A method for forging a GH4169 disc type forging

By optimizing the mold structure and heating method, the problem of uneven deformation of GH4169 disc forgings was solved, achieving high yield, low cost and high efficiency in forging manufacturing.

CN117798314BActive Publication Date: 2026-11-24SHAANXI HONGYUAN AVIATION FORGING
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311766995.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-20
Publication Date
2026-11-24
Estimated Expiration
2043-12-20

AI Technical Summary

Technical Problem

Existing technologies for forging GH4169 disc forgings suffer from uneven deformation, localized substandard microstructure and properties, resulting in low forging pass rates, increased raw material consumption, high production costs, and long production cycles.

Method used

By adopting a reasonably designed mold structure and heating method, and through the grooved surface of the first mold and the annular structure of the second mold, combined with the use of aluminum silicate insulation cotton, the billet is ensured to deform uniformly under triaxial compressive stress, reducing the occurrence of cold mold layers and improving material utilization and deformation uniformity.

Benefits of technology

This improved the pass rate and material utilization of forgings, reduced production costs, shortened the production cycle, and ensured the stability of forging quality and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117798314B_ABST
    Figure CN117798314B_ABST
Patent Text Reader

Abstract

This invention relates to the fields of forging and die design, specifically to a forging method for GH4169 disc forgings. The method includes: blanking; heating to forging temperature in a furnace; simultaneously heating a first die and a second die; the first die has a grooved surface in the middle of its upper surface; the second die has a ring-shaped structure; performing a first upsetting: vertically placing the heated bar stock onto the heated first die for upsetting, obtaining a first upsetting billet, the lower surface of which has small protrusions due to the grooved surface; performing a second upsetting: heating the first upsetting billet plane-down in the furnace, placing it inside the groove of the second die for upsetting, obtaining a billet; during this process, the second die surface contacts the billet, constraining the outer circumference of the billet, making the deformation of the billet more uniform under triaxial compressive stress; and air-cooling the billet to room temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of forging and mold design, and specifically to a forging method for GH4169 disc forgings. Background Technology

[0002] A disc-shaped forging for an aero-engine, made of GH4169, has a diameter of approximately 650 mm and a thickness of approximately 75 mm. The forging is classified as a Class I forging, requiring high performance and microstructure. The average grain size must be grade 10 or finer, and non-destructive testing requires grade AA. For this type of forging, conventional forging involves roughing using free forging upsetting followed by die forging.

[0003] Due to the narrow process window and high deformation resistance of GH4169, uneven deformation often occurs. Simultaneously, heat transfer occurs due to localized contact between the forging and the anvil, resulting in excessively low surface temperatures and the formation of a cold die layer. The combined effect of this cold die layer and small deformation leads to substandard microstructure and properties in some areas of the forging. To improve the forging yield, it is necessary to design a reasonable blank shape to ensure uniform deformation during die forging, increase the feed weight, increase the machining allowance, optimize the billet dimensions using simulation software, adjust the location of small deformation zones and the cold die layer, and finally remove them through machining. This method solves the forging yield problem but increases raw material consumption, leading to increased manufacturing costs and a longer manufacturing cycle. Summary of the Invention

[0004] Purpose of the invention: To improve the pass rate of forgings while reducing the consumption of raw materials for forgings, thereby increasing the production efficiency of forgings, reducing the production cost of forgings, and shortening the production cycle of forgings.

[0005] Technical solution:

[0006] This invention provides a forging method for GH4169 disc-shaped forgings, comprising:

[0007] Material feeding;

[0008] The furnace is heated to the forging temperature; the first mold and the second mold are heated simultaneously; the upper surface of the first mold has a groove in the middle; the second mold has a ring structure.

[0009] First upsetting: The heated bar is placed vertically on the heated first mold and the bar is upset to obtain the first upsetting billet. The lower surface of the first upsetting billet has small protrusions due to the groove surface.

[0010] The second upsetting process involves heating the billet from the first upsetting process with its flat side facing down in the furnace. The billet is then placed inside the second mold slot for upsetting to obtain a new billet. During this process, the surface of the second mold contacts the billet and constrains the outer circumference of the billet, resulting in a more uniform deformation of the billet under triaxial compressive stress.

[0011] The billet is raised and air-cooled to room temperature.

[0012] Furthermore, the method also includes:

[0013] The blank is machined with a lathe to create positioning blind holes; the upper and lower surfaces are machined with a milling machine.

[0014] Perform flaw detection on the billet;

[0015] After the flaw detection is passed, the forgings are heated and then die-forged.

[0016] Forgings that have been water-cooled for 50-80 seconds and then air-cooled to room temperature are then subjected to pre-hot machining.

[0017] The processed forgings are then subjected to aging treatment.

[0018] Furthermore, the first mold has a grooved surface (X12) in the middle; the grooved surface (X12) is an arc surface; the diameter D1 of the grooved surface (X12) is 0.5 to 0.7 times the diameter of the raw material bar; the depth H1 of the groove (X12) is 0.25 to 0.3 times the diameter.

[0019] Furthermore, the first mold also has a profile (X11); the profile (X11) has the aforementioned groove surface (X12) at its center; the profile (X11) is a circular stepped blind hole; the diameter D2 of the profile (X11) is 4 to 10 mm larger than the diameter of the raw material bar, and the depth H2 is 2 to 5 mm.

[0020] Furthermore, the center hole of the second mold is a conical hole, and the angle between the conical hole and its own central axis is 3°.

[0021] Furthermore, the small end diameter D3 of the second tire model cavity is 1.015 times the design rough shape diameter, and the height of the second tire model cavity is 1.018 times the design rough shape height.

[0022] Furthermore, prior to the first upsetting, the method also includes:

[0023] A layer of aluminum silicate insulation cotton is laid on the upper surface of the first mold; a layer of aluminum silicate insulation cotton is laid on the upper end face of the bar stock;

[0024] Before the second upsetting, the method further includes:

[0025] A layer of aluminum silicate insulation cotton is laid on the upper surface of the lower hammer anvil; a layer of aluminum silicate insulation cotton is laid on the upper end surface of the first fire billet.

[0026] Furthermore, during the heating process before die forging, the billet only needs to be wrapped with aluminum silicate insulation cotton.

[0027] Furthermore, the minimum wall thickness of the second mold must be greater than 180mm.

[0028] Beneficial effects: Forgings obtained by this method have a significantly improved material utilization rate, a high forging qualification rate, stable forging quality, short production cycle, and low cost.

[0029] 1. A hollow die was designed to reduce the contact area between the billet and the upsetting die, avoiding the overlap of small deformation zones and cold die layers on the billet end face, thus increasing the billet temperature and preventing localized structural defects in the forging. 2. An upsetting ring die was designed to create a triaxial pressure state on the billet during the upsetting stage, improving the uniformity of deformation during the free forging process. Attached Figure Description

[0030] Figure 1 This is a schematic diagram of the structure of the first mold.

[0031] Figure 2 This is a schematic diagram of the second mold.

[0032] Figure 3 A schematic diagram of the structure for designing the rough shape.

[0033] Figure 4 The image shows the microstructure of the forging in the example. Detailed Implementation

[0034] A forging method for GH4169 disc forgings is provided, and the specific process is as follows:

[0035] Step 1: Material cutting. First, round the edges of the raw material bar with a diameter of 250 and a length of 410 to R15.

[0036] Step 2: Then heat to the forging temperature in a heating furnace. At the same time, the first mold 1 and the second mold 2 are also heated to a temperature of 150-250°C.

[0037] Step 3: First upsetting: First mold ( Figure 1 The upper surface is covered with a layer of aluminum silicate insulation cotton. The bar is placed vertically on the cavity surface X11 of the first mold after heating. A layer of aluminum silicate insulation cotton is then laid on the upper end face of the bar for upsetting the billet, stopping when the height reaches 203mm. The forging temperature is 1000℃ and the pressing speed is 5mm / s.

[0038] Step 4: Perform the second upsetting process by placing the billet face down into the heating furnace for heating, using the second die ( Figure 2 Upsetting is performed by placing the billet inside the second mold groove. A layer of aluminum silicate insulation cotton is laid on both the upper and lower surfaces of the billet. Upsetting is then carried out until the billet height reaches 115 mm. During this process, the mold surface X21 contacts the billet and constrains the outer circumference of the billet, making the deformation of the billet more uniform under triaxial compressive stress.

[0039] Step 5: Air-cool the billet to room temperature. Machin the positioning blind holes using a lathe; machine the upper and lower surfaces using a milling machine.

[0040] Step 6: Perform flaw detection on the billet; the flaw detection method is the contact method.

[0041] Step 7: Heat the forgings that have passed the flaw detection. During the heating process, wrap the billet with aluminum silicate insulation cotton. After heating, perform die forging; the forging temperature is 990℃ and the pressing speed is 3mm / s.

[0042] Step 8: After water cooling for 50-80 seconds and then air cooling to room temperature, perform hot pre-machining.

[0043] Step 9: Aging treatment is performed on the machined forgings.

[0044] Step 10: Perform macroscopic and microscopic structure and performance testing on the heat-treated forgings.

[0045] The first mold in step 3 is a mold with a grooved surface X12 in the middle; furthermore, in order to reduce the stress concentration of the mold, the groove X12 is an arc surface; the diameter D1 of the grooved surface X12 is 0.5 to 0.7 times the diameter of the raw material bar; the depth H1 of the groove X12 is 0.25 to 0.3 times the diameter.

[0046] Furthermore, the first mold also features a surface X11.

[0047] Furthermore, profile X11 is a circular stepped blind hole. Furthermore, the diameter D2 of profile X11 is 4–10 mm larger than the diameter of the raw material bar, and the depth H2 is 2–5 mm. The raw material selected for the first mold is mold steel.

[0048] In step 4, the second mold is an annular mold with a through hole in the middle, and the X21 surface of the mold cavity is a conical surface at an angle of 87° to the bottom surface of the mold.

[0049] Furthermore, the diameter D3 of the small end of the cavity surface X21 of the second model is irregular ( Figure 3 The diameter is 1.015 times that of the rough shape, and the height of the second mold is 1.018 times that of the rough shape.

[0050] Furthermore, the minimum wall thickness of the second mold must be greater than 180mm. The raw material selected for the second mold is mold steel.

[0051] The rough shape is a uniformly distributed shape designed through simulation and optimization. The deformation of the rough shape during the die forging process is between 30% and 70%.

[0052] Example 1

[0053] An integral bladed disk forging for a certain aero-engine is made of GH4169. The forging diameter is 650mm and the forging thickness is about 75mm. The batch consists of 5 pieces.

[0054] For the blanking process, firstly, the ends of a 250mm diameter, 410mm length raw material bar are rounded to R15. Then, it is heated to the forging temperature in a furnace. Simultaneously, the first and second molds are also heated to 250℃. For the first upsetting, the heated bar is placed vertically on the first mold, which has a layer of aluminum silicate insulation on its upper surface. The bar is then placed vertically on the X11 cavity surface of the first mold. Another layer of aluminum silicate insulation is placed on the upper end of the bar, and upsetting is performed until the height reaches 203mm. The forging temperature is 1000℃, and the pressing speed is 5mm / s.

[0055] The second upsetting process involves placing the billet face down into the furnace for heating. Upsetting is then performed using a second mold. The billet is placed inside the mold's groove, with a layer of aluminum silicate insulation cotton laid on both the upper and lower surfaces. Upsetting continues until the billet reaches a height of 115 mm. During this process, the mold surface X21 contacts the billet, constraining the outer circumference and resulting in more uniform deformation under triaxial compressive stress. The billet is then air-cooled to room temperature. Positioning blind holes are machined on a lathe, and the upper and lower surfaces are machined on a milling machine.

[0056] The billet is subjected to flaw detection using the contact method. The forging, after passing flaw detection, is heated. During heating, the billet is wrapped with aluminum silicate insulation cotton. After heating, die forging is performed; the forging temperature is 990℃, and the pressing speed is 3mm / s. The forging, after water cooling for 50 seconds and then air cooling to room temperature, is then pre-machined. The machined forging is then subjected to aging treatment.

[0057] The forgings after heat treatment were subjected to macroscopic and microscopic structure and property testing. The microstructure of the forgings is as follows: Figure 4 As shown.

[0058] The forging qualification rate was increased to 100%, the material utilization rate from bar stock to forgings was increased by 10%, the quality and qualification rate of forgings were improved, the raw material cost of forging production was reduced, the batch production stability of forging quality was guaranteed, the production efficiency of forgings was greatly improved, and the production cycle of forgings was shortened.

Claims

1. A forging method for GH4169 disc-shaped forgings, characterized in that, include: Material feeding; Heat to forging temperature in a heating furnace; simultaneously heat the first mold and the second mold; The upper surface of the first mold has a grooved surface in the middle; The second mold structure is a ring structure; First upsetting: The heated bar is placed vertically on the heated first mold and the bar is upset to obtain the first upsetting billet. The lower surface of the first upsetting billet has small protrusions due to the groove surface. The second upsetting process involves heating the billet from the first upsetting process with its flat side down in the furnace. The billet is then placed inside the second mold slot for upsetting to obtain a new billet. During this process, the contact between the second mold surface and the billet constrains the outer circumference of the billet, making the deformation of the billet more uniform under triaxial compressive stress. At the same time, the contact area between the billet and the upsetting mold is reduced, preventing the occurrence of small deformation zones and overlap of the cold mold layer on the end face of the billet. The billet is lifted up and air-cooled to room temperature; The first mold has a grooved surface (X12) in the middle; the grooved surface (X12) is an arc surface; the diameter D1 of the grooved surface (X12) is 0.5 to 0.7 times the diameter of the raw material bar; the depth H1 of the grooved surface (X12) is 0.25 to 0.3 times the diameter of the raw material bar. The first mold also has a profile (X11); the profile (X11) has the above-mentioned groove surface (X12) in the center; the profile (X11) is a circular stepped blind hole; the diameter D2 of the profile (X11) is 4 to 10 mm larger than the diameter of the raw material bar, and the depth H2 is 2 to 5 mm. The small end diameter D3 of the second mold groove is 1.015 times the design rough shape diameter, and the height of the second mold groove is 1.018 times the design rough shape height.

2. The method according to claim 1, characterized in that, The method further includes: The blank is machined with a lathe to create positioning blind holes; the upper and lower surfaces are machined with a milling machine. Perform flaw detection on the billet; After the flaw detection is passed, the forgings are heated and then die-forged. Forgings that have been water-cooled for 50-80 seconds and then air-cooled to room temperature are then subjected to pre-hot machining. The processed forgings are then subjected to aging treatment.

3. The method according to claim 1, characterized in that, The second mold slot is a conical hole, and the angle between the conical hole and its own central axis is 3°.

4. The method according to claim 1, characterized in that, Before the first upsetting, the method further includes: A layer of aluminum silicate insulation cotton is laid on the upper surface of the first mold; a layer of aluminum silicate insulation cotton is laid on the upper end face of the bar stock; Before the second upsetting, the method further includes: A layer of aluminum silicate insulation cotton is laid on the upper surface of the lower hammer anvil; a layer of aluminum silicate insulation cotton is laid on the upper end surface of the first-fired billet.

5. The method according to claim 2, characterized in that, During the heating process before die forging, the billet only needs to be wrapped with aluminum silicate insulation cotton.

6. The method according to claim 1, characterized in that, The minimum wall thickness of the second mold must be greater than 180mm.

Citation Information

Patent Citations

  • Process method for preforming large-scale high-temperature alloy cone disc moulding bed blank

    CN115889654A