A high-temperature high-hardness high-strength silicone resin composition

By crosslinking hydrogen-based polysiloxanes containing hexafluorocyclobutyl aryl ether structures with organic silsesquioxane resins, a silicone resin composition with high hardness and high strength at high temperatures is formed, solving the problem of hardness and strength loss of phenyl silicone resins at high temperatures. This composition is suitable for laser devices and integrated circuit packaging.

CN117777943BActive Publication Date: 2026-11-24NEW MATERIAL INST OF SHANDONG ACADEMY OF SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311819366.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-27
Publication Date
2026-11-24
Estimated Expiration
2043-12-27

AI Technical Summary

Technical Problem

Existing phenyl silicone resins suffer significant loss of hardness and strength at high temperatures, failing to meet the stable bonding requirements of optoelectronic devices in high-temperature environments.

Method used

A silicone resin composition with high hardness and high strength at high temperature is formed by crosslinking a hydrogen-based polysiloxane containing a hexafluorocyclobutyl aryl ether structure with an organic silsesquioxane resin and curing it through addition.

Benefits of technology

It maintains high hardness and strength at high temperatures, and its material structure is stable, making it suitable for applications such as laser devices and integrated circuit packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117777943B_ABST
    Figure CN117777943B_ABST
Patent Text Reader

Abstract

This invention discloses a high-hardness, high-strength silicone resin composition for high-temperature applications. The composition comprises an alkenyl-containing organic silsesquioxane resin, a hydrogen-based polysiloxane containing a hexafluorocyclobutyl aryl ether structure, a catalyst, an inhibitor, and a tackifier. First, this invention prepares a hydrogen-based polysiloxane containing a hexafluorocyclobutyl aryl ether structure as a crosslinking agent. Then, hexafluorocyclobutyl aryl ether is introduced into the main chain backbone of the organic silsesquioxane resin through addition curing, resulting in a silicone resin composition with a room temperature hardness of 70D or higher and a tensile strength of 25 MPa or higher, and a hardness of 50D or higher and a tensile strength of 5 MPa or higher at 180°C. Therefore, it possesses high hardness and high strength at high temperatures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a high-hardness, high-strength silicone resin composition for high-temperature applications, belonging to the field of organosilicon polymer technology. Background Technology

[0002] Silicone resin is a cross-linked semi-inorganic polymer with a three-dimensional cross-linked Si-O-Si bond as the molecular backbone and organic groups attached to silicon atoms. Its unique organic-inorganic hybrid structure endows it with excellent properties such as high temperature resistance, low dielectric constant, weather resistance, chemical resistance, and electrical insulation. It has important application value in fields such as sealing and bonding of optoelectronic devices, such as bonding of laser devices and packaging of integrated circuits, where high temperature resistance is required.

[0003] Taking laser device bonding as an example, the core component of laser equipment—the laser that generates the laser light—usually requires adhesives to fix and bond optical components, electronic components, and mechanical parts. Due to the special working environment of laser devices, adhesives are required to have high temperature resistance to ensure they do not fail or deform under the high temperatures generated during device operation; good chemical stability to resist potential chemical corrosion; high hardness and strength at both room temperature and high temperature to ensure the bonded components do not loosen or detach at operating temperatures; and good sealing performance to prevent external dust, moisture, or gases from entering the laser device and affecting its performance and stability. These requirements are common in the field of optoelectronic devices. For these requirements, phenyl silicone resin is an ideal material. Phenyl silicone resin has a high refractive index, typically above 1.50, and a light transmittance greater than 90%, especially in terms of temperature resistance, which is significantly better than conventional organic resins. However, conventional phenyl silicone resin also suffers from the problems of other polymer materials: at high temperatures, due to increased molecular thermal energy, molecular chains undergo untangling and creeping, increasing mobility, weakening intermolecular interactions, and resulting in a decrease in overall material hardness and strength. Therefore, minimizing the loss of hardness and strength of phenyl silicone resin at high temperatures through molecular structure design is an urgent problem to be solved.

[0004] CN100465233C discloses an addition-curable organopolysiloxane resin composition and an optical material, which comprises an organopolysiloxane resin containing phenyl and alkenyl groups, and an organohydrogen polysiloxane (H) containing phenyl groups. e R 5 f SiO (4-e-f) / 2The resin composition consists of a diluent and a catalyst. By limiting the content of phenyl and alkenyl groups in the resin structure, a cured body with a hardness of 60-100 Shore D at 25°C and a hardness that remains at 40-100 Shore D at 150°C is obtained. The beneficial effects of this patent are "transparency, high hardness and strength in the cured state, and the ability to maintain its hardness at high temperatures," but it does not provide data on strength at room temperature and high temperatures, nor does it explain whether its strength can be maintained at high temperatures. The main chain of this resin composition contains only Si-O structures, with low molecular polarity and low intermolecular cohesive energy density. Its hardness and strength at room temperature mainly come from high crosslinking density. At high temperatures, high crosslinking density prevents the free movement of molecular chains, so the hardness decreases only slightly. Moreover, high crosslinking density cannot achieve forced high-elastic deformation when the material is subjected to thermal shock, and it is prone to brittle fracture, which is an unreliable factor in applications with alternating high and low temperatures. CN113105863A discloses an ultra-high hardness silicone resin film and its preparation method. The hardness of the cured product can reach 80 Shore D at room temperature, but the hardness and strength at high temperatures were not investigated. Currently, there are no reports of silicone resin compositions that can maintain high hardness and high strength at high temperatures. Summary of the Invention

[0005] Based on the above-mentioned technological status and application requirements, this invention provides a high-hardness and high-strength silicone resin composition for high temperatures. This invention first prepares a hydrogen-based polysiloxane containing a hexafluorocyclobutyl aryl ether structure as a crosslinking agent, and then introduces hexafluorocyclobutyl aryl ether into the main chain backbone of an organic silsesquioxane resin through addition curing. This yields a silicone resin composition with a room temperature hardness of 70D or higher and a tensile strength of 25 MPa or higher, and a hardness of 50D or higher and a tensile strength of 5 MPa or higher at 180°C. Therefore, it possesses high hardness and high strength characteristics at high temperatures.

[0006] This invention is achieved through the following technical solution: a high-hardness, high-strength silicone resin composition at high temperatures, comprising the following five components:

[0007] (A) The average unit formula is (R) 1 R 2 2SiO 0.5 ) a (R 3 SiO 1.5 ) b Organic silsesquioxane resins

[0008] Among them, R 1 It is one or more of vinyl or alkenyl groups having 3 to 10 carbon atoms, preferably vinyl; R 2 It is a saturated hydrocarbon group or aryl group with 1 to 10 carbon atoms, preferably a saturated hydrocarbon group with 1 to 3 carbon atoms; R 3It is aryl, preferably phenyl; a+b=1, the value of a is 0<a≤0.5, preferably 0.1≤a≤0.5; the value of b is 0.5≤b<1, preferably 0.5≤b≤0.9;

[0009] (B) Hydrogen-based polysiloxanes with the average unit formula shown below, containing a hexafluorocyclobutyl aryl ether structure.

[0010]

[0011] Among them, R 4 It is a saturated hydrocarbon group or aryl group with 1 to 10 carbon atoms, preferably a saturated hydrocarbon group with 1 to 3 carbon atoms; R 5 It is a hexafluorocyclobutyl aryl ether group; m is 1 or 2. If the value of m exceeds the specified range, the product viscosity will be high, which is not conducive to operation.

[0012] (C) A catalyst capable of catalyzing hydrosilylation reactions, preferably a complex of chloroplatinic acid with a diene or 1,3-divinyltetramethyldisiloxane or a similar platinum metal group catalyst.

[0013] (D) Inhibitors, preferably compounds containing alkynyl groups and polyvinyl groups;

[0014] (E) A tackifier that promotes adhesion between the resin and the substrate, preferably a phenyl silicone resin containing one or both of vinyl and hydrogen groups and one of epoxy, acyl, and alkoxy groups.

[0015] For every 100 parts by weight of component (A) of the organosilsesquioxane resin, the amount of component (B) is 20-100 parts by weight, and the molar ratio of hydrogen groups in (B) to alkenyl groups in (A) is 0.8-1.5:1, preferably 1-1.2:1; the amount of component (E) is 1-10 parts by weight, preferably 2-5 parts by weight; the amount of component (C) is 1-30 ppm, preferably 5-15 ppm; the amount of component (D) is 50-2000 ppm, preferably 300-1000 ppm.

[0016] The preparation method of the above component (B) containing a hydrogen-based polysiloxane with a hexafluorocyclobutyl aryl ether structure includes the following steps:

[0017] (1) Hexafluorocyclobutylaryl ether silane (R 6 O)R 4 2SiR 5 SiR 4 2(OR 6 Add acidic catalyst and acetic acid (I) to the reaction flask, mix well, heat to 60-65℃ and react for 30-60 minutes, then distill off the low-boiling substances;

[0018] (2) Add hydrogen-based terminator HR to the remaining solution in (1). 4 2SiOSiR 4 After 2 hours, raise the temperature to 45-55℃ and add acetic acid (II) dropwise. After the addition is complete, add acetic anhydride dropwise. Maintain the temperature at 45-55℃ for 2-3 hours.

[0019] (3) After the reaction is completed, the mixture is allowed to stand and separate into layers. The organic phase is separated, washed with water until neutral, dried, and the filtrate is distilled under reduced pressure to obtain a hydrogen-based polysiloxane containing a hexafluorocyclobutyl aryl ether structure.

[0020] In step (1), the raw material structure R 6 It is a saturated hydrocarbon group with 1 to 10 carbon atoms, preferably methyl and ethyl.

[0021] The acidic catalyst used in step (1) is one or more of hydrochloric acid, concentrated sulfuric acid, trifluoromethanesulfonic acid, strong acid ion exchange resin, and solid acid, preferably hydrochloric acid or trifluoromethanesulfonic acid.

[0022] In step (2), R 4 It is a saturated hydrocarbon group or aryl group with 1 to 10 carbon atoms.

[0023] In steps (1) and (2), hexafluorocyclobutylaryl ether silane, acidic catalyst, acetic acid (I), and HR are used. 4 2SiOSiR 4 The molar ratio of 2H, acetic acid (II), and acetic anhydride is 1:0.001-0.01:0.5-5:0.5-3:0.6-5:0.5-5.

[0024] Compared with the prior art, the beneficial effects of the present invention are:

[0025] 1. A cured product is obtained by hydrosilylation of alkenylphenyl silsesquioxane resin and hydrogen-based polysiloxane containing hexafluorocyclobutyl aryl ether structure. It has no release of small molecules, regular structure, is not prone to material defects, and has excellent mechanical properties, temperature resistance and chemical stability.

[0026] 2. At high temperatures, the T-structure of phenylsilsesquioxane, the rigid four-membered ring in the hexafluorocyclobutylaryl ether segment, and the conjugated system can effectively resist the increased molecular chain mobility caused by temperature rise, providing stable structural support and maintaining hardness; the presence of ether bonds increases the toughness of the material, alleviates the generation of concentrated stress, and enables it to maintain high strength at high temperatures: hardness above 50D and tensile strength above 5MPa at 180℃.

[0027] 3. Hydrogen-based polysiloxanes can be prepared by copolymerizing hexafluorocyclobutyl aryl ether silane and dialkoxy silane. The composition and hydrogen content can be adjusted according to the application requirements, thereby adjusting the content of hexafluorocyclobutyl aryl ether in the cured product to meet different application needs. Attached Figure Description

[0028] Figure 1 The nuclear magnetic resonance hydrogen spectrum of the hexafluorocyclobutyl aryl ether-containing hydrogen polysiloxane (PFCB-H1) obtained in Example 1 of this invention is shown. Detailed Implementation

[0029] The present invention will be further described below with reference to the embodiments and accompanying drawings.

[0030] The structural formula is (CH2=CHMe2SiO) 0.5 ) m (PhSiO 1.5 ) n The vinyl silicone resin is prepared by acid-catalyzed hydrolysis and alkali-catalyzed polycondensation of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane and phenyltrimethoxysilane in a certain proportion; its structural formula is (HMe2SiO). 0.5 ) x (PhSiO 1.5 ) y The hydrogen-based silicone resin is prepared by hydrolysis of tetramethyldisiloxane and phenyltrimethoxysilane in a certain proportion under acid catalysis; the tackifier phenylvinylhydroepoxysilane can be prepared by co-hydrolysis and polycondensation of phenyltrimethoxysilane, glycidyltrimethoxysilane, vinylmethyldimethoxysilane and methylhydrodimethoxysilane in a molar ratio of 1:1:0.25:0.275.

[0031] The synthetic route for hexafluorocyclobutylaryl ether silanes is as follows:

[0032]

[0033] The specific preparation steps are as follows:

[0034] (1) Preparation of 4-(trifluorovinyloxy)phenyldimethylethoxysilane by Grignard method

[0035] Take 24.52g of magnesium powder and place it in a reaction flask under nitrogen protection. Add two iodine crystals and 200ml of tetrahydrofuran. While stirring continuously, add 232g (0.23mol) of 4-(trifluoroethyleneoxy)bromobenzene diluted with 600ml of tetrahydrofuran. Keep the temperature at 35℃. The color of the reaction solution gradually turns dark brown. The reaction is completed in about 4 hours. Continue the reaction for another 2 hours.

[0036] Under nitrogen protection, the Grignard reagent was added dropwise to 400 mL of dimethyldiethoxysilane (272.84 g, 1.84 mol) diluted in tetrahydrofuran. The temperature was maintained at 0–5 °C. After the addition was complete, the temperature was slowly raised to room temperature and stirred for 30 min. Then, the temperature was further increased to 70 °C and the reaction was carried out for 17 h. After the reaction was completed, the mixture was filtered through diatomaceous earth, and the filtrate was distilled under reduced pressure to obtain 124.56 g of a colorless and transparent liquid.

[0037] (2) Thermal cyclization of 4-(trifluorovinyloxy)phenyldimethylethoxysilane yields hexafluorocyclobutylaryl ether silane

[0038] 124 g of 4-(trifluorovinyloxy)phenyldimethylethoxysilane was placed in a reaction flask and heated to 170 °C under nitrogen protection for 18 h. After cooling to room temperature, unreacted starting material was removed by vacuum distillation to obtain 93.5 g of a pale yellow transparent liquid, namely hexafluorocyclobutylaryl ether silane.

[0039] Example 1

[0040]

[0041] 27.6 g of hexafluorocyclobutylaryl ether silane, 0.03 g of trifluoromethanesulfonic acid, and 3.1 g of acetic acid were added sequentially to a reaction flask equipped with a thermometer, stirrer, dropping funnel, and reflux condenser. The mixture was stirred thoroughly and heated to 65 °C for 1 hour. Low-boiling-point substances were then removed by vacuum distillation. The remaining liquid was added to HR... 4 2SiOSiR 4 2H(R 4 6.7 g of CH3 was added, and after heating to 50 °C, 4.1 g of acetic acid was slowly added dropwise. After the addition was complete, 5.1 g of acetic anhydride was added dropwise, and the reaction was maintained at 50 °C for 2 h. After the reaction was completed, the mixture was cooled to room temperature, and the reaction solution was allowed to stand and separate into layers. The organic phase was separated. The organic phase was washed with water until neutral, and then dried overnight with anhydrous calcium chloride. The calcium chloride was removed by filtration, and the filtrate was distilled under reduced pressure to remove low-boiling substances, yielding a hexafluorocyclobutyl aryl ether-containing hydrogen-based polysiloxane (PFCB-H1) with the structure shown above.

[0042] 1 HNMR (with) Figure 1 The peak at δ = 7–7.5 ppm is a characteristic peak of Si-C6H5-O, the peak at δ = 4.4–4.5 ppm is attributed to Si-H, and the peak at δ = 0–0.5 ppm is a characteristic peak of Si-CH3.

[0043] Example 2

[0044] Add 66.0 g of hexafluorocyclobutylaryl ether silane, 0.05 g of trifluoromethanesulfonic acid, and 6.0 g of acetic acid sequentially to a reaction flask equipped with a thermometer, stirrer, dropping funnel, and reflux condenser. Mix thoroughly and heat to 65°C for 1 hour. Then, remove low-boiling-point substances by vacuum distillation. Add the remaining liquid to HR... 4 2SiOSiR 4 2H(R 4 8.1 g of CH3 was added, and after heating to 50 °C, 7.2 g of acetic acid was slowly added dropwise. After the addition was complete, 12.3 g of acetic anhydride was added dropwise, and the reaction was maintained at 50 °C for 2 hours. After the reaction was completed, the mixture was cooled to room temperature, and the reaction solution was allowed to stand and separate into layers. The organic phase was separated. The organic phase was washed with water until neutral, and then dried overnight with anhydrous calcium chloride. The calcium chloride was removed by filtration, and the filtrate was distilled under reduced pressure to remove low-boiling substances, yielding a hexafluorocyclobutylaryl ether-containing hydrogen-based polysiloxane (PFCB-H2) with the following structure.

[0045]

[0046] Example 3

[0047] 100 parts by mass have the structural formula (CH2=CHMe2SiO) 0.5 ) 0.25 (PhSiO 1.5 ) 0.75 An addition-curable silicone resin composition was prepared by using 60 parts by weight of vinyl silicone resin, PFCB-H1 prepared in Example 1, 0.27 parts by weight of a solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex (platinum content 3000 ppm), 0.048 parts by weight of 1-ethynylcyclohexanol, and 3 parts by weight of phenylvinylhydroepoxy silicone resin as tackifiers.

[0048] Example 4

[0049] 100 parts by mass have the structural formula (CH2=CHMe2SiO) 0.5 ) 0.2 (PhSiO 1.5 ) 0.8 An addition-curable silicone resin composition was prepared by using 89 parts by weight of vinyl silicone resin, PFCB-H2 prepared in Example 2, 0.3 parts by weight of a solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex (platinum content 3000 ppm), 0.055 parts by weight of 1-ethynylcyclohexanol, and 3 parts by weight of phenylvinylhydroepoxy silicone resin as tackifiers.

[0050] Example 5

[0051] 100 parts by mass have the structural formula (CH2=CHMe2SiO) 0.5 ) 0.15(PhSiO 1.5 ) 0.85 A vinyl silicone resin, 36 parts by weight of PFCB-H1 prepared in Example 1, 0.23 parts by weight of a solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex (platinum content 3000 ppm), 0.041 parts by weight of 1-ethynylcyclohexanol and 3 parts by weight of phenylvinylhydroepoxy silicone resin as tackifiers were used to prepare an addition-curable silicone resin composition.

[0052] Example 6

[0053] 100 parts by mass have the structural formula (CH2=CHMe2SiO) 0.5 ) 0.15 (PhSiO 1.5 ) 0.85 A vinyl silicone resin, 67 parts by weight of PFCB-H2 prepared in Example 2, 0.3 parts by weight of a solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex (platinum content 3000 ppm), 0.054 parts by weight of 1-ethynylcyclohexanol and 4 parts by weight of phenylvinylhydroepoxy silicone resin as tackifiers were used to prepare an addition-curable silicone resin composition.

[0054] Comparative Example 1

[0055] 100 parts by mass have the structural formula (CH2=CHMe2SiO) 0.5 ) 0.15 (PhSiO 1.5 ) 0.85 Vinyl silicone resin, 32 parts by weight (HMe2SiO) 0.5 ) 0.4 (PhSiO 1.5 ) 0.6 An addition-curable silicone resin composition was prepared by using 0.22 parts by weight of a solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex (platinum content 3000 ppm), 0.04 parts by weight of 1-ethynylcyclohexanol, and 3 parts by weight of phenylvinylhydroepoxy silicone resin as tackifiers.

[0056] Comparative Example 2

[0057] 100 parts by mass have the structural formula (CH2=CHMe2SiO) 0.5 ) 0.25 (PhSiO 1.5 ) 0.75 Vinyl silicone resin, 37 parts by weight (HMe2SiO) 0.5 ) 0.6 (PhSiO 1.5 ) 0.4, 0.23 parts by mass of a solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex (platinum content: 3000 ppm), 0.041 parts by mass of 1-ethynylcyclohexanol, and 3 parts by mass of a phenylvinylhydrido epoxy silicone resin as a tackifier to prepare an addition-curable silicone resin composition.

[0058] The silicone resin compositions of Examples 3, 4, 5, 6 and Comparative Examples 1, 2 were poured into circular stainless steel molds (diameter 50 mm, depth 6 mm) and dumbbell-shaped stainless steel molds (gauge length 50 mm, width 10 mm, depth 4 mm) lined with a polytetrafluoroethylene coating, respectively, and cured at 80 °C for 1 h, then heated to 150 °C for further curing for 3 h. The hardness of the cured samples was tested at 25 °C and on a 180 °C hot plate according to GB / T 2411-2008, respectively. The tensile strength was tested at 25 °C and 180 °C according to GB / T 1040-2006, respectively. The tensile strength at 180 °C was measured in a high-temperature chamber attached to a universal electronic testing machine.

[0059] Table 1: Hardness and tensile strength of the cured products of Examples 3, 4, 5, 6 and Comparative Examples 1, 2

[0060]

[0061] As shown in Table 1, compared with Comparative Examples 1-2, the cured product of the silicone resin material prepared by the present invention exhibits high hardness and high strength at both room temperature and high temperature. The room temperature hardness reaches 70D or above, the tensile strength is 25 MPa or above, the hardness at 180 °C is 50D or above, and the tensile strength is 5 MPa or above, which is suitable for application fields such as bonding of laser devices and packaging of integrated circuits.

[0062] The above is a description of the preferred embodiments of the present invention, but is not intended to limit the protection scope of the present invention. Various modifications or changes that can be made by those skilled in the art without creative efforts based on the technical solutions of the present invention still fall within the protection scope of the present invention.

Claims

1. A high-hardness, high-strength silicone resin composition for high temperatures, characterized in that, It includes the following five components: (A) the average unit formula is (R 1 R 2 2SiO 0.5 ) a (R 3 SiO 1.5 ) b organic silsesquioxane resin wherein R 1 is one or more of vinyl or alkenyl groups having 3 to 10 carbon atoms; R 2 is a saturated hydrocarbon group having 1 to 10 carbon atoms or an aryl group; R 3 is an aryl group; a + b = 1, the value of a is 0 < a < 0.5, and the value of b is 0.5 < b < 1. (B) Hydrogen-based polysiloxanes with the following average unit formula containing a hexafluorocyclobutylaryl ether structure. Among them, R 4 It is a saturated hydrocarbon group or aryl group with 1 to 10 carbon atoms; R 5 It is a hexafluorocyclobutylaryl ether group; m is 1 or 2; (C) Catalysts capable of catalyzing hydrosilylation reactions; (D) Inhibitor; (E) Tackifiers that promote adhesion between resin and substrate.

2. The high-hardness, high-strength silicone resin composition at high temperature as described in claim 1, characterized in that, The preparation method of the hydrogen-based polysiloxane containing the hexafluorocyclobutylaryl ether structure includes the following steps: (1) Hexafluorocyclobutylaryl ether silane (R 6 O)R 4 2SiR 5 SiR 4 2(OR 6 Acidic catalyst and acetic acid (I) are added to the reaction vessel, mixed evenly, heated to 60-65℃ and reacted for 30-60 minutes, and then the low-boiling substances are distilled off. (2) Add hydrogen-based end-capping agent HR to the remaining solution in (1). 4 2SiOSiR 4 After 2 hours, raise the temperature to 45-55℃ and add acetic acid (II) dropwise. After the addition is complete, add acetic anhydride dropwise. Maintain the temperature at 45-55℃ for 2-3 hours. (3) After the reaction is complete, let it stand to separate the layers, separate the organic phase, wash with water until neutral, dry, and distill the filtrate under reduced pressure to obtain hydrogen-based polysiloxane containing hexafluorocyclobutylaryl ether structure.

3. The high-hardness, high-strength silicone resin composition at high temperature as described in claim 2, characterized in that, The R 6 It is a saturated hydrocarbon group with 1 to 10 carbon atoms.

4. The high-hardness, high-strength silicone resin composition at high temperature as described in claim 2, characterized in that, The acidic catalyst used in step (1) is one or more of hydrochloric acid, concentrated sulfuric acid, trifluoromethanesulfonic acid, strong acid ion exchange resin, and solid acid.

5. The high-hardness, high-strength silicone resin composition at high temperature as described in claim 2, characterized in that, In steps (1) and (2), hexafluorocyclobutylaryl ether silane, acidic catalyst, acetic acid (I), and HR are used. 4 2SiOSiR 4 The molar ratio of 2H, acetic acid (II), and acetic anhydride is 1:0.001-0.01:0.5-5:0.5-3:0.6-5:0.5-5.

6. A high-hardness, high-strength silicone resin composition at high temperature as described in claim 1 or 2, characterized in that, in, R 1 For vinyl; R 2 It is a saturated hydrocarbon group with 1 to 3 carbon atoms; R 3 It is a phenyl group; a+b=1, the value of a is 0.1≤a≤0.5; the value of b is 0.5≤b≤0.9; the R... 4 It is a saturated hydrocarbon group with 1 to 3 carbon atoms.

7. The high-hardness, high-strength silicone resin composition at high temperature as described in claim 1, characterized in that, The catalyst (C) capable of catalyzing the hydrosilylation reaction is a complex of chloroplatinic acid with a diene or 1,3-divinyltetramethyldisiloxane.

8. The high-hardness, high-strength silicone resin composition at high temperature as described in claim 1, characterized in that, The (D) inhibitor is a compound containing an alkynyl group and polyvinyl groups.

9. The high-hardness, high-strength silicone resin composition at high temperature as described in claim 1, characterized in that, The tackifier (E) that promotes the adhesion between the resin and the substrate is a phenyl silicone resin containing one or both of vinyl and hydrogen groups and one of epoxy, acyl, and alkoxy groups.

10. A high-hardness, high-strength silicone resin composition at high temperature according to any one of claims 7-9, characterized in that, For every 100 parts by mass of component (A) of the organosilsesquioxane resin, the amount of component (B) is 20-100 parts by mass, and the molar ratio of hydrogen groups in (B) to alkenyl groups in (A) is 0.8-1.5:1; the amount of component (E) is 1-10 parts by mass; the amount of component (C) is 1-30 ppm; and the amount of component (D) is 50-2000 ppm.

Citation Information

Patent Citations

  • An addition-curable organopolysiloxane resin composition and an optical material

    CN100465233C

  • Ultrahigh-hardness silicon resin film as well as preparation method and application thereof

    CN113105863A

  • Heat-resistant silicon resin capable of being cured at room temperature, and preparation method thereof

    CN107459652A

  • Process for the production of organosilsesquioxanes

    US20070122636A1