Electrochemical lithium extraction device and method based on flexible electrodes

The electrochemical oxidation-reduction lithium extraction device with flexible electrode H-type structure solves the problems of leakage, complex assembly and high cost of existing devices, and achieves efficient and economical lithium ion extraction and cycle stability, while reducing the content of impurity ions.

CN117778717BActive Publication Date: 2026-11-24EAST CHINA UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410135489.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-31
Publication Date
2026-11-24
Estimated Expiration
2044-01-31

AI Technical Summary

Technical Problem

Existing lithium extraction devices from salt lake brine suffer from problems such as leakage, complex assembly, large amount of anion exchange membrane, uneven flow field, slow adsorption kinetics, and short cycle life, resulting in high cost and high impurity ion content.

Method used

An electrochemical oxidation-reduction lithium extraction device based on flexible electrodes is adopted. The flexible electrodes are rolled up to form an H-shaped structure, which simplifies the device structure, reduces the use of anion exchange membranes, achieves uniform flow field and fast adsorption-desorption kinetics, and improves the device life.

Benefits of technology

It achieves high selectivity for lithium ions, fast adsorption-desorption kinetics, uniform flow field, low polarization, long service life, and good economy, while reducing the amount of anion exchange membrane used and the content of impurity cations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117778717B_ABST
    Figure CN117778717B_ABST
Patent Text Reader

Abstract

This invention discloses an electrochemical redox lithium extraction device and method based on flexible electrodes. The lithium extraction device includes an anode pipe, a cathode pipe, and an intermediate pipe connecting the anode pipe and the cathode pipe. The anode pipe is filled with an unactivated electrode, and the cathode pipe is filled with an activated electrode; both the activated and unactivated electrodes are flexible electrodes. The anode pipe is used to introduce a desorption solution, and the cathode pipe is used to introduce a lithium-containing solution. An anion exchange membrane is disposed in the intermediate pipe to separate the lithium-containing solution from the desorption solution. The electrochemical redox lithium extraction device based on flexible electrodes provided by this invention has the advantages of low leakage, uniform flow field, simple device, fast adsorption kinetics, long cycle life, high lithium-ion selectivity, and low anion exchange membrane usage, and significantly reduces the cost of electrochemical lithium extraction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of resource recycling technology, specifically to an electrochemical oxidation-reduction lithium extraction device and method based on flexible electrodes. Background Technology

[0002] With the emergence and development of electric vehicles and other clean energy and energy storage devices, the demand for lithium has exploded, making lithium a crucial metal resource for the nation's new energy development strategy. Therefore, lithium extraction from salt lake brine, which has lower extraction costs, has attracted increasing attention. However, my country's salt lake brines are characterized by high magnesium-to-lithium or sodium-to-lithium ratios, posing new challenges to lithium extraction from salt lakes.

[0003] Methods for lithium extraction from salt lake brine include chemical precipitation, solvent extraction, membrane methods, and adsorption. Adsorption is considered the most promising method due to its high selectivity, non-toxicity, and cost-effectiveness. The key to lithium extraction via adsorption is finding an adsorbent with selective adsorption of lithium ions. Ion sieves are widely used due to their high adsorption capacity and selectivity. However, in traditional chemical acid desorption processes, dissolution loss is unavoidable, significantly reducing the cycle stability of ion sieves and hindering their industrial application. Electrochemical redox technology is the most effective method to reduce dissolution loss. This technology combines the properties of electrochemistry and ion exchange, depositing electroactive materials onto a conductive substrate to create selective electrodes. The oxidation / reduction potential can be controlled electrochemically to reversibly introduce / release ions from the solution, achieving selective separation of target ions. Lithium iron phosphate (LFP), lithium manganese oxide (LMO), lithium titanate (LTO), and lithium manganese iron phosphate are the most commonly used electrochemical active materials. Currently, pilot-scale or commercially operational electrochemical lithium extraction devices all adopt a plate-and-frame structure. This structure uses anion exchange membranes to separate rigid cathodes and anodes, which are continuously stacked. Flat plates are used at both ends to press together to achieve selective extraction of lithium ions. However, this structure has problems such as complex assembly, easy leakage and liquid cross-contamination, large amount of ion exchange membranes, and many impurity ions in the eluent. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to provide an electrochemical oxidation-reduction lithium extraction device and method based on flexible electrodes. The electrochemical lithium extraction device has the characteristics of not being prone to leakage, uniform flow field, simple device, fast adsorption kinetics, long cycle life, high lithium ion selectivity, and low amount of anion exchange membrane, and greatly reduces the cost of electrochemical lithium extraction.

[0005] In a first aspect, the present invention provides an electrochemical oxidation-reduction lithium extraction device based on a flexible electrode, comprising an anode pipe, a cathode pipe, and an intermediate pipe connecting the anode pipe and the cathode pipe; the anode pipe is filled with an unactivated electrode, and the cathode pipe is filled with an activated electrode, both the activated electrode and the unactivated electrode being flexible electrodes; the anode pipe is used to pass through a desorption solution, and the cathode pipe is used to pass through a lithium-containing solution; an anion exchange membrane is disposed in the intermediate pipe, the anion exchange membrane being used to separate the lithium-containing solution from the desorption solution.

[0006] Please see the appendix Figure 1 The plate-and-frame electrochemical lithium extraction device widely used in the existing technology is based on rigid electrode materials. It generally consists of an outermost clamping plate, a cathode-anion exchange membrane-anode-anion exchange membrane-cathode stacked continuously (generally, commercially operating devices consist of 100 to 200 pairs of electrodes), and a flow channel. Brine and desorption solution enter the anode and cathode through the bottom inlet and flow out through the top outlet, respectively.

[0007] This plate-and-frame lithium extraction device has several drawbacks in application: First, it relies entirely on a small cavity composed of anion exchange membranes and anodes to contain the brine and desorption solution, making it prone to leakage or cross-contamination, which is detrimental to industrial operation. Second, this type of lithium extraction device requires a large number of anion exchange membranes, resulting in high costs. Third, since the selectivity of anion exchange membranes currently cannot exceed 95%, the extensive use of anion exchange membranes will cause the content of impurity cations in the desorption solution to exceed the standard, requiring more complex processes to remove impurity cations to obtain relatively pure LiCl. Finally, due to the continuous decrease in hydraulic head, the liquid flow velocity near the inlet is significantly greater than that far from the inlet, and due to the rough surface of the rigid electrodes, the flow field inside each flow channel is not uniform. This causes "dead zones" to easily appear in the electrode cavity, resulting in problems such as active material polarization, inconsistent electrode adsorption and desorption termination times, slow adsorption kinetics, and long single cycle times. Active material polarization will reduce the service life of the entire device.

[0008] The electrochemical lithium extraction device provided by this invention is completely different from the plate-and-frame structure. (See attached diagram) Figure 2As shown, the electrochemical lithium extraction device of the present invention is based on a flexible, rollable electrode, which consists of an anode pipe, a cathode pipe, and an intermediate pipe connecting the anode and cathode pipes. The flexible electrode is rolled up and placed into the anode and cathode pipes. The anode pipe serves as the anode cavity, and the cathode pipe serves as the cathode cavity, respectively containing the desorption solution and brine. This not only greatly simplifies the complex stacking structure in plate-and-frame lithium extraction devices but also avoids leakage or cross-contamination problems. By sandwiching a single anion exchange membrane in the intermediate pipe, selective permeation of anions in the desorption solution and brine can be achieved, thereby significantly reducing the number of anion exchange membranes used. This not only reduces operating costs and improves economic efficiency but also significantly reduces the content of impurity cations in the desorption solution due to the reduced membrane area. Furthermore, due to the simplified structure, the flow channels between the brine and desorption solution in this device are smoother and the flow field is more uniform, resulting in fast adsorption-desorption kinetics, less polarization of active substances, and a longer service life of the device.

[0009] In this invention, the arrangement of the anode pipe, cathode pipe and intermediate pipe is not limited. In a preferred embodiment, the anode pipe and cathode pipe are parallel to each other, and the anode pipe, cathode pipe and intermediate pipe together form an H-shaped structure.

[0010] In this invention, the shape of the anode and cathode pipes is not limited; for example, they can be cylindrical or prismatic, with cylindrical being preferred.

[0011] In this invention, the cavities in the anode and cathode pipes are preferably cylindrical, so that when the flexible electrode is wound into a roll and placed into the anode and cathode pipes, the rolled electrode can better fit against the wall of the cavity. Furthermore, the diameter of the cylindrical cavity is not limited in this invention; however, considering industrial requirements, it is generally set to 1m or more.

[0012] In this invention, an intermediate pipe connects the anode and cathode pipes on both sides. A single anion exchange membrane sandwiched in the intermediate pipe separates the desorption solution in the cathode pipe from the lithium-containing solution in the cathode pipe. In some embodiments, to facilitate fixing and replacing the anion exchange membrane, the intermediate pipe includes a first intermediate pipe connected to the anode pipe and a second intermediate pipe connected to the cathode pipe. The cross-sections of the first and second intermediate pipes can be provided with tanks for placing the anion exchange membrane. The first and second intermediate pipes can be sealed together using flanges or other mechanisms.

[0013] In this invention, the area of ​​the anion exchange membrane can be determined based on the current density during lithium extraction, and it is necessary to ensure that the amount of anions corresponding to this current density is less than the maximum exchange capacity of the anion exchange membrane.

[0014] In this invention, the anode pipe, cathode pipe, and intermediate pipe can be made of plastic, resin, or corrosion-resistant metal materials. The intermediate pipe is preferably made by integral molding with the anode pipe and cathode pipe.

[0015] In this invention, the flexible electrode is prepared by immersing a flexible electrode substrate material in a precursor solution containing an active substance, removing it, coating its surface with a hydrophilic modifier, and then drying it to obtain a hydrophilic flexible electrode. The flexible electrode substrate material is preferably a carbon-based flexible electrode substrate material, including but not limited to one or more of graphene, carbon nanotubes, carbon nanofibers, conductive polymers, carbon cloth, carbon felt, and graphite felt.

[0016] In some embodiments of the present invention, the precursor solution includes an active substance, a binder, and an organic solvent. The active substance includes, but is not limited to, one or more of lithium iron phosphate, lithium manganese oxide, lithium manganese iron phosphate, and lithium titanate.

[0017] It should be noted that in this invention, "lithium iron phosphate" refers to LiFePO4, and "lithium manganese oxide" includes one or more of various lithium manganese compounds, such as LiMn2O4 and Li4Mn5O4. 12 Li 1.6 Mn 1.6 O4, Li 1.33 Mn 1.67 O4, etc., lithium manganese iron phosphate includes compounds with different doping ratios, and lithium titanate includes Li2TiO3, Li4Ti5O, etc. 12 Li4TiO4, Li2Ti3O7, etc.

[0018] In some embodiments of the present invention, the adhesive includes, but is not limited to, at least one of polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene, and aqueous polystyrene ester.

[0019] In some embodiments of the present invention, the organic solvent includes, but is not limited to, at least one of N-methylpyrrolidone, N-ethylpyrrolidone, N-vinylpyrrolidone, dimethylformamide, and dimethylacetamide.

[0020] In some embodiments of the present invention, the hydrophilic modifier includes, but is not limited to, at least one of polystyrene, polyethylene glycol, polyvinyl chloride, polyoxymethylene, epoxy resin, polyglycolic acid, lignin, cellulose, and hemicellulose.

[0021] In some embodiments of the present invention, the mass ratio of the organic solvent, active material, binder, and hydrophilic modifier is 10–20:8–10:0.01–1:0.01–1. Preferably, the mass ratio is 20:8:0.2:0.2. This ratio has a relatively large amount of organic solvent compared to conventional formulations, allowing the precursor solution to easily penetrate the interior of the flexible electrode and form a uniform electrode layer.

[0022] In some embodiments of the present invention, if the coating thickness on the flexible electrode substrate material is high, a small amount of conductive agent can be selectively added to the precursor solution. The conductive agent includes, but is not limited to, at least one of carbon black, acetylene black, graphite, carbon fiber, carbon nanotubes, graphene, and composite conductive paste.

[0023] In some embodiments of the present invention, after the flexible electrode substrate material is removed from the precursor solution, a portion of the organic solvent can be removed, for example, 5% to 85% of the organic solvent can be removed. Solvent removal methods include air drying, spin drying, and general drying. Furthermore, the electrode can be further dried in an oven (pre-drying the heated electrode) for a period of time. The temperature inside the oven can be between 30°C and 50°C, for example, 30°C, 35°C, 40°C, 45°C, 50°C, etc.

[0024] In some embodiments of the present invention, after coating with a hydrophilic modifier, the hydrophilic modifier in the membrane is removed by heating. The heating includes drying the flexible electrode substrate material in an oven at 30°C to 60°C to remove ≥90wt% of organic solvent, followed by further heating in a muffle furnace to 150°C to 380°C. The drying temperature in the oven can be 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, etc.; the drying temperature in the muffle furnace can be 150°C, 200°C, 250°C, 300°C, 350°C, 380°C, etc.; and the drying time can be 1–10 hours, for example, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 8 hours, 10 hours, etc.

[0025] In some embodiments of the present invention, the activation of the electrode includes the following steps:

[0026] An activation device is provided, the activation device comprising an anode chamber, a cathode chamber and a diaphragm; wherein, a salt solution is disposed in the anode chamber, and a conductive electrode and an oxidant solution are disposed in the cathode chamber;

[0027] The electrode to be activated is placed into the salt solution in the anode chamber;

[0028] The electrode to be activated is connected to the positive terminal of the power supply, and the conductive electrode in the cathode cavity serves as the counter electrode and is connected to the negative terminal of the power supply. A constant current is applied to the electrode to be activated for electro-activation.

[0029] In some embodiments of the present invention, the oxidant solution includes Fe 2+ Fe 3+ Cu 2+ Cu + I2, I 3- Sn 4+ Cr 3+ Cd 2+ Pb 2+ PO4 3- V 3+ Sn 2+ HCOOH, HCHO, CH3OH, SbO + VO 2+ H2MoO4, MnO 4- 、Tl 3+ Ag + A solution of at least one of the following. The concentration of the oxidant solution can be 0.001 to 10 mol / L, for example 0.001, 0.01, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 2, 3, 4, 5, 6, 7, 8, 9, 10 mol / L, etc.

[0030] In some embodiments of the present invention, the salt solution includes solutions containing Cl- and SO4. 2- SO3 2- NO 3- NO 2- PO4 3- CO3 2- A solution of at least one of the soluble salts of chlorate and perchlorate. The concentration of the salt solution can be 0.1 to 10 mol / L, for example 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 2, 3, 4, 5, 6, 7, 8, 9, 10 mol / L, etc.

[0031] In some embodiments of the present invention, the conductive electrode is an inert conductive electrode; further, the conductive electrode includes at least one of carbon electrode, graphite electrode, carbon cloth electrode, titanium electrode, glassy carbon electrode, carbon felt electrode, platinum electrode, gold electrode, stainless steel electrode, copper electrode, silver electrode, aluminum electrode, and metal alloy electrode.

[0032] In some embodiments of the present invention, the activation voltage can be 0.3 to 1V, for example 0.3V, 0.4V, 0.5V, 0.6V, 0.7V, 0.8V, 0.9V, 1.0V, etc.; the activation time can be 0.1 to 100h, for example 0.1h, 1h, 5h, 10h, 20h, 30h, 40h, 50h, 60h, 70h, 80h, 90h, 100h, etc.

[0033] In addition, detailed descriptions of the hydrophilic flexible electrode and activation process are found in patent application 202210656926.0 filed with the State Intellectual Property Office on June 10, 2022 (publication date: August 5, 2022) and patent application 202211254215.7 filed with the State Intellectual Property Office on October 13, 2022 (publication date: December 27, 2022), which are incorporated herein by reference in their entirety.

[0034] Secondly, the present invention provides an electrochemical redox method for lithium extraction, comprising the following steps:

[0035] The above-mentioned electrochemical oxidation-reduction lithium extraction device based on flexible electrodes is provided;

[0036] A desorption solution is introduced into the anode pipe of the electrochemical lithium extraction device, and a lithium-containing solution is introduced into the cathode pipe of the electrochemical lithium extraction device.

[0037] The flexible electrodes in the anode and cathode pipes are connected to a power source to extract lithium.

[0038] In some embodiments of the present invention, the lithium-containing solution (i.e., catholyte) in the cathode conduit includes brine or other lithium-rich solutions.

[0039] In some embodiments of the present invention, the desorption solution (i.e., anolyte) in the anode pipe can be one or more lithium-containing solutions such as lithium chloride solution, lithium bromide solution, lithium fluoride solution, lithium nitrate solution, lithium acetate solution, lithium oxalate solution, lithium sulfate solution, lithium acetate solution, and lithium formate solution; the concentration of the desorption solution can be 0.01 to 1 M, for example, 0.01 M, 0.1 M, 0.2 M, 0.3 M, 0.4 M, 0.5 M, 0.6 M, 0.7 M, 0.8 M, 0.9 M, 1 M, etc.

[0040] In this invention, the liquid introduced into the anode and cathode pipes is in a flowing state, and the flow rate of the liquid is generally controlled between 0.1 and 10 m / s, preferably between 0.5 and 5 m / s. If the flow rate is too fast, energy will be wasted; if the flow rate is too slow, mass transfer will be hindered, causing electrode polarization and thus affecting the lithium extraction effect.

[0041] In some embodiments of the present invention, the electrochemical redox lithium extraction method further includes the following steps:

[0042] After lithium extraction is completed, the flexible electrodes in the anode and cathode channels are removed, cleaned, and exchanged to continue lithium extraction.

[0043] Repeat the above steps to cycle and extract lithium until the lithium content in the cathode solution is below 10 ppm.

[0044] Lithium is recovered from the anolyte.

[0045] In the aforementioned electrochemical redox lithium extraction process, lithium ions in the cathode solution are selectively adsorbed by the flexible electrode in the cathode channel until adsorption equilibrium is reached. Then, after exchanging the cathode and anode, when electrochemical redox lithium extraction continues, the lithium ions adsorbed by the flexible electrode desorb and enter the anolyte. By repeating these lithium extraction steps, lithium ions in the cathode solution are separated and enriched in the anolyte.

[0046] In some embodiments of the present invention, the lithium extraction voltage can be 0.3 to 1.2V, for example 0.3V, 0.4V, 0.5V, 0.6V, 0.7V, 0.8V, 0.9V, 1.0V, 1.1V, 1.2V, etc.; the lithium extraction time can be 1 to 100 hours, for example 1 hour, 5 hours, 10 hours, 20 hours, 30 hours, 40 hours, 50 hours, 60 hours, 70 hours, 80 hours, 90 hours, 100 hours, etc.

[0047] The number of cycles for lithium extraction is determined based on factors such as the lithium concentration in the cathode solution. In some embodiments of the present invention, the number of cycles can be 3 to 500.

[0048] In some embodiments of the present invention, a method for recovering lithium from the anolyte includes: concentrating the anolyte to obtain crude water and crude lithium salt. Further, Na₂CO₃ may be added to the concentrated anolyte to obtain crude lithium carbonate.

[0049] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0050] 1. The electrochemical oxidation-reduction lithium extraction device based on flexible electrodes provided by the present invention can achieve selective adsorption / desorption of lithium. The device has a simple configuration and has the advantages of fast adsorption / desorption kinetics, uniform flow field inside the cavity, low polarization, long service life, low leakage, and good economy.

[0051] 2. The electrochemical oxidation-reduction lithium extraction device based on flexible electrodes provided by the present invention uses only a single anion exchange membrane, which greatly reduces the membrane area of ​​the lithium extraction device, thereby significantly reducing the content of impurity cations in the desorption solution. Attached Figure Description

[0052] Figure 1 This is a schematic diagram of a plate-and-frame lithium extraction device in the prior art;

[0053] Figure 2 This is a schematic diagram of the H-shaped columnar lithium extraction device of the present invention;

[0054] Figure 3 for Figure 2 An exploded schematic diagram of the H-shaped columnar lithium extraction device;

[0055] Figure 4 This is a process route diagram for electrochemical oxidation-reduction lithium extraction according to an embodiment of the present invention;

[0056] Figure 5 The adsorption kinetics (a) and cycling stability (b) of Example 1 and Comparative Example 1 are shown.

[0057] Figure 6 Bar charts showing the equilibrium adsorption time and equilibrium adsorption capacity of Examples 2-6 and Comparative Examples 2-5;

[0058] The labels in the diagram are as follows: 1. Anode pipe; 11. Anode cavity; 2. Cathode pipe; 21. Cathode cavity; 3. Intermediate pipe; 4. Anion exchange membrane; 5. Flexible anode cylindrical roll; 6. Flexible cathode cylindrical roll. Detailed Implementation

[0059] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, so that those skilled in the art can better understand and implement the present invention. However, the embodiments described are not intended to limit the present invention.

[0060] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0061] Unless otherwise specified, the experimental methods used in the following examples are conventional methods, and the materials and reagents used are commercially available.

[0062] Example 1

[0063] Please see the appendix Figure 2-3This embodiment provides an electrochemical oxidation-reduction lithium extraction device based on a flexible electrode. The device has an overall H-shaped columnar structure, specifically including an anode pipe 1 and a cathode pipe 2. The anode pipe 1 has an anode cavity 11, and the cathode pipe 2 has a cathode cavity 21. The anode cavity 11 and the cathode cavity 21 are connected by an intermediate pipe 3. The anode cavity 11 is filled with a flexible anode cylindrical roll 5, and the cathode cavity 21 is filled with a flexible cathode cylindrical roll 6. Both the flexible anode cylindrical roll 5 and the flexible cathode cylindrical roll 6 are connected to an external power source via electrodes. An anion exchange membrane 4 is sandwiched within the intermediate pipe 3.

[0064] In this embodiment, both the flexible anode cylindrical roll and the flexible cathode cylindrical roll are obtained by winding a flexible electrochemical lithium extraction electrode. The preparation method of the flexible electrochemical lithium extraction electrode is as follows:

[0065] (1) Weigh LiMn2O4 ion sieve, PVDF binder, NMP solvent, and polyvinyl chloride hydrophilic modifier according to the mass ratio of 8:0.2:20:0.2. First, mix PVDF, LiMn2O4 ion sieve and NMP. Then, immerse the carbon cloth electrode in the precursor solution. After 1 hour, take it out, coat it with the weighed polyvinyl chloride for surface modification, and then dry it to obtain hydrophilic flexible electrochemical lithium extraction electrodes A and B.

[0066] (2) Electrode A is used as the anode, and the solution in the anode cavity is 0.01M LiCl solution; a titanium plate is used as the cathode, and the solution in the cathode cavity is 0.5M CuCl2 solution, 10A / m 2 The activated electrode A was obtained by constant current activation for 10 hours.

[0067] Electrochemical oxidation-reduction lithium extraction was performed using the activated A electrode prepared above in brine. The specific operation is as follows:

[0068] Electrodes A and B were rolled into cylindrical shapes and filled into the cathode and anode chambers of the electrochemical lithium extraction device, respectively. A brine solution was introduced into the cathode chamber, and a 0.01M LiCl solution was introduced into the anode chamber. The flow rate was 15 A / m. 2 Lithium extraction was performed under constant current until the voltage reached 0.8V, and then under constant voltage of 0.8V for 1 hour for selective lithium extraction. After lithium extraction, the surfaces of electrodes A and B were rinsed. Then, using electrode B as the cathode and electrode A as the anode, the electrodes were placed in the cathode chamber and anode chamber respectively for secondary lithium extraction. The lithium extraction operation conditions were the same as the initial lithium extraction, and the cycle was repeated 500 times.

[0069] Comparative Example 1

[0070] The only difference between Comparative Example 1 and Example 1 is that Comparative Example 1 uses a titanium mesh as the electrode substrate material and uses a flat plate structure device for electrochemical lithium extraction.

[0071] Example 2

[0072] The only difference between Example 2 and Example 1 is that in Example 2, LiFePO4 is used instead of LiMn2O4 as the active material.

[0073] Comparative Example 2

[0074] The only difference between Comparative Example 2 and Comparative Example 1 is that Comparative Example 2 uses LiFePO4 instead of LiMn2O4 as the active material.

[0075] Example 3

[0076] The only difference between Example 3 and Example 2 is that in Example 3, 2% by mass of acetylene black was added to the precursor solution as an additional conductive agent.

[0077] Example 4

[0078] The only difference between Example 4 and Example 1 is that in Example 4, Li2TiO3 is used instead of LiMn2O4 as the active material.

[0079] Comparative Example 3

[0080] The only difference between Comparative Example 3 and Comparative Example 1 is that Comparative Example 3 uses Li2TiO3 instead of LiMn2O4 as the active material.

[0081] Example 5

[0082] The only difference between Example 5 and Example 1 is that Example 5 uses LiFe 0.4 Mn 0.6 PO4 replaces LiMn2O4 as the active material.

[0083] Comparative Example 4

[0084] The only difference between Comparative Example 4 and Comparative Example 1 is that Comparative Example 4 uses LiFe. 0.4 Mn 0.6 PO4 replaces LiMn2O4 as the active material.

[0085] Example 6

[0086] The only difference between Example 6 and Example 1 is that Example 6 uses LiFePO4 and LiMn2O4 in a 1:1 ratio to replace LiMn2O4 as the active material.

[0087] Comparative Example 5

[0088] The only difference between Comparative Example 5 and Comparative Example 1 is that Comparative Example 5 uses LiFePO4 and LiMn2O4 in a 1:1 ratio to replace LiMn2O4 as the active material.

[0089] Results Analysis

[0090] The results of electrochemical redox lithium extraction in the above embodiments and comparative examples are as follows: Figure 5-6 As shown in Table 1.

[0091] Table 1 Adsorption selectivity results of each example and comparative example

[0092]

[0093] Figure 5 Figure a shows the adsorption kinetics curve of the H-type columnar structure device. As can be seen from the figure, the adsorption kinetics of this H-type columnar structure device are rapid, reaching the constant pressure stage in about 50 minutes, with a total duration of 110 minutes. It exhibits a fast adsorption rate, short equilibrium time, and an equilibrium adsorption capacity as high as 32 mg / g.

[0094] Figure 5 Figure b shows the cyclic stability of the H-type columnar structure device. As can be seen from the figure, the capacity stabilizes above 31 mg / g for the first 100 cycles, and maintains a stable capacity of 30 mg / g even after 500 cycles. Table 1 shows the Li... + / Na + Li + / Mg 2+ Li + / Ca 2+ The selectivity is very high, among which the key Li + / Na + Up to 20.

[0095] Figure 5 Figure a shows the adsorption kinetics curves of the flat-plate structure device. As can be seen from the figure, the adsorption kinetics of the flat-plate structure device are slow, reaching the isobaric stage at approximately 360 min, with a total duration of 420 min. The adsorption rate is slow, the equilibrium time is long, and the equilibrium adsorption capacity is only 22 mg / g.

[0096] Figure 5 Figure b shows the cyclic stability of the flat-plate structure device. As can be seen from the figure, the capacity decreases rapidly in the first 100 cycles, reaching an equilibrium capacity of only 13 mg / g after 500 cycles. Table 1 shows the Li... + / Na + Li + / Mg 2+ Li + / Ca 2+ The selectivity is very low, with the key Li + / Na + Only 1.1.

[0097] Figure 6 The table shows bar charts of equilibrium adsorption time and equilibrium adsorption capacity for Examples 2-6 and Comparative Examples 2-5. As can be seen from the figures, the H-type columnar structure devices in Examples 2 and 4-6 exhibit rapid adsorption kinetics, reaching the constant pressure stage at approximately 70 min, 100 min, 85 min, and 77 min, respectively. They demonstrate fast adsorption rates, short equilibrium times, and equilibrium adsorption capacities as high as 22 mg / g, 27 mg / g, 31 mg / g, and 28 mg / g, respectively. Furthermore, Table 1 shows that the Li... + / Na + Li + / Mg 2+ Li + / Ca 2+ The selectivity is very high, among which the key Li + / Na + The figures are as high as 15, 18, 17 and 19 respectively.

[0098] The figure also shows that the adsorption kinetics of the flat-plate structures in Comparative Examples 2–5 are slow, reaching the isobaric stage at approximately 550 min, 780 min, 530 min, and 680 min, respectively, with long equilibrium times and equilibrium adsorption capacities of only 13 mg / g, 19 mg / g, 14 mg / g, and 18 mg / g, respectively. Table 1 shows that the Li... + / Na + Li + / Mg 2+ Li + / Ca 2+ The selectivity is very low, with the key Li + / Na + The values ​​were as low as 0.7, 1, 0.9 and 1 respectively.

[0099] In addition, Example 3 used an H-type columnar structure device and added an additional conductive agent to the precursor. The results were basically consistent with Example 2, with slight improvements in equilibrium adsorption time and capacity. Specifically, this device reached the constant pressure stage in about 65 minutes, with a short equilibrium time and a high equilibrium adsorption capacity of 23 mg / g. Table 1 shows that the Li... + / Na + Li + / Mg 2+ Li + / Ca 2+ The selectivity is very high, among which the key Li + / Na + Up to 16.

[0100] The above-described embodiments are merely preferred embodiments provided to fully illustrate the present invention, and the scope of protection of the present invention is not limited thereto. Equivalent substitutions or modifications made by those skilled in the art based on the present invention are all within the scope of protection of the present invention. The scope of protection of the present invention is defined by the claims.

Claims

1. An electrochemical oxidation-reduction lithium extraction device based on a flexible electrode, characterized in that, It includes an anode pipe, a cathode pipe, and an intermediate pipe connecting the anode pipe and the cathode pipe; The anode pipe is filled with an unactivated electrode, and the cathode pipe is filled with an activated electrode. Both the activated electrode and the unactivated electrode are flexible electrodes. The anode pipe is used to introduce the desorption solution, and the cathode pipe is used to introduce the lithium-containing solution; An anion exchange membrane is provided in the intermediate pipe, and the anion exchange membrane is used to separate the lithium-containing solution from the desorption solution; The anode pipe, cathode pipe, and intermediate pipe form an H-shaped structure; Both the anode pipe and the cathode pipe are cylindrical. The flexible electrode is filled into the anode channel and the cathode channel in the form of a roll; The flexible electrode is obtained by immersing the flexible electrode matrix material in a precursor solution containing active substances, removing it, coating the surface with a hydrophilic modifier, and then drying it. The flexible electrode substrate material includes one or more of graphene, carbon nanotubes, carbon nanofibers, conductive polymers, carbon cloth, carbon felt, and graphite felt.

2. The electrochemical oxidation-reduction lithium extraction device based on a flexible electrode according to claim 1, characterized in that, The precursor solution includes active substances, binders, and organic solvents; The active material includes one or more of lithium iron phosphate, lithium manganese oxide, lithium manganese iron phosphate, and lithium titanate; and / or, The adhesive comprises one or more of polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene rubber, and waterborne polystyrene ester; and / or, The organic solvent includes one or more of N-methylpyrrolidone, N-ethylpyrrolidone, N-vinylpyrrolidone, dimethylformamide, and dimethylacetamide; and / or, The hydrophilic modifier includes one or more of polystyrene, polyethylene glycol, polyvinyl chloride, polyoxymethylene, epoxy resin, polyglycolic acid, lignin, cellulose, and hemicellulose.

3. The electrochemical oxidation-reduction lithium extraction device based on a flexible electrode according to claim 2, characterized in that, The mass ratio of the organic solvent, active substance, binder, and hydrophilic modifier is 10-20:8-10:0.01-1:0.01-1.

4. The electrochemical oxidation-reduction lithium extraction device based on a flexible electrode according to claim 2, characterized in that, The precursor solution also includes a conductive agent, which includes one or more of carbon black, acetylene black, graphite, carbon fiber, carbon nanotubes, graphene, and composite conductive paste.

5. A method for extracting lithium through electrochemical oxidation-reduction, characterized in that, Includes the following steps: Provide an electrochemical oxidation-reduction lithium extraction apparatus based on a flexible electrode as described in any one of claims 1 to 4; A desorption solution is introduced into the anode pipe of the electrochemical lithium extraction device, and a lithium-containing solution is introduced into the cathode pipe of the electrochemical lithium extraction device. The flexible electrodes in the anode and cathode pipes are connected to a power source to extract lithium.

6. The method for electrochemical oxidation-reduction lithium extraction according to claim 5, characterized in that, The desorption solution is one or more of the following: lithium chloride solution, lithium bromide solution, lithium fluoride solution, lithium nitrate solution, lithium acetate solution, lithium oxalate solution, lithium sulfate solution, lithium acetate solution, and lithium formate solution, at a concentration of 0.01–1 M; and / or, The lithium-containing solution includes brine solutions or other lithium-rich solutions.

7. The method for electrochemical oxidation-reduction lithium extraction according to claim 5, characterized in that, It also includes the following steps: After lithium extraction is completed, the flexible electrodes in the anode and cathode channels are removed, cleaned, and exchanged to continue lithium extraction. Repeat the above steps to extract lithium in a cyclic manner until the lithium content in the lithium-containing solution is below 10 ppm. Lithium is recovered from the desorption solution.

8. The method for electrochemical oxidation-reduction lithium extraction according to claim 7, characterized in that, The lithium extraction voltage is 0.3–1.2V; and / or, The lithium extraction time is 1–100 h; and / or, The number of lithium extraction cycles is 3 to 500; and / or, A method for recovering lithium from the desorption solution includes: concentrating the desorption solution to obtain crude water and crude lithium salt; or Na2CO3 was added to the concentrated desorption solution to obtain crude lithium carbonate.

Citation Information

Patent Citations

  • Method for hydrophilic modification of the surface of manganese-based ion sieve electro-controlled lithium extraction membrane electrode

    CN114864876B

  • Device and method for activating electrodes

    CN115522071A

  • Method for stripping two-dimensional material and synchronously producing high-purity lithium hydroxide by utilizing salt lake brine

    CN110923739A

  • Electrochemistry-based waste lithium iron phosphate repairing and recycling method

    CN113086961A

  • Electrochemical lithium extraction electrode and electrochemical lithium extraction method

    CN116555564A