Glass fiber with good alkali resistance and method for preparing the same

By optimizing the glass composition and process, glass fibers with good alkali resistance were prepared, which solved the shortcomings of medium-alkali glass fibers in terms of alkali resistance and production efficiency, and realized a high-strength and low-cost glass fiber alternative.

CN117800609BActive Publication Date: 2026-11-20ТАЙ'АНЬ ШУНЬМАО НЬЮ МЕТЕРИАЛ ТЕХНОЛОДЖИ КО ЛТД
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310727311.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-19
Publication Date
2026-11-20
Estimated Expiration
2043-06-19

AI Technical Summary

Technical Problem

Existing glass fibers have shortcomings in terms of alkali resistance and production cost. In particular, medium-alkali glass fibers are prone to leaching alkali metal ions in humid environments, leading to corrosion. Moreover, they have low production efficiency and high costs, and cannot effectively replace AR and C glass.

Method used

By optimizing the glass composition and introducing oxides such as ZrO₂, ZnO, and TiO₂, and controlling their proportions, glass fibers with good alkali resistance are formed. Using specific melting and drawing processes, glass fibers with high mechanical strength and good alkali resistance are prepared.

Benefits of technology

It achieves significant improvements in the alkali and water resistance of glass fiber, increases production efficiency, reduces costs, and can replace medium-alkali glass fiber for EIFS and GRC reinforcement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004293404350000061
    Figure BDA0004293404350000061
Patent Text Reader

Abstract

The application discloses a glass fiber with good alkali resistance and a preparation method thereof, which comprises the following components: 61.0-72.0 wt% of SiO2; 0-5.0 wt% of Al2O3; 6.0-20.0 wt% of alkaline earth metal oxide RO; 6.0-16.0 wt% of alkali metal oxide R2O; 1.0-7.0 wt% of ZrO2; 0.1-5.0 wt% of ZnO; 0-1.0 wt% of iron oxide and 0-2.0 wt% of F ‑ The glass fiber with good alkali resistance has a glass melting and clarifying temperature of 1400-1480 DEG C, a fiber drawing forming temperature of 1170-1250 DEG C, a crystallization temperature interval of 1030-1120 DEG C, is easy to be drawn into a fiber, has low manufacturing cost, high mechanical strength, good alkali resistance, can replace medium-alkali mesh cloth and is used for EIFS reinforcement and can also be used for GRC reinforcement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to glass fiber materials for reinforcement, and particularly to a glass fiber with good alkali resistance that can be used to reinforce EIFS and GRC, and a method for preparing the same. Background Technology

[0002] Fiberglass products are widely used in various sectors of the national economy, with electronics, transportation, and construction being the three main application areas. In particular, the fiberglass reinforced cement and fiberglass mesh used for wall reinforcement in the construction industry have high requirements for the alkali resistance of the fiberglass.

[0003] The Chinese building materials standard JC 935-2004 defines alkali-resistant glass (AR glass) as having the following composition: 59.2-60.8 wt% SiO2, 13.9-16.1 wt% R2O, 13.7-15.3 wt% ZrO2, 5.5-6.5 wt% TiO2, 4.0-5.0 wt% CaO, and no more than 1 wt% Al2O3, including 2.2-2.8 wt% K2O and no more than 0.5 wt% Fe2O3. AR glass has strong acid and alkali corrosion resistance, but due to the large amount of ZrO and TiO2 in its composition, the forming temperature reaches 1300℃, and the overall cost of manufacturing fibers is more than three times that of ordinary ECR glass fiber, which limits its application.

[0004] The Chinese building materials standard JC 935-2004 defines medium-alkali glass (C glass) as having the following composition: 66.5%-67.5% SiO2, 5.8-6.6wt% Al2O3, 9.2-9.8wt% CaO, 3.9-4.5wt% MgO, and 11.6-12.4wt% R2O, of which K2O≦0.4wt% and Fe2O3≦not greater than 0.4wt%. C glass has good acid resistance but poor alkali resistance. Moreover, because alkali metal ions are easily released in humid environments, forming alkaline corrosion, C glass also has poor water resistance. C glass belongs to the sodium-calcium-aluminum-silicon quaternary system. It has a relatively high content of silicon oxide and alkali metal oxides, and its viscosity-temperature curve is flatter than that of alkali-free glass. It has a slow hardening speed, making it impossible to achieve large-scale, high-flow-rate, and stable wire drawing. Its production efficiency is low, and its overall cost is not advantageous. Therefore, medium-alkali C glass has been listed as a restricted and eliminated industry in my country's "Catalogue of Industries for Restriction and Elimination" and no new additions are allowed. Summary of the Invention

[0005] The purpose of this invention is to address the shortcomings of the prior art by providing a glass fiber with excellent alkali resistance and its preparation method. The glass fiber has a glass melting and clarifying temperature between 1380℃ and 1460℃, a drawing temperature between 1170℃ and 1250℃, and a crystallization temperature range of 1030℃ to 1120℃, making it easy to draw into fibers. This glass fiber has low manufacturing cost, high mechanical strength, and good alkali resistance, and can replace medium-alkali mesh for EIFS reinforcement, as well as for GRC reinforcement.

[0006] A glass fiber with good alkali resistance, comprising:

[0007] 61.0-72.0 wt% SiO2;

[0008] 6.0-20.0 wt% alkaline earth metal oxides (RO);

[0009] 6.0-16.0 wt% alkali metal oxides R₂O;

[0010] 1.0-7.0 wt% ZrO2;

[0011] 0.1-5.0 wt% ZnO;

[0012] 0-5.0 wt% Al2O3;

[0013] 0-1.0 wt% iron oxides;

[0014] 0-2.0wt% F-;

[0015] The mass fraction ratio of ZnO / ZrO2 is 0.02-1.0, and the mass fraction ratio of SiO2 / ZrO2 is 15-36.

[0016] The glass fiber with good alkali resistance further comprises: 0-6.0 wt% TiO2; 0-3.0 wt% MnO; 0-3.0 wt% La2O3; 0-3.0 wt% CeO2; 0-2.0 wt% Y2O3; 0-5.0 wt% B2O3;

[0017] Furthermore, the alkaline earth metal oxide RO includes CaO and MgO.

[0018] Furthermore, the alkali metal oxide comprises Na2O, Li2O and K2O, with the K2O content preferably being 0-3.0 wt%.

[0019] Furthermore, the iron oxide comprises FeO and Fe2O3, preferably FeO comprising 20%-50% of the combined amount of the two.

[0020] In addition, a method for preparing the above-mentioned glass fiber with good alkali resistance is also provided, including the following steps:

[0021] The mineral raw materials are weighed according to the composition ratio, thoroughly mixed, and then put into a high-temperature melting pool for melting. The melting hot spot temperature is controlled between 1380℃ and 1460℃. After a series of physicochemical reactions in the melting pool, the mineral raw materials become molten glass. After debubbling and clarification, the homogenized molten glass enters the main channel through the flow hole, and is then distributed to the working channel. The temperature of the working channel is controlled between 1270℃ and 1320℃. Each working channel is equipped with a platinum-rhodium alloy sprue, which is electrically heated and its temperature is controlled between 1170℃ and 1250℃, with a temperature control accuracy of no more than ±0.5℃. After the molten glass flows out of the sprue, it is rapidly cooled and simultaneously drawn and wound at high speed by a high-speed drawing machine to produce glass fiber filaments with a fiber diameter of approximately 6μm-25μm.

[0022] Alkali erosion of glass fibers occurs through hydroxide ions (OH-). ˉ The alkali damages the silicon-oxygen framework, generating -Si-O- groups. Ultimately, SiO2 dissolves in the alkaline solution, causing the fiber to lose its original strength. By adding the alkali-resistant oxide ZrO2 to ordinary glass fibers, the ZrO2 on the fiber surface transforms into a gel-like substance of Zr(OH)2, which then undergoes dehydration and polymerization to form a dense film on the glass fiber surface. This film blocks and slows down the erosion rate of hydroxide ions on the silicon-oxygen framework, thus significantly improving the alkali resistance of the glass fiber. Because the raw material price of ZrO2 is relatively high, and increasing the amount of ZrO2 introduced will raise the glass liquidus temperature and drawing temperature, which is detrimental to fiber production control, this invention controls the amount of ZrO2 introduced to below 7%, thereby reducing production costs while ensuring a certain level of alkali resistance in the glass. The applicant's research found that when the amount of ZrO2 introduced is less than 10%, the alkali resistance of glass fibers decreases. However, by introducing a certain amount of ZnO, especially controlling the ratio of ZnO / ZrO2 between 0.03 and 0.25, the surface tension of the glass can be significantly improved, limiting the precipitation of alkali oxides and alkaline earth metal oxides in water and alkaline solutions. This significantly improves the alkali resistance, water resistance, and durability of the glass fibers. Furthermore, the addition of ZnO inhibits the crystallization tendency of the glass and effectively controls the crystallization range, which is beneficial to the stability of glass fiber forming. Therefore, in this application, the amount of ZrO2 introduced is not less than 1%, and preferably the ZnO / ZrO2 content ratio is controlled between 0.03 and 0.25. In addition, since ZnO has a significant effect on improving the acid resistance of glass, the glass fiber described in this invention achieves excellent acid resistance while also achieving good alkali resistance.

[0023] Al₂O₃ is a metal oxide and also an acidic oxide. Adding a small amount of Al₂O₃ can significantly reduce the crystallinity of glass. The incorporation of Al₂O₃ can improve the mechanical strength, durability, chemical stability, and thermal stability of the fibers, but it has a negative impact on alkali resistance. Increasing the Al₂O₃ content will raise the melting temperature and viscosity of the molten glass during manufacturing, thus increasing production costs. Therefore, in this application, the amount of Al₂O₃ introduced is controlled to below 5%.

[0024] Introducing an appropriate amount of TiO2 into the glass composition can improve the crystallization properties of the glass, which is beneficial to the production of glass fibers. Simultaneously, TiO2·nH2O titanium dioxide gel is an amphoteric oxide with high chemical stability. In alkaline solutions, only a trace amount dissolves to form Na2TiO3, while most of the TiO2·nH2O deposits on the glass surface, preventing further alkali corrosion and thus improving the glass's alkali resistance. While TiO2 contributes to improved alkali resistance, more is not always better. When the amount of TiO2 introduced is low, the alkali resistance of the glass gradually increases with increasing TiO2 content. However, when the amount of TiO2 introduced is excessive, the alkali resistance of the glass tends to decrease with increasing TiO2 content. Therefore, in this patent application, the amount of TiO2 introduced is controlled below 6%. Detailed Implementation

[0025] This invention provides a glass composition formed from a batch composition of mineral or chemical products for manufacturing glass fibers with good alkali resistance.

[0026] In an embodiment, the present invention provides a glass composition formed from a batch composition comprising sandstone, zircon, albite, limestone, dolomite, and soda ash.

[0027] The glass composition of the present invention is fiberizable, with a forming temperature of 1170°C-1250°C and a crystallization temperature of 1120°C.

[0028] In the fiber preparation process of this invention, mineral raw materials are weighed according to the component ratio, thoroughly mixed, and then added to a high-temperature melting pool for melting. The melting hot spot temperature is controlled between 1380℃ and 1460℃. After a series of physicochemical reactions in the melting pool, the mineral raw materials become molten glass. After defoaming and clarification, the homogenized molten glass enters the main channel through the flow hole, and is then distributed to the working channel. The temperature of the working channel is controlled between 1270℃ and 1320℃. A platinum-rhodium alloy stencil is installed under each working channel. The stencil is electrically heated, and its temperature is controlled between 1170℃ and 1250℃, with a temperature control accuracy of no more than ±0.5℃. After the molten glass flows out of the stencil, it is rapidly cooled and simultaneously drawn and wound at high speed by a high-speed drawing machine to produce glass fiber filaments with a fiber diameter of approximately 6μm-25μm.

[0029] In one embodiment, the glass composition provided by the present invention comprises 70.3 wt% SiO2, 0.5 wt% Al2O3, 11.6 wt% CaO, 1.9 wt% MgO, 7.1 wt% Na2O, 1.4 wt% K2O, 2.2 wt% ZrO2, 0.15 wt% ZnO, 3.3 wt% TiO2 and 0.6 wt% iron oxide.

[0030] In another embodiment, the glass composition provided by the present invention comprises 66.7 wt% SiO2, 0.9 wt% Al2O3, 12.1 wt% CaO, 4.2 wt% MgO, 8.4 wt% Na2O, 0.8 wt% K2O, 3.3 wt% ZrO2, 0.8 wt% ZnO, 1.2 wt% TiO2 and 0.42 wt% iron oxide.

[0031] In another embodiment, the glass composition provided by the present invention comprises 65.0 wt% SiO2, 2.7 wt% Al2O3, 8.8 wt% CaO, 4.1 wt% MgO, 11.6 wt% Na2O, 1.5 wt% K2O, 2.9 wt% ZrO2, 0.55 wt% ZnO, 0.8 wt% TiO2 and 0.6 wt% iron oxide.

[0032] In another embodiment, the glass composition provided by the present invention comprises 68.8 wt% SiO2, 1.5 wt% Al2O3, 12.6 wt% CaO, 2.8 wt% MgO, 5.5 wt% Na2O, 1.7 wt% K2O, 2.9 wt% ZrO2, 0.4 wt% ZnO, 1.7 wt% TiO2 and 0.58 wt% iron oxide.

[0033] In another embodiment, the glass composition provided by the present invention comprises 71.8 wt% SiO2, 1.6 wt% Al2O3, 10.0 wt% CaO, 2.9 wt% MgO, 6.5 wt% Na2O, 0.6 wt% K2O, 2.5 wt% ZrO2, 0.4 wt% ZnO, 2.4 wt% TiO2, and 0.54 wt% F. - And 0.32 wt% iron oxide.

[0034] In an embodiment of the present invention, the glass fiber with good alkali resistance obtained by the method of the present invention has a tensile strength of more than 0.5 N / TEX (see Table 1).

[0035] In the embodiments of the present invention, the glass fiber with good alkali resistance obtained by the method of the present invention can be stably drawn into fibers on a large stencil with 2400, 4000 or even more holes, with a production efficiency of over 95% (see Table 1).

[0036] In an embodiment of the present invention, the glass fiber yarn with good alkalinity prepared by the method of the present invention can retain more than 80% of its strength after being soaked in a mixed alkaline solution for 24 hours. Under the same conditions, the strength retention rate of C glass fiber yarn is only 60%, while that of E glass fiber yarn is 45%, and that of AR glass fiber yarn is 83% under the same conditions (see Table 1).

[0037] In the embodiments of the present invention, the glass fiber yarn with good alkalinity obtained by the method of the present invention has good hydrolysis resistance and a lower hydrolysis mass loss rate than that of alkali-free glass fiber and medium-alkali glass fiber (see Table 1).

[0038] Table 1. Composition and some physicochemical properties of glass fiber

[0039]

[0040] Note: (1) Oxide data in the table are in wt%;

[0041] (2) Comparative Example 1 is glass fiber for objects, Comparative Example 2 is medium alkali glass fiber, and Comparative Example 3 is based on Example 2, with the ZnO / ZrO2 ratio adjusted to 1.2;

[0042] (3) The alkali resistance strength retention rate test method refers to the rapid alkali resistance test method specified in GB / T29906-2013. Specifically, the alkali solution is a mixed solution of Ca(OH)2, NaOH, and KOH, the immersion temperature is (60±2)℃, and the test time is 24h. The alkali resistance mass retention rate test method is to measure the mass retention rate by accelerated aging at 96℃ for 24h in a 5% NaOH solution.

[0043] (4) Acid resistance mass retention rate test: The test method is to immerse the sample in a 5% (w / w) H2SO4 solution at 80℃.

[0044] The acid resistance strength retention rate was measured after 24 hours of accelerated aging under certain conditions; the results were obtained by immersing the sample in a 10% hydrochloric acid solution at 25°C for 7 days.

[0045] (5) The test method for hydrolysis resistance mass loss rate is to use flowing deionized water at 96±2℃ for 24 hours in complete contact.

[0046] The comparison of the above embodiments and comparative examples shows that by optimizing the dosage of SiO2, ZrO2 and ZnO, the alkali resistance of glass fiber is unexpectedly improved. The alkali resistance strength retention rate is higher than that of alkali-free glass fiber and medium-alkali glass fiber. Moreover, the tensile strength of the precursor fiber is higher than that of medium-alkali glass fiber, and it can replace medium-alkali glass fiber mesh for wall reinforcement, etc.

[0047] This specification illustrates various aspects relating to the invention, but does not present certain aspects that would be obvious to those skilled in the art, in order to simplify the specification. Although certain embodiments have been set forth in the description of the invention, the invention is not limited to the specific embodiments disclosed, which are intended to explain the invention in accordance with the definition provided in the appended claims.

Claims

1. A glass fiber with good alkali resistance, characterized in that, It consists of the following components by mass percentage of oxides: 65.0-72.0 wt% SiO2; 12.9-20.0 wt% alkaline earth metal oxides (RO); 6.0-16.0 wt% alkali metal oxides R₂O; 1.0-7.0 wt% ZrO2; 0.15-5.0 wt% ZnO; 0.5-5.0 wt% Al2O3; 0-1.0 wt% iron oxides; 0-2.0wt%F - ; 0.8-3.3 wt% TiO2; The mass fraction ratio of ZnO / ZrO2 is 0.03-0.25, and the mass fraction ratio of SiO2 / ZrO2 is 15-36. The alkali resistance strength retention rate is between that of alkali-resistant glass fiber (AR glass fiber) and medium-alkali glass fiber (C glass).

2. The glass fiber with good alkali resistance as described in claim 1, characterized in that, Also includes: 0-3.0wt% MnO; 0-3.0wt% La2O3; 0-3.0wt% CeO2; 0-2.0 wt% Y₂O₃; 0-5.0 wt% B₂O₃ and 0-3.0 wt% Li₂O.

3. The glass fiber with good alkali resistance as described in claim 1, characterized in that, The alkaline earth metal oxide RO contains CaO and MgO.

4. The glass fiber with good alkali resistance as described in claim 1, characterized in that, The alkali metal oxide comprises Na2O, Li2O and K2O, with the K2O content being 0-3.0 wt%.

5. The glass fiber with good alkali resistance as described in claim 1, characterized in that, The iron oxide comprises FeO and Fe2O3, wherein the FeO constitutes 20%-50% of the combined amount of the two.

6. The glass fiber with good alkali resistance as described in claim 1, characterized in that, The fiberglass mesh woven from it has a tensile breaking strength that is more than 50% higher than that of medium-alkali fiberglass mesh.

7. The method for preparing glass fiber with good alkali resistance as described in any one of claims 1-6, characterized in that, The process includes the following steps: Mineral raw materials are weighed according to their composition ratio, thoroughly mixed, and then melted in a high-temperature melting pool, with the melting hot spot temperature controlled between 1380℃ and 1460℃; after a series of physicochemical reactions in the melting pool, the mineral raw materials become molten glass. After debubbling and clarification, the homogenized molten glass enters the main channel through the flow hole, and is then distributed to the working channels. The temperature of the working channels is controlled between 1270℃ and 1320℃. Each working channel is equipped with a platinum-rhodium alloy sprue, which is electrically heated, with the sprue temperature controlled between 1170℃ and 1250℃, and the sprue temperature control accuracy not exceeding ±0.5℃; after flowing out of the sprue, the molten glass is rapidly cooled while being drawn and wound at high speed by a high-speed drawing machine to produce glass fiber filaments with a fiber diameter of 6μm-25μm.

Citation Information

Patent Citations

  • Alkali-resistant glass fiber composition

    GB2029399A