Light emitting diode epitaxial wafer and preparation method thereof, LED

By setting a composite structure of Si₃N₄ grid layer, nitrided graphene layer, AlN layer and ScAlN layer on Si substrate, the lattice mismatch and thermal mismatch problems of GaN epitaxial layer on Si substrate are solved, and high-quality growth of epitaxial layer and improvement of luminescence efficiency are achieved.

CN117790654BActive Publication Date: 2026-11-24JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311830308.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2026-11-24
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

Growing GaN on Si substrates presents lattice and thermal mismatch problems, leading to numerous defects and cracks that affect the crystal quality and luminous efficiency of the GaN epitaxial layer.

Method used

Composite layers, including Si₃N₄ grid layers, nitrided graphene layers, AlN layers, and ScAlN layers, are fabricated on Si substrates. The combination of these layers alleviates stress caused by lattice mismatch and thermal mismatch, prevents epitaxial layer cracking, reduces dislocation density, and improves crystal quality.

Benefits of technology

It effectively prevents epitaxial layer cracking, reduces dislocation density, releases stress, improves the crystal quality of GaN epitaxial layer, and enhances the luminous efficiency of light-emitting diodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117790654B_ABST
    Figure CN117790654B_ABST
Patent Text Reader

Abstract

This invention discloses a light-emitting diode (LED) epitaxial wafer and its fabrication method, as well as an LED. The LED epitaxial wafer includes a silicon substrate, on which a composite layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially deposited. The composite layer includes a Si3N4 mesh layer, a graphene nitride layer, an AlN layer, and a ScAlN layer sequentially deposited on the silicon substrate. The LED epitaxial wafer provided by this invention can prevent epitaxial layer cracking, reduce epitaxial layer dislocation density, release stress between the substrate and the GaN epitaxial layer, improve the crystal quality of the GaN epitaxial layer, reduce non-radiative recombination caused by defects, and improve the luminous efficiency of the LED.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of optoelectronic technology, and in particular to a light-emitting diode epitaxial wafer and its preparation method, and LEDs. Background Technology

[0002] In the field of optoelectronic devices, GaN and its alloy (In / Al)GaN-based LEDs, as direct wide-bandgap semiconductor materials, can cover the entire visible light spectrum from red to violet. The commercialization of high-brightness GaN-based blue LEDs provides technological support for future low-energy and environmentally friendly white light lighting and broadens the application areas of LEDs. Currently, significant progress has been made in growing GaN on Si substrates, with reports of successful fabrication of blue LEDs with multi-quantum-well structures on Si(111) substrates. Although many breakthroughs have been achieved in LED fabrication technology on Si substrates, insurmountable problems remain in material growth and fundamental research.

[0003] Depositing GaN on Si substrates has the following drawbacks: First, the lattice mismatch and thermal mismatch between Si substrate and GaN are as high as 16.9% and 54%, respectively, which makes it easy for a large number of defects and cracks to form in GaN; Second, during the high-temperature growth of GaN, Si atoms diffuse along the grain boundaries into GaN and undergo "remelting etching", which greatly reduces the crystal quality of GaN epitaxial films. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to provide an epitaxial wafer for light-emitting diodes that prevents epitaxial layer cracking, reduces epitaxial layer dislocation density, releases stress on the substrate and GaN epitaxial layer, improves GaN epitaxial layer crystal quality, reduces nonradiative recombination caused by defects, and improves the luminous efficiency of light-emitting diodes.

[0005] The technical problem to be solved by the present invention is to provide a method for preparing an epitaxial wafer of a light-emitting diode, which has a simple process and can stably produce an epitaxial wafer of a light-emitting diode with good luminous efficiency.

[0006] To solve the above-mentioned technical problems, the present invention provides a light-emitting diode epitaxial wafer, comprising a silicon substrate, wherein a composite layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially disposed on the silicon substrate.

[0007] The composite layer comprises a Si3N4 mesh layer, a nitrided graphene layer, an AlN layer, and a ScAlN layer sequentially deposited on the silicon substrate.

[0008] In one embodiment, the thickness of the Si3N4 mesh layer is 10 nm to 100 nm;

[0009] The Si3N4 mesh layer has a mesh area of ​​1 μm. 2 ~100μm 2 .

[0010] In one embodiment, the thickness of the nitrided graphene layer is 10 nm to 100 nm.

[0011] In one embodiment, the thickness of the AlN layer is 10 nm to 100 nm.

[0012] In one embodiment, the thickness of the ScAlN layer is 10 nm to 100 nm;

[0013] The Sc component of the ScAlN layer is 0.01 to 0.99.

[0014] In one embodiment, the Sc composition of the ScAlN layer gradually increases along the growth direction.

[0015] To address the above problems, the present invention also provides a method for fabricating a light-emitting diode epitaxial wafer, comprising the following steps:

[0016] S1. Prepare the silicon substrate;

[0017] S2. Sequentially deposit a composite layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer on the silicon substrate.

[0018] The composite layer comprises a Si3N4 mesh layer, a nitrided graphene layer, an AlN layer, and a ScAlN layer sequentially deposited on the silicon substrate.

[0019] In one embodiment, the Si3N4 mesh layer is prepared by the following method:

[0020] The pressure in the reaction chamber was controlled at 50 to 100 tor, and Si and N sources were introduced to grow a Si3N4 layer.

[0021] The Si3N4 layer is etched to form a Si3N4 mesh layer.

[0022] In one embodiment, the nitrided graphene layer is prepared by the following method:

[0023] The temperature of the reaction chamber was controlled at 800℃~1000℃, the pressure at 50torr~100torr, the radio frequency power at 15W~22W, CH4 and H2 were introduced, and the ratio of CH4 to H2 was 1:(1~20) to grow a graphene layer.

[0024] The graphene layer was treated with nitrogen plasma to obtain a nitrided graphene layer.

[0025] Accordingly, the present invention also provides an LED, which includes the above-described light-emitting diode epitaxial wafer.

[0026] Implementing this invention has the following beneficial effects:

[0027] The light-emitting diode epitaxial wafer provided by the present invention has a composite layer with a specific structure on a silicon substrate. The composite layer includes a Si3N4 grid layer, a graphene nitride layer, an AlN layer and a ScAlN layer deposited sequentially on the silicon substrate.

[0028] The Si3N4 grid layer ensures that subsequent material growth is restricted to designated patterned regions, with each growth region operating independently. This avoids the accumulation of thermal stress during growth, achieving stress separation and preventing film cracking. After nitrogen plasma pretreatment, defects are introduced into the graphene surface of the nitrided graphene layer. The graphene surface is partially etched, and in addition to incorporating into the graphene lattice, N atoms also bond with C atoms in the etched regions, forming out-of-plane N-sp atoms on the graphene surface. 3 C bonds serve as effective nucleation sites, promoting the subsequent nucleation and growth of AlN. Furthermore, the nitrided graphene layer prevents reactions between Si and Ga atoms on the silicon substrate surface, avoiding the so-called "Ga remelting," ensuring a smooth epitaxial layer surface, preventing the formation of micron-sized giant holes, and reducing the defect density of the GaN epitaxial layer. The AlN layer alleviates stress caused by lattice and thermal mismatch between the substrate and the epitaxial layer. Further, after high-temperature annealing, crystal defects can be controlled, improving the crystal quality of the AlN layer and the quality of subsequently grown crystals. The lattice constant of ScN in the ScAlN layer is close to that of GaN, and the gradual increase in the Sc composition of the ScAlN layer reduces lattice mismatch with undoped GaN, improving the crystal quality of undoped GaN.

[0029] In summary, by providing a composite layer with a specific structure on a silicon substrate, this invention can prevent epitaxial layer cracking, reduce epitaxial layer dislocation density, release stress between the substrate and GaN epitaxial layer, improve GaN epitaxial layer crystal quality, reduce non-radiative recombination caused by defects, and improve the luminous efficiency of light-emitting diodes. Attached Figure Description

[0030] Figure 1 This is a schematic diagram of the structure of the light-emitting diode epitaxial wafer provided by the present invention;

[0031] Figure 2 A flowchart illustrating the method for fabricating a light-emitting diode epitaxial wafer provided by the present invention;

[0032] Figure 3 The flowchart shows step S2 of the method for preparing a light-emitting diode epitaxial wafer provided by the present invention. Detailed Implementation

[0033] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below.

[0034] Unless otherwise stated or in case of contradiction, the terms or phrases used herein shall have the following meanings:

[0035] In this invention, "preferred" is merely a description of a more effective implementation method or embodiment, and should be understood as not constituting a limitation on the scope of protection of this invention.

[0036] In this invention, the technical features described in an open-ended manner include both closed-ended technical solutions composed of the listed features and open-ended technical solutions that include the listed features.

[0037] In this invention, numerical ranges are involved, and unless otherwise specified, they include the two endpoints of the numerical range.

[0038] To address the above problems, the present invention provides a light-emitting diode epitaxial wafer, such as... Figure 1 As shown, it includes a silicon substrate 100, on which a composite layer 200, an undoped GaN layer 300, an N-type GaN layer 400, a multiple quantum well layer 500, an electron blocking layer 600, and a P-type GaN layer 700 are sequentially disposed.

[0039] The composite layer 200 includes a Si3N4 mesh layer 210, a nitrided graphene layer 220, an AlN layer 230 and a ScAlN layer 240 sequentially deposited on the silicon substrate 100.

[0040] The specific structure of the composite layer 200 is as follows:

[0041] In one embodiment, the thickness of the Si3N4 mesh layer 210 is 10nm to 100nm; exemplary thicknesses of the Si3N4 mesh layer 210 are 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, and 90nm, but are not limited thereto. In one embodiment, the mesh area of ​​the Si3N4 mesh layer 210 is 1μm. 2 ~100μm 2 An exemplary size of the grid area of ​​the Si3N4 grid layer 210 is 10 μm. 2 20μm 2 30μm 2 40μm 2 50μm 2 60μm 2 70μm 2 80μm 2 90μm 2However, it is not limited to this. The Si3N4 mesh layer ensures that subsequent materials can only grow in designated patterned areas, with each growth area being independent of the others. This avoids the accumulation of thermal stress during the growth process, achieving stress separation and preventing film cracking.

[0042] In one embodiment, the thickness of the nitrided graphene layer 220 is 10 nm to 100 nm; exemplary thicknesses of the nitrided graphene layer 220 are 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, and 90 nm, but are not limited thereto. In one embodiment, the nitrided graphene layer 220 is prepared by the following method: the temperature of the reaction chamber is controlled at 800°C to 1000°C, the pressure is controlled at 50 torr to 100 torr, the radio frequency power is 15 W to 22 W, CH4 and H2 are introduced, and the ratio of CH4 to H2 is 1:(1 to 20), and a graphene layer is grown; the graphene layer is then treated with nitrogen plasma to obtain the nitrided graphene layer. After the nitrogen plasma pretreatment, defects are generated on the surface of the nitrided graphene layer. When the graphene surface is partially etched, nitrogen atoms not only incorporate into the graphene lattice but also form bonds with carbon atoms in the etched areas, creating out-of-plane N-sp atoms on the graphene surface. 3 C bonds serve as effective nucleation sites, promoting subsequent AlN nucleation and growth. Furthermore, the nitrided graphene layer prevents reactions between Si and Ga atoms on the silicon substrate surface, avoiding the so-called "Ga remelting," thus ensuring a smooth epitaxial layer surface, preventing the formation of micron-sized giant pores on the epitaxial layer surface, and reducing the defect density of the GaN epitaxial layer.

[0043] In one embodiment, the thickness of the AlN layer 230 is 10 nm to 100 nm; exemplary thicknesses of the AlN layer 230 are 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, and 90 nm, but are not limited thereto. In one embodiment, the AlN layer 230 is an AlN layer annealed at a high temperature of 1000 °C to 1200 °C. The AlN layer can alleviate the stress caused by lattice mismatch and thermal mismatch between the substrate and the epitaxial layer. Furthermore, after high-temperature annealing, crystal defects can be controlled, the crystal quality of the AlN layer can be improved, and the quality of subsequently grown crystals can be improved.

[0044] In one embodiment, the thickness of the ScAlN layer 240 is 10 nm to 100 nm; exemplary thicknesses of the ScAlN layer 240 are 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, and 90 nm, but are not limited thereto. In one embodiment, the Sc composition of the ScAlN layer 240 is 0.01 to 0.99, preferably, the Sc composition of the ScAlN layer 240 gradually increases along the growth direction. The lattice constant of the ScN in the ScAlN layer is close to that of GaN, and the gradual increase in the Sc composition of the ScAlN layer can reduce the lattice mismatch with undoped GaN and improve the crystal quality of undoped GaN.

[0045] In summary, by providing a composite layer with a specific structure on a silicon substrate, this invention can prevent epitaxial layer cracking, reduce epitaxial layer dislocation density, release stress between the substrate and GaN epitaxial layer, improve GaN epitaxial layer crystal quality, reduce non-radiative recombination caused by defects, and improve the luminous efficiency of light-emitting diodes.

[0046] Accordingly, the present invention provides a method for fabricating a light-emitting diode epitaxial wafer, such as... Figure 2 As shown, it includes the following steps:

[0047] S1. Prepare silicon substrate 100;

[0048] Silicon substrates are large in size and inexpensive, which can reduce the cost of epitaxial growth. Compared with sapphire substrates, which have high hardness and poor thermal and electrical properties, silicon substrates have a significant advantage. Moreover, they simplify the substrate thinning process and reduce costs.

[0049] S2. A composite layer 200, an undoped GaN layer 300, an N-type GaN layer 400, a multiple quantum well layer 500, an electron blocking layer 600, and a P-type GaN layer 700 are sequentially deposited on the silicon substrate 100.

[0050] like Figure 3 As shown, step S2 specifically includes the following steps:

[0051] S21. Deposit a composite layer 200 on a silicon substrate 100.

[0052] The composite layer 200 includes a Si3N4 mesh layer 210, a nitrided graphene layer 220, an AlN layer 230 and a ScAlN layer 240 sequentially deposited on the silicon substrate 100.

[0053] In one embodiment, the Si3N4 mesh layer 210 is prepared by the following method:

[0054] The pressure in the reaction chamber was controlled at 50 to 100 tor, and Si and N sources were introduced to grow a Si3N4 layer.

[0055] The Si3N4 layer is etched to form a Si3N4 mesh layer.

[0056] In one embodiment, the nitrided graphene layer 220 is prepared by the following method:

[0057] The temperature of the reaction chamber was controlled at 800℃~1000℃, the pressure at 50torr~100torr, the radio frequency power at 15W~22W, CH4 and H2 were introduced, and the ratio of CH4 to H2 was 1:(1~20) to grow a graphene layer.

[0058] The graphene layer was treated with nitrogen plasma to obtain a nitrided graphene layer.

[0059] In one embodiment, the AlN layer 230 is prepared by the following method:

[0060] The temperature of the reaction chamber was controlled at 700℃~800℃, and the pressure was controlled at 50 torr~300 torr. Al source and N source were introduced to grow AlN layer.

[0061] Then, the AlN layer is subjected to high-temperature annealing at 1000℃~1200℃.

[0062] In one embodiment, the ScAlN layer 240 is prepared by the following method:

[0063] The temperature of the reaction chamber was controlled at 900℃~1000℃, and the pressure was controlled at 50 torr~500 torr. Sc source, Ga source and N source were introduced to grow ScGaN layer.

[0064] S22. Deposit an undoped GaN layer 300 on the composite layer 200.

[0065] In one embodiment, the temperature of the reaction chamber is controlled at 1050℃~1200℃, the pressure is controlled at 100 torr~600 torr, and an N source and a Ga source are introduced to grow an undoped GaN layer with a thickness of 1μm~5μm.

[0066] S23. Deposit an N-type GaN layer 400 on the undoped GaN layer 300.

[0067] In one embodiment, the temperature of the reaction chamber is controlled at 1050°C to 1200°C, the pressure is controlled at 100 torr to 600 torr, and an N source, a Ga source, and a Si source are introduced to grow the N-type GaN layer.

[0068] S24. Deposit a multi-quantum-well layer 500 on the N-type GaN layer 400.

[0069] The multi-quantum-well layer comprises multiple alternating layers of InGaN quantum well layers and AlGaN quantum barrier layers, with a stacking period of 6 to 12. The InGaN quantum well layers are grown at a temperature of 790°C to 810°C, with a thickness of 2 nm to 5 nm and a growth pressure of 50 torr to 300 torr. The AlGaN quantum barrier layers are grown at a temperature of 800°C to 900°C, with a thickness of 5 nm to 15 nm and a growth pressure of 50 torr to 300 torr.

[0070] S25. Deposit an electron blocking layer 600 on the multi-quantum well layer 500.

[0071] In one embodiment, the temperature of the reaction chamber is controlled at 900℃~1000℃, the pressure is controlled at 100torr~300torr, and N source, Al source, Ga source and In source are introduced to grow an AlInGaN electron blocking layer with a thickness of 10nm~40nm.

[0072] S26. Deposit a P-type GaN layer 700 on the electron blocking layer 600.

[0073] In one embodiment, the temperature of the reaction chamber is controlled at 900℃~1050℃, and the pressure is controlled at 100 torr~600 torr. An N source, a Ga source, and a Mg source are introduced to grow a P-type GaN layer with a thickness of 10nm~5nm. Preferably, the Mg doping concentration is 1×10⁻⁶. 19 atoms / cm 3 ~1×10 21 atoms / cm 3 .

[0074] Accordingly, the present invention also provides an LED comprising the aforementioned light-emitting diode epitaxial wafer. The photoelectric efficiency of the LED is effectively improved, and other electrical properties are also excellent.

[0075] The present invention is further illustrated below with specific embodiments:

[0076] Example 1

[0077] This embodiment provides a light-emitting diode epitaxial wafer, wherein a composite layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially disposed on the silicon substrate.

[0078] The composite layer comprises a Si3N4 mesh layer, a nitrided graphene layer, an AlN layer, and a ScAlN layer sequentially deposited on the silicon substrate.

[0079] The Si3N4 mesh layer has a thickness of 45 nm and a mesh area of ​​35 μm. 2

[0080] The thickness of the nitrided graphene layer is 65 nm.

[0081] The thickness of the AlN layer is 40 nm.

[0082] The ScAlN layer has a thickness of 40 nm, and the Sc composition gradually increases from 0.1 to 0.9 along the growth direction.

[0083] Example 2

[0084] This embodiment provides a light-emitting diode epitaxial wafer, wherein a composite layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially disposed on the silicon substrate.

[0085] The composite layer comprises a Si3N4 mesh layer, a nitrided graphene layer, an AlN layer, and a ScAlN layer sequentially deposited on the silicon substrate.

[0086] The Si3N4 mesh layer has a thickness of 10 nm and a mesh area of ​​1 μm. 2

[0087] The thickness of the nitrided graphene layer is 10 nm.

[0088] The thickness of the AlN layer is 10 nm.

[0089] The ScAlN layer has a thickness of 10 nm, and the Sc composition gradually increases from 0.1 to 0.5 along the growth direction.

[0090] Example 3

[0091] This embodiment provides a light-emitting diode epitaxial wafer, wherein a composite layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially disposed on the silicon substrate.

[0092] The composite layer comprises a Si3N4 mesh layer, a nitrided graphene layer, an AlN layer, and a ScAlN layer sequentially deposited on the silicon substrate.

[0093] The Si3N4 mesh layer has a thickness of 100 nm and a mesh area of ​​100 μm. 2

[0094] The thickness of the nitrided graphene layer is 100 nm.

[0095] The thickness of the AlN layer is 100 nm.

[0096] The ScAlN layer has a thickness of 100 nm, and the Sc composition gradually increases from 0.5 to 0.9 along the growth direction.

[0097] Comparative Example 1

[0098] This comparative example provides a light-emitting diode epitaxial wafer. The difference between this example and the other examples of Example 1 is that no composite layer is provided. The rest are the same as in Example 1.

[0099] Comparative Example 2

[0100] This comparative example provides a light-emitting diode epitaxial wafer. The difference between the other examples in Example 1 is that the composite layer includes a nitrided graphene layer, an AlN layer and a ScAlN layer deposited sequentially on the silicon substrate, but does not include the Si3N4 mesh layer. The rest is the same as in Example 1.

[0101] Comparative Example 3

[0102] This comparative example provides a light-emitting diode epitaxial wafer. The difference between the other examples in Example 1 is that its composite layer includes a Si3N4 mesh layer, an AlN layer and a ScAlN layer deposited sequentially on the silicon substrate, but does not include a nitrided graphene layer. The rest is the same as in Example 1.

[0103] Comparative Example 4

[0104] This comparative example provides a light-emitting diode epitaxial wafer. The difference between the other examples in Example 1 is that the composite layer includes a Si3N4 mesh layer, a graphene nitride layer and a ScAlN layer deposited sequentially on the silicon substrate, but does not include an AlN layer. The rest is the same as in Example 1.

[0105] Comparative Example 5

[0106] This comparative example provides a light-emitting diode epitaxial wafer. The difference between the other examples in Example 1 is that the composite layer includes a Si3N4 mesh layer, a graphene nitride layer, and an AlN layer deposited sequentially on the silicon substrate, but does not include the ScAlN layer. The rest is the same as in Example 1.

[0107] The light-emitting diode epitaxial wafers prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were fabricated into 10mil×24mil chips using the same chip process conditions. 300 LED chips were randomly selected from each example and tested at a current of 120mA / 60mA. With Comparative Example 1 as a reference, the luminous efficiency improvement rate of each example and comparative example was calculated. The specific test results are shown in Table 1.

[0108] Table 1. Performance test results of LEDs prepared in Examples 1-3 and Comparative Examples 1-5

[0109]

[0110] As can be seen from the above results, the LED epitaxial wafer provided by the present invention, compared with the existing epitaxial wafer, prevents epitaxial layer cracking, reduces epitaxial layer dislocation density, releases stress between the substrate and GaN epitaxial layer, improves GaN epitaxial layer crystal quality, reduces non-radiative recombination caused by defects, and improves the luminous efficiency of LED by providing a composite layer with a specific structure on the silicon substrate.

[0111] The above description is a preferred embodiment of the invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the invention, and these improvements and modifications are also considered to be within the scope of protection of the invention.

Claims

1. A light-emitting diode epitaxial wafer, characterized in that, The substrate includes a silicon substrate, on which a composite layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially disposed; The composite layer comprises a Si3N4 mesh layer, a nitrided graphene layer, an AlN layer, and a ScAlN layer sequentially deposited on the silicon substrate; The thickness of the Si3N4 mesh layer is 10nm~100nm; The Si3N4 mesh layer has a mesh area of ​​1 μm. 2 ~100μm 2 ; The thickness of the nitrided graphene layer is 10 nm to 100 nm.

2. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The thickness of the AlN layer is 10nm~100nm.

3. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The thickness of the ScAlN layer is 10nm~100nm; The Sc component of the ScAlN layer is 0.01~0.

99.

4. The light-emitting diode epitaxial wafer as described in claim 3, characterized in that, The Sc composition of the ScAlN layer gradually increases along the growth direction.

5. A method for fabricating a light-emitting diode epitaxial wafer as described in any one of claims 1 to 4, characterized in that, Includes the following steps: S1. Prepare the silicon substrate; S2. Sequentially deposit a composite layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer on the silicon substrate. The composite layer comprises a Si3N4 mesh layer, a nitrided graphene layer, an AlN layer, and a ScAlN layer sequentially deposited on the silicon substrate.

6. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 5, characterized in that, The Si3N4 mesh layer was prepared using the following method: The pressure in the reaction chamber was controlled at 50 to 100 torr, and Si and N sources were introduced to grow a Si3N4 layer. The Si3N4 layer is etched to form a Si3N4 mesh layer.

7. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 5, characterized in that, The nitrided graphene layer was prepared by the following method: The temperature of the reaction chamber was controlled at 800℃~1000℃, the pressure at 50 torr~100 torr, the radio frequency power at 15W~22W, and CH4 and H2 were introduced in a ratio of 1:(1~20) to grow a graphene layer. The graphene layer was treated with nitrogen plasma to obtain a nitrided graphene layer.

8. An LED, characterized in that, The LED includes a light-emitting diode epitaxial wafer as described in any one of claims 1 to 4.

Citation Information

Patent Citations

  • Light-emitting diode epitaxial wafer, preparation method thereof and LED

    CN116936696A

  • Light-emitting diode epitaxial wafer, preparation method thereof and LED

    CN116978991A