-acrylonitrile copolymer, and the polyethylene-grafted glycidyl methacrylate into an extruder, stirring and melting them together, and finally extruding them to form a light guide film.
[0019] By adopting the above technical solution, the extrusion molding method can better integrate the three components to obtain the raw material for the light guide film. The raw material is then made into the light guide film. Compared with some molding methods, such as injection molding, casting, blow molding, calendering, etc., the yield rate is higher.
[0020] One possible method for preparing the light guide film is to set the maximum temperature inside the extruder to 250-260℃.
[0021] By adopting the above technical solution, the poly(4-methyl-1-pentene), the styrene-acrylonitrile copolymer, and the polyethylene-grafted glycidyl methacrylate are appropriately melt-composite.
[0022] One possible method for preparing the light guide film is as follows: the extrudate is first made into a film material, then the film material is passed through a molding die, the film material is heated and molded by the molding die, and then the light guide film is obtained by cutting and edge grinding.
[0023] By adopting the above technical solutions and controlling the quality of the film material, the yield rate of the light guide film can be improved, thus enhancing product quality.
[0024] One alternative method for preparing the light guide film is to perform a drying process before feeding the styrene-acrylonitrile copolymer into the extruder.
[0025] By adopting the above technical solution, the styrene-acrylonitrile copolymer has a high moisture absorption rate. It is first dried and then compounded with other materials to reduce the impact of the moisture carried by the styrene-acrylonitrile copolymer on the light transmittance and weather resistance of the composite material.
[0026] In summary, the light guide film and its preparation method of this application have the following beneficial effects: Grafting glycidyl methacrylate onto polyethylene improves the compatibility of poly(4-methyl-1-pentene) and styrene-acrylonitrile copolymer and enhances the stability of the three-dimensional structure. The light guide film made from this composite material has high light transmittance and good light guiding uniformity. The light guide film also has good scratch resistance and damp heat resistance, and can maintain good light guiding performance under long-term irradiation by a light source. Attached Figure Description
[0027] Figure 1 It is a light guide film with a prismatic microstructure. Detailed Implementation
[0028] The main sources of materials used in the following embodiments and comparative examples are as follows: Poly(4-methyl-1-pentene) (TPX), supplied by Ningbo Shengyilong Plastics Co., Ltd. Styrene-acrylonitrile copolymer (SAN), supplied by Dongguan Zhanyu Plastic Raw Materials Co., Ltd. Polyethylene grafted with glycidyl methacrylate (HDPE-G-GMA), supplier: Dongguan Shenghao Plastic Raw Materials Co., Ltd., model SH030, grafting rate 0.5-0.6%, density 0.92 g / cm³. 3 .
[0029] Examples 1-4 An example of preparing a light guide film was described. First, the styrene-acrylonitrile copolymer was baked at 80°C for 2 hours to remove moisture, thereby reducing the expansion rate of the prepared material.
[0030] Poly(4-methyl-1-pentene), styrene-acrylonitrile copolymer and polyethylene grafted glycidyl methacrylate are fed into an extruder. The screw speed of the extruder is 500 r / min. The temperature of the front section of the extruder is set to 220-240℃, the temperature of the middle section is set to 240-250℃, and the temperature of the rear section is set to 250-260℃. The materials are melted and mixed evenly during the stirring process, and finally extruded and granulated.
[0031] The extruded granules are remelted and pressed into a roll film using rollers with flat upper and lower surfaces. The roll film is then passed through a forming die. The upper die of the forming die has diamond-shaped teeth, and the pressure of the upper die is set at 3-5 kN. The lower die of the forming die heats the film material to a temperature of 100-150℃, pressing the film material together to form a light guide film with a prismatic microstructure. Figure 1 As shown, the light guide film of this structure achieves uniform display in multiple directions; after pressing and cooling, it is die-cut to obtain a sheet film, and the edges of the sheet film are polished to obtain the light guide film.
[0032] In the above method for preparing the light guide film, the raw materials of the light guide film, calculated by mass percentage, contain 55-70% of the aforementioned poly-4-methyl-1-pentene, 28-44% of the aforementioned styrene-acrylonitrile copolymer, and 1-2% of the aforementioned polyethylene-grafted glycidyl methacrylate. Specifically, Examples 1-4 were produced according to the formulations in Table 1.
[0033] Table 1. Raw Material Formulation of Light Guide Film Comparative Example 1 This comparative example uses the same preparation method and raw material mass ratio as Example 3. The only difference is that polyethylene grafted with maleic anhydride is used instead of polyethylene grafted with glycidyl methacrylate. Extrusion granulation is also performed using an extruder, and the membrane material and light guide film are also prepared in the same way.
[0034] The supplier of the polyethylene grafted maleic anhydride (LDPE-G-MAH) is Dongguan Shenghao Plastic Raw Materials Co., Ltd., with the model number PE-12H, a grafting rate of 0.9%, and a density of 0.93 g / cm³. 3 .
[0035] Comparative Example 2 This comparative example uses the same preparation method and raw material mass ratio as Example 3. The only difference is that pure poly(4-methyl-1-pentene) is used as the raw material for preparing the light guide film. The same extruder is used for extrusion granulation, and the same film material and light guide film are prepared.
[0036] Comparative Example 3 This comparative example uses the same preparation method and raw material mass ratio as Example 3. The only difference is that pure styrene-acrylonitrile copolymer is used as the raw material for preparing the light guide film. The same extruder is used for extrusion granulation, and the same film material and light guide film are prepared.
[0037] Comparative Example 4-5 Comparative Examples 4-5 used the same preparation method and raw material types as Examples 1-4. The only difference was that the mass percentage ratio of poly(4-methyl-1-pentene), styrene-acrylonitrile copolymer and polyethylene-grafted glycidyl methacrylate was adjusted. The specific formulation is shown in Table 2 below. Extrusion granulation was carried out using an extruder in the same way, and the film material and light guide film were prepared in the same way.
[0038] Table 2 Raw material formulation for light guide film Experimental Example 1 The properties of the light guide materials prepared in Examples 1-4 and Comparative Examples 1-5 were tested.
[0039] The light transmittance of the membrane material was tested according to GB / T 2410-2008.
[0040] Notched impact strength: According to the test standard GB / T1843-2008, notched impact strength test of cantilever beam membrane material.
[0041] Scratch resistance test: The test is conducted in accordance with GB / T 36952-2018, and the result is expressed by visually inspecting the surface of the membrane material for scratches.
[0042] Xenon lamp irradiation: wavelength 290–800 nm, irradiance 550 W / m 2They were continuously irradiated at room temperature of 25°C for 20 days.
[0043] High temperature and high humidity test: temperature 80℃, relative humidity 95%, duration 500h. After the high temperature and high humidity test, place at room temperature for 2h, then visually inspect the appearance, and finally test the light transmittance according to standard GB / T 2410-2008.
[0044] The test results for the above items are statistically summarized in Table 3.
[0045] Table 3. Test results of light guide material performance The test results in Table 3 show that the membrane material prepared using the schemes in Examples 1-4 has high light transmittance, high impact strength, scratch resistance, is not prone to yellowing under long-term lamp illumination, and is resistant to damp heat, and is generally superior to the schemes in Comparative Examples 1-5.
[0046] Comparing Comparative Example 1 and Example 3, Comparative Example 1 used polyethylene grafted with maleic anhydride instead of polyethylene grafted with glycidyl methacrylate. The light transmittance, impact strength, scratch resistance, anti-yellowing performance under long-term lamp illumination, and resistance to damp heat of the prepared film were all inferior to those of Example 3. It can be seen that the polyethylene grafted with glycidyl methacrylate used in Example 3 is better. The reason is that polyethylene grafted with glycidyl methacrylate can improve the compatibility of poly(4-methyl-1-pentene) and styrene-acrylonitrile copolymer, improve the stability of the three-dimensional structure, so that the prepared composite material has high light transmittance, good scratch resistance, resistance to damp heat, and is not easy to yellow after long-term use. Polyethylene grafted with maleic anhydride basically does not have this effect.
[0047] Comparing Comparative Examples 2, 3, and 3, Comparative Example 2 used pure poly(4-methyl-1-pentene) as the raw material for preparing the light guide film, while Comparative Example 3 used pure styrene-acrylonitrile copolymer as the raw material for preparing the light guide film. The light transmittance, impact strength, scratch resistance, anti-yellowing performance under long-term lamp illumination, and damp heat resistance of the films prepared by Comparative Examples 2 and 3 were all inferior to those of Example 3. It can be seen that the film prepared by Example 3 using poly(4-methyl-1-pentene), styrene-acrylonitrile copolymer, and polyethylene grafted glycidyl methacrylate as raw materials has better optical properties, mechanical properties, and weather resistance.
[0048] Comparing Comparative Examples 4, 5, and 1-4, Examples 1-4 used 55-70% poly(4-methyl-1-pentene), 28-44% styrene-acrylonitrile copolymer, and 1-2% polyethylene grafted glycidyl methacrylate as composite materials. Comparative Example 4 used 40% poly(4-methyl-1-pentene), 50% styrene-acrylonitrile copolymer, and 10% polyethylene grafted glycidyl methacrylate as composite materials. Comparative Example 5 used 80% poly(4-methyl-1-pentene), 15% styrene-acrylonitrile copolymer, and 5% polyethylene grafted glycidyl methacrylate as composite materials. The membranes prepared in Examples 1-4 showed better light transmittance, impact strength, scratch resistance, anti-yellowing performance under long-term lamp irradiation, and resistance to damp heat than the membranes prepared in Comparative Examples 4 and 5. It is evident that the formulations in Examples 1-4 can achieve better results.
[0049] The light guide films prepared by the schemes in Examples 1-4 can be used to prepare display light guide devices, key films, automotive light guide devices, etc. Under long-term light source irradiation, high temperature and high humidity environment, scratches, collisions and other usage conditions, they can maintain good light transmission performance and good appearance for a long time, and have high application value.
[0050] The above are merely some embodiments of this application. The scope of protection of this application is not limited to the above embodiments. For those skilled in the art, any improvements and modifications made without departing from the inventive design of this application should also fall within the scope of protection of this application.
Claims
1. A light guide film, characterized in that, The raw materials for preparing the light guide film, by weight percentage, consist of 55-70% poly4-methyl-1-pentene, 28-44% styrene-acrylonitrile copolymer and 1-2% polyethylene grafted glycidyl methacrylate. The grafting rate of the polyethylene grafted with glycidyl methacrylate is 0.5-0.6%; The polyethylene used to prepare the polyethylene-grafted glycidyl methacrylate is high-density polyethylene.
2. A method for preparing the light guide film as described in claim 1, characterized in that, The poly(4-methyl-1-pentene), the styrene-acrylonitrile copolymer, and the polyethylene-grafted glycidyl methacrylate are fed into an extruder, stirred evenly and melt-mixed, and finally extruded and molded, and the extrudate is made into a light guide film.
3. The method for preparing the light guide film according to claim 2, characterized in that, The maximum temperature inside the extruder is set to 250-260℃.
4. The method for preparing the light guide film according to claim 2, characterized in that, The process of making the extrudate into a light guide film includes: first, making the extrudate into a film material, then passing the film material through a molding die, heating and molding the film material through the molding die, and then cutting and grinding the edges to obtain the light guide film.
5. The method for preparing the light guide film according to claim 2, characterized in that, The styrene-acrylonitrile copolymer is dried before being fed into the extruder.
Citation Information
Patent Citations
SAN material, preparation method thereof and refrigerator vacuum sealing box
CN113789017A
Laminated film
JP2007210175A
Film, method for producing the same, and method for producing LED package using the same
JP2012153775A