A process for the hydrolysis and esterification of nitriles

The cyano hydrolysis esterification reaction using hierarchical porous Silicalite-1 molecular sieve catalyst solves the problems of equipment corrosion and wastewater treatment in traditional esterification reactions, achieving efficient and low-cost conversion and esterification of nitrile compounds, which has significant application value.

CN117800840BActive Publication Date: 2026-11-20CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211153994.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-21
Publication Date
2026-11-20
Estimated Expiration
2042-09-21

AI Technical Summary

Technical Problem

Traditional esterification reactions using liquid protic acid catalysts lead to equipment corrosion, cumbersome post-treatment, high production costs for enterprises, and difficulty in meeting wastewater standards. Existing solid acid catalysts suffer from short catalyst life, high cost, and difficulty in commercialization.

Method used

Using hierarchical porous Silicalite-1 molecular sieve as a catalyst, esterification of nitrile compounds is carried out under heterogeneous, non-toxic, and harmless conditions via cyano hydrolysis esterification reaction. Highly efficient catalysis is achieved by utilizing the multi-cavity structure and silanol active centers of the molecular sieve.

Benefits of technology

High conversion rates of nitrile compounds and selectivity of ester compounds were achieved under mild reaction conditions. The method is simple, efficient, low-cost, and environmentally friendly. The catalyst has thermal stability and a large specific surface area, making it suitable for various reactor types.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117800840B_ABST
    Figure CN117800840B_ABST
Patent Text Reader

Abstract

The present disclosure relates to a method for hydrolysis-esterification of nitrile compounds, comprising the following steps: contacting nitrile compounds with a catalyst for hydrolysis-esterification of cyano group; the catalyst comprises hierarchical pore Silicalite-1 molecular sieve, which has multiple cavity structures in the crystal. The method can achieve high conversion of nitrile compounds and high selectivity of ester products without using toxic and harmful solvents.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of organic chemical engineering, and specifically to a method for the hydrolysis and esterification of nitrile. Background Technology

[0002] Esterification is an important chemical reaction in the field of organic chemistry. The esters produced by the reaction are used in food, coatings, fragrances, detergents, cosmetics, plasticizers, pharmaceuticals and pesticide intermediates.

[0003] Traditional ester synthesis typically involves a two-step process: first, the aldehyde is oxidized to the corresponding acid or its derivative, and then the acid undergoes further esterification. The esterification reaction uses an acid as a catalyst; liquid proton acids such as sulfuric acid are commonly used catalysts in this type of reaction and are widely applied in chemical production. Although the synthesis technology using liquid proton acids like sulfuric acid as catalysts is relatively mature, the severe corrosion of equipment caused by these catalysts, the cumbersome post-processing steps, and the significant increase in production costs for enterprises are problems that are currently facing and urgently need to be solved. Simultaneously, with increasing emphasis on environmental protection, the high salinity wastewater generated by traditional processes is difficult to meet the environmental impact assessment requirements for industrial wastewater discharge. Therefore, researchers are exploring the use of solid acids to replace traditional catalysts to address the problems caused by proton acids.

[0004] In recent years, solid acid catalysts that have been extensively studied include molecular sieves, supported heteropoly acids, modified clay minerals, ion exchange resins, metal oxides, and solid superacids, all of which have been reported in esterification reaction studies. Tejero et al. (MATejero, E. Ramírez, C. Fité, J. Tejero, F. Cunill. Applied Catalysis A: General, 2016, 517: 56-66) reported on the esterification reaction of oleic acid and methanol catalyzed by modified ion exchange resin catalysts. Experimental results showed that ZnCl2-modified ion exchange resins exhibited good catalytic activity and high yields. However, the preparation process of modified ion exchange resins is cumbersome and not conducive to industrial application, thus limiting their application scope. Wang et al. (Wang BH, Sun WJ, Zhu J. Industrial & Engineering Chemistry Research, 2012, 51(46): 15004–15010) prepared a Pd-Pb / SDB catalyst by depositing Pb and Pd on a hydrophobic styrene-divinylbenzene (SDB) copolymer. This catalyst can be used for the oxidative esterification of methacrolein with methanol to methyl methacrylate. However, many problems still exist, such as short catalyst lifetime and high catalyst synthesis cost, making it difficult to achieve commercialization. Summary of the Invention

[0005] The purpose of this disclosure is to provide a simple, efficient, low-cost, and environmentally friendly method for the hydrolysis and esterification of nitrile compounds, which does not require the use of toxic or harmful solvents and can achieve high conversion rates of nitrile compounds and selectivity of esterification reaction products.

[0006] To achieve the above objectives, this disclosure provides a method for cyanide hydrolysis esterification, comprising the following steps: contacting a cyanide compound with a catalyst to carry out a cyano hydrolysis esterification reaction; wherein the catalyst comprises a hierarchical porous Silicalite-1 molecular sieve, the hierarchical porous Silicalite-1 molecular sieve having multiple cavity structures within its crystals.

[0007] Optionally, the nitrile compound is selected from one or more of hydrocarbon nitrile compounds and aryl nitrile compounds and their derivatives;

[0008] Preferably, in the hydrocarbon nitrile compounds, the hydrocarbon group is selected from one or more of alkyl groups having 2 to 10 carbon atoms and alkenyl groups having 3 to 10 carbon atoms; in the aryl nitrile compounds and their derivatives, the aryl group is selected from one or more of aryl groups having 6 to 12 carbon atoms and heteroaryl groups having 5 to 15 carbon atoms.

[0009] More preferably, the hydrocarbon nitrile compound is selected from one or more of acetonitrile, propionitrile, butyronitrile, valerate, hexanoic acid, heptanitrile, octanoic acid, nonanoic acid, decanitrile, acrylonitrile, butenonitrile, and hexenonitrile; the aryl nitrile compound and its derivatives are selected from one or more of phthalonitrile, 4-cyanopyridine, cyclohexanenitrile, and 2-(3-methoxyphenyl)-2-methylpropionitrile.

[0010] Preferably, the method further includes: contacting the nitrile compound with a catalyst in the presence of a solvent to carry out the cyano hydrolysis esterification reaction;

[0011] Optionally, the solvent is selected from one or more of methanol, ethanol, propanol, butanol and hexanol;

[0012] Preferably, the molar ratio of the nitrile compound to the solvent is 1:(3-100), more preferably 1:(5-50).

[0013] Optionally, the conditions for the cyano hydrolysis esterification reaction include: a reaction temperature of 200–450°C, preferably 350–400°C; a reaction time of 1–72 h, preferably 10–24 h; a reaction pressure of 0.1–3 MPa, preferably 0.1–2 MPa; and a weight hourly space velocity (WHSV) of 0.1–15 h⁻¹ for the nitrile compound. -1 Preferably 0.2 to 10 hours -1 ;

[0014] Optionally, the reactor for the cyano hydrolysis esterification reaction is selected from any one of a fixed-bed reactor, a batch reactor, a moving-bed reactor, a suspended-bed reactor, or a slurry-bed reactor.

[0015] Optionally, in the hierarchical porous Silicalite-1 molecular sieve, the size of a single cavity structure is 5 to 150 nm, preferably 10 to 100 nm;

[0016] Preferably, the volume of all the cavity structures accounts for 10-95% of the total volume of the molecular sieve; more preferably, it is 15-90% by volume.

[0017] Optionally, the shape of the cavity structure is selected from one or more of the following: sphere, cube, ellipsoid, and irregular cube.

[0018] Optionally, the hierarchical porous Silicalite-1 molecular sieve has the following characteristics: 31 P MAS NMR characteristics:

[0019] The peak intensity of the characteristic peak at a chemical shift of -5±1ppm for the hierarchical porous Silicalite-1 molecular sieve is denoted as N1; the peak intensity of the characteristic peak at a chemical shift of -34±1ppm for the hierarchical porous Silicalite-1 molecular sieve is denoted as N2; and the peak intensity of the characteristic peak at a chemical shift of -61±1ppm for the hierarchical porous Silicalite-1 molecular sieve is denoted as N3.

[0020] As defined in equation (1), X1 can be any value between 0.10 and 0.30;

[0021] X1 = N1 / N3 (Equation 1); and

[0022] As defined in equation (2), X2 is any value between 0.15 and 0.45;

[0023] X2 = N2 / N3 (Equation 2);

[0024] Preferably, X1 is any value between 0.15 and 0.25; X2 is any value between 0.20 and 0.35.

[0025] Optionally, the hierarchical porous Silicalite-1 molecular sieve has the following characteristics: 29 Si MAS NMR characteristics:

[0026] The peak area of ​​the chemical shift peak of the hierarchical porous Silicalite-1 molecular sieve in the range of -102 to -104 ppm is denoted as Q. 3 The peak area of ​​the spectral peak with a chemical shift in the range of -112 to -114 ppm is denoted as Q.4 As defined in equation (3), X3 is any value between 2% and 30% in the following formula:

[0027] X3 = Q 3 / Q 4 ×100% Equation (3);

[0028] Preferably, X3 is any value between 5% and 25%.

[0029] Optionally, the hierarchical porous Silicalite-1 molecular sieve has the following characteristics: 1 HMAS NMR characteristics:

[0030] The hierarchical porous Silicalite-1 molecular sieve 1 In the peak separation results of the 1–6 ppm chemical shift range of the HMAS NMR spectrum: the peak area of ​​the peak in the 1.6–1.8 ppm chemical shift range is recorded as A1, the peak area of ​​the peak in the 2.0–2.2 ppm chemical shift range is recorded as A2, the peak area of ​​the peak in the 3.1–3.3 ppm chemical shift range is recorded as A3, the peak area of ​​the peak in the 4.4–4.6 ppm chemical shift range is recorded as A4, and the sum of the peak areas of A1 to A4 is recorded as A0.

[0031] X is defined as follows (4-1) 4-1 Any value between 14% and 32%

[0032] X 4-1 =A1 / A0×100% Equation (4-1);

[0033] X is defined as follows (4-2) 4-2 Any value between 23% and 41%

[0034] X 4-2 =A2 / A0×100% Equation (4-2);

[0035] X is defined as follows (4-3) 4-3 Any value between 16% and 35%

[0036] X 4-3 =A3 / A0×100% Equation (4-3);

[0037] X is defined as follows (4-4) 4-4 Any value between 4% and 20%

[0038] X 4-4 =A4 / A0×100% Equation (4-4).

[0039] Optionally, the multi-level porous Silicalite-1 molecular sieve includes molecular sieve particles composed of a single crystal, and / or molecular sieve particles composed of aggregates of multiple crystals.

[0040] Optionally, the molecular sieve particles have an average particle size of 0.1–2 μm, preferably 0.2–1.2 μm; and a BET specific surface area of ​​300–650 m². 2 / g, preferably 350-550m 2 / g; microporous specific surface area is 200-550m² 2 / g, preferably 250-450m 2 / g; total pore volume is 0.2–0.7 cm³. 3 / g, preferably 0.3-0.5cm 3 / g; mesopore volume is 0.1~0.5cm³ 3 / g, preferably 0.2~0.4cm 3 / g;

[0041] Optionally, a hysteresis loop exists between the adsorption isotherm and desorption isotherm of the hierarchical porous Silicalite-1 molecular sieve for low-temperature nitrogen adsorption.

[0042] Optionally, the hierarchical porous Silicalite-1 molecular sieve is prepared by a method comprising the following steps:

[0043] S1. Mix the silicon source, the first template agent, water, the silanizing agent and the structural filler to obtain a reaction mixture, wherein the structural filler is an amphiphilic surfactant and / or a hard template agent;

[0044] S2. The reaction mixture is subjected to a first hydrothermal crystallization treatment and a first calcination treatment in sequence to obtain a molecular sieve intermediate;

[0045] S3. Mix the molecular sieve intermediate, the second template agent and water, and then perform a second hydrothermal crystallization treatment and a second calcination treatment in sequence.

[0046] Optionally, in step S1, the molar ratio of silicon source: first template agent: water: silanizing agent is 1:(0.01~2):(1~50):(0.02~0.2); preferably 1:(0.02~0.3):(5~30):(0.03~0.15); the weight ratio of SiO2 to structural filler in the reaction mixture is (5~40):1, preferably (5~30):1.

[0047] Optionally, in step S1, the silicon source is selected from at least one of silicone grease, solid silica gel, fumed silica, and silica sol; preferably, it is selected from at least one of silicone grease, solid silica gel, and fumed silica.

[0048] A further preferred option is a silicone grease, wherein the silicone grease has the general formula shown in formula (A):

[0049]

[0050] Where R a R b R c R d Each is independently selected from alkyl groups having 1 to 6 carbon atoms, wherein the alkyl group is branched or straight-chain alkyl; preferably, R a R b R c R d Each is independently selected from straight-chain alkyl groups having 1 to 4 carbon atoms or branched alkyl groups having 3 to 4 carbon atoms; more preferably, the R a R b R c R d Each of the following is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, or tert-butyl; more preferably, the silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate, and dimethyl diethyl silicone grease.

[0051] Optionally, the first template agent in step S1 and the second template agent in step S3 are organic bases; and each is preferably selected independently from at least one of quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines;

[0052] More preferably, the first template agent and the second template agent are each independently selected from at least one of quaternary ammonium bases having the structure shown in formula (B):

[0053] R1, R2, R3 and R4 are each selected from alkyl groups having 1 to 4 carbon atoms, preferably straight-chain alkyl groups having 1 to 4 carbon atoms and branched alkyl groups having 3 to 4 carbon atoms, and more preferably R1, R2, R3 and R4 are each selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.

[0054] More preferably, the first template agent and the second template agent are each independently tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide.

[0055] Optionally, in step S1, the silanizing agent has the general formula R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, alkyl, alkoxy, aromatic, mercapto, or amino group, and at least one of R5, R6, R7, and R8 is an alkyl, alkoxy, aromatic, mercapto, or amino group; the alkyl, alkoxy, mercapto, and amino groups each have an independent number of carbon atoms of C1 to C2. 18 ;

[0056] Preferably, the silanizing agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane; more preferably, it is selected from one or more of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane.

[0057] Optionally, in step S1, the structural filler is selected from one or more of hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, PEO-PPO-PEO triblock copolymer, mesoporous carbon, and natural cellulose.

[0058] Optionally, step S1 includes:

[0059] a. Mix the silicon source, the first template agent, and water to obtain a silicon hydrolysis sol;

[0060] b. Add the silanizing agent and the structural filler to the hydrolyzed silicon sol, respectively, and mix to obtain the reaction mixture;

[0061] Optionally, the mixing conditions in step a include stirring at 40–90°C for 6–12 hours;

[0062] Optionally, the mixing conditions in step b include stirring at 20–50°C for 2–4 hours;

[0063] Preferably, the silicon source is an organosilicon grease, and step a further includes a hydrolysis and alcohol removal treatment after mixing the silicon source, the first template agent and water to obtain the silicon hydrolysate;

[0064] Optionally, the conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 40–90°C for 6–12 hours; preferably, stirring and hydrolyzing at 60–85°C for 8–10 hours.

[0065] Optionally, in step S3, the weight ratio of the molecular sieve intermediate: the second template agent: water is 1:(0.01~1.5):(1~15); preferably 1:(0.1~1):(2~10).

[0066] Optionally, the conditions for the first hydrothermal crystallization treatment in step S2 and the second hydrothermal crystallization treatment in step S3 each independently include: a hydrothermal crystallization time of 0.25 to 7 days and a hydrothermal crystallization temperature of 130 to 200°C; preferably, a hydrothermal crystallization time of 1 to 3 days and a hydrothermal crystallization temperature of 150 to 180°C; and the pressure is self-generated pressure.

[0067] The conditions for the first roasting treatment in step S2 and the second roasting treatment in step S3 each independently include: a roasting temperature of 300-700℃ and a roasting time of 1-16h; preferably, a roasting temperature of 400-600℃ and a roasting time of 2-5h.

[0068] Through the above technical solution, this disclosure provides a method for cyanohydrolysis esterification of nitrile compounds, realizing the cyanohydrolysis esterification reaction of nitrile compounds under heterogeneous, non-toxic, and harmless reaction conditions. High conversion rates of nitrile compounds and selectivity of ester compounds can be obtained under mild reaction conditions. This method is simple, efficient, low-cost, and environmentally friendly, possessing significant application value and sustainable development significance. The catalyst used in this disclosure is a molecular sieve material, which possesses thermal and chemical stability and a hierarchical porous structure, facilitating product diffusion. Furthermore, the molecular sieve crystal has a multi-cavity structure containing abundant silanol active centers. Its multi-cavity structure provides numerous independent reaction units, and the concentrated distribution of silanol groups enables the molecular sieve to simultaneously possess… It possesses both acid and Lewis acid properties, along with a large specific surface area and pore volume, which is beneficial for efficient catalytic reactions.

[0069] Other features and advantages of this disclosure will be described in detail in the following detailed description section. Attached Figure Description

[0070] The accompanying drawings are provided to further illustrate the present disclosure and form part of the specification. They are used together with the following detailed description to explain the present disclosure, but do not constitute a limitation thereof. In the drawings:

[0071] Figure 1 These are TEM images of the molecular sieve products obtained in Example 1.

[0072] Figure 2 This is the XRD pattern of the molecular sieve product obtained in Example 1;

[0073] Figure 3The molecular sieve product obtained in Preparation Example 1 is compared with the molecular sieve product obtained in Preparation Example 2. 31 P-TMP MASNMR spectrum;

[0074] Figure 4 These are SEM images of the molecular sieve products obtained in Example 1.

[0075] Figure 5 This is a BET curve of the molecular sieve product obtained in Example 1;

[0076] Figure 6 This is the infrared hydroxyl spectrum of the molecular sieve product obtained in Example 1;

[0077] Figure 7 It is the molecular sieve product obtained in Example 1. 29 Si MAS NMR spectrum;

[0078] Figure 8 It is the molecular sieve product obtained in Example 1. 1 HMAS NMR spectrum;

[0079] Figure 9 These are TEM images of the intermediate product obtained in Example 1.

[0080] Figure 10 This is the XRD pattern of the molecular sieve product obtained in Preparation Example 10;

[0081] Figure 11 This is the XRD pattern of the molecular sieve product obtained in Preparation Example 11;

[0082] Figure 12 These are TEM images of the molecular sieve products obtained in Comparative Example 2. Detailed Implementation

[0083] The following provides a detailed description of specific embodiments of this disclosure. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit this disclosure.

[0084] This disclosure provides a method for the hydrolysis and esterification of nitrile, comprising the following steps:

[0085] A cyano hydrolysis esterification reaction is carried out by contacting nitriles with a catalyst;

[0086] The catalyst comprises a hierarchical porous Silicalite-1 molecular sieve, wherein the hierarchical porous Silicalite-1 molecular sieve has multiple cavity structures within its crystals.

[0087] This disclosure provides a method for the hydrolytic esterification of nitrile compounds, achieving cyanohydrolytic esterification of nitrile compounds under heterogeneous, non-toxic, and harmless reaction conditions. High conversion rates of nitrile compounds and selectivity of ester compounds can be obtained under mild reaction conditions. This method is simple, efficient, low-cost, and environmentally friendly, possessing significant application value and implications for sustainable development. The catalyst used in this disclosure is a molecular sieve material, exhibiting thermal and chemical stability and a hierarchical porous structure that facilitates product diffusion. Furthermore, the molecular sieve has a multi-cavity structure within its crystals, containing abundant silanol active centers. This multi-cavity structure provides numerous independent reaction units, and the concentrated distribution of silanol groups allows the molecular sieve to simultaneously possess… It possesses both acid and Lewis acid properties, along with a large specific surface area and pore volume, which is beneficial for efficient catalytic reactions.

[0088] In one embodiment, the nitrile compound is selected from one or more of hydrocarbon nitrile compounds and aryl nitrile compounds and their derivatives;

[0089] Preferably, in the hydrocarbon nitrile compounds, the hydrocarbon group is selected from one or more of alkyl groups having 2 to 10 carbon atoms and alkenyl groups having 3 to 10 carbon atoms; in the aryl nitrile compounds and their derivatives, the aryl group is selected from one or more of aryl groups having 6 to 12 carbon atoms and heteroaryl groups having 5 to 15 carbon atoms.

[0090] More preferably, the hydrocarbon nitrile compound is selected from one or more of acetonitrile, propionitrile, butyronitrile, valerate, hexanonitrile, heptanonitrile, octanonitrile, nonanonitrile, decanonitrile, acrylonitrile, butenonitrile, and hexenonitrile; the aryl nitrile compound and its derivatives are selected from one or more of phthalonitrile, 4-cyanopyridine, cyclohexanenitrile, and 2-(3-methoxyphenyl)-2-methylpropionitrile.

[0091] In a preferred embodiment, the method further includes:

[0092] The cyano hydrolysis esterification reaction is carried out by contacting a nitrile compound with a catalyst in the presence of a solvent.

[0093] In one specific embodiment, the solvent is selected from one or more of methanol, ethanol, propanol, butanol, and hexanol;

[0094] Preferably, the molar ratio of the nitrile compound to the solvent is 1:(3-100), more preferably 1:(5-50).

[0095] In one embodiment, the conditions for the cyano hydrolysis esterification reaction include: a reaction temperature of 200–450°C; a reaction time of 1–72 h; a reaction pressure of 0.1–3 MPa; and a weight hourly space velocity (WHSV) of 0.1–15 h⁻¹ for the nitrile compound. -1The weight ratio of nitrile compounds to catalysts is (1-100):1.

[0096] In a preferred embodiment, the conditions for the cyano hydrolysis esterification reaction include: a reaction temperature of 350–400°C; a reaction time of 10–24 h; a reaction pressure of 0.1–2 MPa; and a weight hourly space velocity (WHSV) of 0.2–10 h⁻¹ for the nitrile compound. -1 The weight ratio of nitrile compound to catalyst is (1-20):1. Following this embodiment, the hydrolysis-esterification reaction of nitrile compounds yields higher nitrile compound conversion and ester product selectivity.

[0097] In one specific embodiment, the reactor for the catalytic reaction is selected from any one of a fixed-bed reactor, a batch reactor, a moving-bed reactor, a suspended-bed reactor, or a slurry-bed reactor.

[0098] In a preferred embodiment, the hierarchical porous Silicalite-1 molecular sieve has multiple cavity structures within its crystal; wherein the size of a single cavity structure is 5–150 nm, preferably 10–100 nm.

[0099] In this disclosure, the cavity structure and its size in the molecular sieve are obtained by transmission electron microscopy (TEM). In this disclosure, the size of the cavity structure refers to the distance between any two positions on the cavity wall passing through the center of the cavity structure in a TEM image of the molecular sieve; for example, "the size of a single cavity structure is 5–150 nm" means that the distance between any two positions on the cavity wall passing through the center of any cavity structure in the molecular sieve is within the range of 5–150 nm.

[0100] In a preferred embodiment, the volume of all the cavity structures accounts for 10-95% of the total volume of the molecular sieve, more preferably 15-90% by volume;

[0101] Optionally, the shape of the cavity structure is selected from one or more of the following: sphere, cube, ellipsoid, and irregular cube.

[0102] In one embodiment, the hierarchical porous Silicalite-1 molecular sieve has the following characteristics: 31 P MAS NMR characteristics:

[0103] The peak intensity of the characteristic peak at a chemical shift of -5±1ppm for the hierarchical porous Silicalite-1 molecular sieve is denoted as N1; the peak intensity of the characteristic peak at a chemical shift of -34±1ppm for the hierarchical porous Silicalite-1 molecular sieve is denoted as N2; and the peak intensity of the characteristic peak at a chemical shift of -61±1ppm for the hierarchical porous Silicalite-1 molecular sieve is denoted as N3.

[0104] As defined in equation (1), X1 can be any value between 0.10 and 0.30;

[0105] X1 = N1 / N3 (Equation 1); and

[0106] As defined in equation (2), X2 is any value between 0.15 and 0.45;

[0107] X2 = N2 / N3 Equation (2).

[0108] In this disclosure, for hierarchical porous Silicalite-1 molecular sieves 31 In the P-TMP MAS NMR spectrum analysis, trimethylphosphorus (TMP) was used as the probe molecule, and the testing method is a conventional method in the art. The inventors of this disclosure have discovered that when the hierarchical porous Silicalite-1 molecular sieve simultaneously possesses… When considering acid and Lewis acid properties, trimethylphosphorus (TMP) is used as a probe molecule. 31 In the pMAS NMR spectrum, a chemical shift of -5 ± 1 ppm was used as... The characteristic peaks of acid properties were determined, with a chemical shift of -34±1 ppm as the characteristic peak of Lewis acid properties, and a chemical shift of -61±1 ppm as the characteristic peak of TMP physisorption; using these TMP physisorption characteristic peaks as a comparison benchmark, ... The characteristic peaks of the acid properties and Lewis acid properties were compared with the characteristic peak of the TMP physisorption. When the ratio of the peak intensity of the two acid properties to the peak intensity of the TMP physisorption characteristic peak meets a certain range, the hierarchical porous Silicalite-1 molecular sieve can have better catalytic activity and reaction stability.

[0109] In a preferred embodiment, X1 is any value between 0.15 and 0.25; X2 is any value between 0.2 and 0.35. When X1 and X2 of the hierarchical porous Silicalite-1 molecular sieve meet the range of this embodiment, the hierarchical porous Silicalite-1 molecular sieve exhibits higher catalytic activity and catalytic stability.

[0110] In one embodiment, the hierarchical porous Silicalite-1 molecular sieve has the following characteristics: 29 Si MAS NMR characteristics:

[0111] The peak area of ​​the chemical shift peak of the hierarchical porous Silicalite-1 molecular sieve in the range of -102 to -104 ppm is denoted as Q. 3The peak area of ​​the spectral peak with a chemical shift in the range of -112 to -114 ppm is denoted as Q. 4 As defined in equation (3), X3 is any value between 2% and 30% in the following formula:

[0112] X3 = Q 3 / Q 4 ×100% Equation (3);

[0113] Preferably, X3 is any value between 5% and 25%.

[0114] In this disclosure, a peak with a chemical shift around -103 ppm represents a tricoordinated silica group, and a peak with a chemical shift around -113 ppm represents a tetracoordinated silica group. The hierarchical porous Silicalite-1 molecular sieve has abundant silanol groups.

[0115] The hierarchical porous Silicalite-1 molecular sieve disclosed herein 1 In the 1H MAS NMR spectrum, peak signals in the chemical shift range of 1.6–1.8 ppm represent isolated silanol groups, while peak signals in the chemical shift range of 2–6 ppm (2.0–2.2 ppm, 3.1–3.3 ppm, and 4.4–4.6 ppm, respectively) represent silanol groups with hydrogen bonding interactions. The relationship between the peak areas of the above four silanol peaks and the total peak area can be used to reflect the catalytic activity and catalytic stability of the hierarchical porous Silicalite-1 molecular sieve.

[0116] In one embodiment, the hierarchical porous Silicalite-1 molecular sieve has the following characteristics: 1 HMAS NMR characteristics:

[0117] The hierarchical porous Silicalite-1 molecular sieve 1 In the peak separation results of the 1–6 ppm chemical shift range of the HMAS NMR spectrum: the peak area of ​​the peak in the 1.6–1.8 ppm chemical shift range is recorded as A1, the peak area of ​​the peak in the 2.0–2.2 ppm chemical shift range is recorded as A2, the peak area of ​​the peak in the 3.1–3.3 ppm chemical shift range is recorded as A3, the peak area of ​​the peak in the 4.4–4.6 ppm chemical shift range is recorded as A4, and the sum of the peak areas of A1 to A4 is recorded as A0.

[0118] X is defined as follows (4-1) 4-1 Any value between 14% and 32%

[0119] X 4-1 =A1 / A0×100% Equation (4-1);

[0120] X is defined as follows (4-2) 4-2 Any value between 23% and 41%

[0121] X 4-2 =A2 / A0×100% Equation (4-2);

[0122] X is defined as follows (4-3) 4-3 Any value between 16% and 35%

[0123] X 4-3 =A3 / A0×100% Equation (4-3);

[0124] X is defined as follows (4-4) 4-4 Any value between 4% and 20%

[0125] X 4-4 =A4 / A0×100% Equation (4-4).

[0126] In a preferred embodiment, the X of the hierarchical porous Silicalite-1 molecular sieve 4-1 X is any value between 17% and 30%. 4-2 X is any value between 27% and 38%. 4-3 X is any value between 19% and 32%. 4-4 Any value between 6% and 18%. When the hierarchical porous Silicalite-1 molecular sieve meets the X requirement of this embodiment... 1-1 ~X 1-4 Numerical values ​​can further improve the conversion rate of nitrile compounds and the selectivity of esterification products in the hydrolysis and esterification reactions of nitrile compounds.

[0127] In one specific embodiment, the hierarchical porous Silicalite-1 molecular sieve comprises molecular sieve particles consisting of single crystals, and / or molecular sieve particles composed of aggregates of multiple crystals; optionally, the average particle size of the molecular sieve particles is 0.1–2 μm, preferably 0.2–1.2 μm; and the external specific surface area is 300–800 cm². 2 / g, preferably 400-600cm 2 / g; total pore volume is 0.2–0.7 cm³. 3 / g, preferably 0.3-0.5cm 3 / g; mesopore volume is 0.1~0.5cm³ 3 / g, preferably 0.2~0.4cm 3 / g.

[0128] In a preferred embodiment, a hysteresis loop exists between the adsorption isotherm and desorption isotherm of the hierarchical porous Silicalite-1 molecular sieve for low-temperature nitrogen adsorption.

[0129] In one specific embodiment, the initial relative pressure (P / P0) at which the hysteresis loop appears is 0.2 to 0.99, preferably 0.4 to 0.99.

[0130] In one specific embodiment, the configuration of the hierarchical porous Silicalite-1 molecular sieve is selected from one or more of the MFI topology, MEL topology, BEA topology and SVR topology.

[0131] In a preferred embodiment, the hierarchical porous Silicalite-1 molecular sieve is prepared by a method comprising the following steps:

[0132] S1. Mix the silicon source, the first template agent, water, the silanizing agent and the structural filler to obtain a reaction mixture, wherein the structural filler is an amphiphilic surfactant and / or a hard template agent;

[0133] S2. The reaction mixture is subjected to a first hydrothermal crystallization treatment and a first calcination treatment in sequence to obtain a molecular sieve intermediate;

[0134] S3. Mix the molecular sieve intermediate, the second template agent and water, and then perform a second hydrothermal crystallization treatment and a second calcination treatment in sequence.

[0135] This disclosure achieves the effect of expanding the pores of molecular sieves by introducing silanizing agents and macromolecular structural fillers into the molecular sieve synthesis raw materials, thereby preparing molecular sieve materials with open channels. Then, a second template agent is added for dissolution and recrystallization to prepare a hierarchical porous Silicalite-1 molecular sieve with a multi-cavity structure.

[0136] Specifically, in this disclosure, the silanizing agent and the silanizing group of the organosilicon source undergo hydrolytic condensation to generate stable Si-O-Si bonds, thereby ensuring the achievement of the pore-expanding effect. Furthermore, the long carbon chain of the silanizing agent and the structural filler of the amphiphilic surfactant can form stable and controllable structural units (the long carbon chain of the silanizing agent and the hydrophobic group of the surfactant are close to each other and interact by van der Waals forces), thus playing a fine-tuning role in pore expansion; or, a size-controllable hard template agent can be used to fill the space, enabling the molecular sieve to produce an ordered, mesoporous structure with controllable pore size (controlled by the chain length of the alkyl chain of the silanizing agent); then, a second template agent is introduced into the molecular sieve with open pores, utilizing its dissolution-recrystallization mechanism to obtain a hierarchical porous structure of Silicalite-1 molecular sieve.

[0137] In one embodiment, in step S1, the molar ratio of silicon source: first template agent: water: silanizing agent is 1:(0.01~2):(1~50):(0.02~0.2); the weight ratio of SiO2 to structural filler in the reaction mixture is (5~40):1.

[0138] In a preferred embodiment, in step S1, the molar ratio of silicon source: first template agent: water: silanizing agent is 1:(0.02~0.3):(5~30):(0.03~0.15); the weight ratio of SiO2 to structural filler in the reaction mixture is (5~30):1.

[0139] In one embodiment, in step S1, the silicon source is selected from at least one of silicone grease, solid silicone, fumed silica, and silica sol; preferably, it is selected from at least one of silicone grease, solid silicone, and fumed silica.

[0140] A further preferred option is a silicone grease, wherein the silicone grease has the general formula shown in formula (A):

[0141]

[0142] Where R a R b R c R d Each is independently selected from alkyl groups having 1 to 6 carbon atoms, wherein the alkyl group is branched or straight-chain alkyl; preferably, R a R b R c R d Each is independently selected from straight-chain alkyl groups having 1 to 4 carbon atoms or branched alkyl groups having 3 to 4 carbon atoms; more preferably, the R a R b R c R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, or tert-butyl.

[0143] In a preferred embodiment, the silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate, and dimethyl diethyl silicone grease.

[0144] In one embodiment, in step S1, the first template agent is an organic base, preferably at least one selected from quaternary ammonium bases, aliphatic amines, and aliphatic alcohol amines.

[0145] In one specific embodiment, the first template agent is selected from at least one of the quaternary ammonium bases with the general formula (B) shown below:

[0146] R1, R2, R3 and R4 are each selected from alkyl groups having 1 to 4 carbon atoms, preferably straight-chain alkyl groups having 1 to 4 carbon atoms and branched alkyl groups having 3 to 4 carbon atoms, and more preferably R1, R2, R3 and R4 are each selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.

[0147] In a preferred embodiment, the first template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide.

[0148] In one embodiment, step S1 includes:

[0149] a. Mix the silicon source, the first template agent, and water to obtain a silicon hydrolysis sol;

[0150] b. Add the silanizing agent and the structural filler to the hydrolyzed silicon sol, respectively, and mix to obtain the reaction mixture;

[0151] Optionally, the mixing conditions in step a include stirring at 40–90°C for 6–12 hours;

[0152] Optionally, the mixing conditions in step b include stirring at 20–50°C for 2–4 hours.

[0153] In one specific embodiment, the silicon source is an organosilicon grease, and step a further includes a hydrolysis and alcohol removal treatment after mixing the silicon source, the first template agent and water to obtain the silicon hydrolysate;

[0154] Optionally, the conditions for the hydrolysis-induced alcohol removal treatment include: stirring and hydrolyzing at 40–90°C for 6–12 hours; preferably, stirring and hydrolyzing at 60–85°C for 8–10 hours. Preferably, the hydrolysis-induced alcohol removal treatment results in the alcohol content in the silicone hydrolysate of the obtained silicone grease being below 10 ppm by mass.

[0155] In one embodiment, in step S1, the silanizing agent has the general formula R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, alkyl, alkoxy, aromatic, mercapto, or amino group, and at least one of R5, R6, R7, and R8 is an alkyl, alkoxy, aromatic, mercapto, or amino group; the alkyl, alkoxy, mercapto, and amino groups each have an independent number of carbon atoms of C1 to C2. 18 ;

[0156] Preferably, the silanizing agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane; more preferably, it is selected from one or more of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane.

[0157] In one embodiment, the conditions for the first hydrothermal crystallization treatment in step S2 include: a hydrothermal crystallization time of 0.25 to 7 days, a hydrothermal crystallization temperature of 130 to 200°C, and an autogenous pressure.

[0158] The conditions for the first calcination treatment in step S2 include: a calcination temperature of 300–700°C and a calcination time of 1–16 h.

[0159] In a preferred embodiment, the conditions for the first hydrothermal crystallization treatment in step S2 include: a hydrothermal crystallization time of 1 to 3 days, a hydrothermal crystallization temperature of 150 to 180°C, and an autogenous pressure.

[0160] The conditions for the first calcination treatment in step S2 include: a calcination temperature of 400–600°C and a calcination time of 2–5 h. The hierarchical porous Silicalite-1 molecular sieve prepared according to this embodiment exhibits better catalytic activity and catalytic stability.

[0161] In one specific embodiment, after the first hydrothermal crystallization treatment, the method further includes the steps of subjecting the product of the first hydrothermal crystallization treatment to a first filtration treatment and a first drying treatment, followed by the first calcination treatment. The temperature of the first drying treatment is 50–120°C, and the time is 1–12 hours.

[0162] In one embodiment, in step S3, the selection range of the second template agent is the same as that of the first template agent, which will not be repeated here; preferably, the first template agent and the second template agent are the same template agent.

[0163] In one embodiment, in step S3, the weight ratio of the molecular sieve intermediate, the second template agent, and water is 1:(0.01-1.5):(1-15); preferably 1:(0.1-1):(2-10). Preparing the molecular sieve according to the preferred weight ratio in this embodiment yields a molecular sieve with higher catalytic activity.

[0164] In one embodiment, the conditions for the second hydrothermal crystallization treatment in step S3 include: a hydrothermal crystallization time of 0.25 to 7 days, a hydrothermal crystallization temperature of 130 to 200°C, and an autogenous pressure.

[0165] The conditions for the second calcination treatment in step S3 include: a calcination temperature of 300–700°C and a calcination time of 1–16 h.

[0166] In a preferred embodiment, the conditions for the second hydrothermal crystallization treatment in step S3 include: a hydrothermal crystallization time of 1 to 3 days, a hydrothermal crystallization temperature of 150 to 180°C, and an autogenous pressure.

[0167] The conditions for the second calcination treatment in step S3 include: a calcination temperature of 400–600°C and a calcination time of 2–5 hours.

[0168] In one specific embodiment, after the second hydrothermal crystallization treatment, the method further includes a second filtration treatment and a second drying treatment of the product from the second hydrothermal crystallization treatment, followed by the second calcination treatment. The temperature of the second drying treatment is 50–120°C, and the time is 1–12 hours.

[0169] The present disclosure will be described in detail below through examples.

[0170] The sample 31 P-TMP MAS NMR characterization was performed using an AVANCEⅢ 600WB nuclear magnetic resonance spectrometer with a 4mm dual resonance probe, a Ф4mm ZrO2 rotor, a resonance frequency of 242.9MHz, a magic angle rotation speed of 10kHz, a pulse width of 1.4μs, a cycle delay of 1s, and approximately 6000 scans.

[0171] The X-ray diffraction (XRD) phase pattern of the sample was determined on a Siemens D5005 X-ray diffractometer with Kα (Cu) as the X-ray source and the test range 2θ from 0.5° to 70°.

[0172] Transmission electron microscopy (TEM) images of the samples were obtained using a Tecnai G2F20S-TWIN TEM microscope from FEI. The cavity structure and its dimensions were determined based on TEM measurements. The volume fraction of the cavity structure relative to the total volume of the molecular sieve was obtained by measuring the TEM images: the volume of each cavity in the molecular sieve particles was measured based on the TEM images (calculated spherically, using the median of the sum of the maximum and minimum lengths passing through the center of the cavity structure as the spherical diameter, then obtaining the spherical radius, and finally calculating the percentage of the total volume of all cavities relative to the total volume of the molecular sieve particles; the average value was taken after calculating the cavity structure volume fraction of 50 molecular sieve particles).

[0173] Scanning electron microscopy (SEM) images of the samples were obtained using a Hitachi S4800 high-resolution cold field emission scanning electron microscope. The average particle size of the samples was determined by measuring the SEM images (the average value was taken after testing the particle size of 50 molecular sieves).

[0174] The total specific surface area and total pore volume of the samples were determined using a Micromeritics ASAP245 static nitrogen adsorption analyzer according to the ASTM D4222-98 standard method. The adsorption and desorption isotherms of the samples at low temperatures were determined according to the ASTM D4222-98 standard method.

[0175] Q of the sample 3 / Q 4 Measurement method adopted 29 The Si MAS NMR method was performed on an AVANCEⅢ500WB nuclear magnetic resonance spectrometer using a 7mm dual resonance probe, a Ф7mm ZrO2 rotor, a resonance frequency of 99.3MHz, a rotation speed of 5kHz, a pulse width of 1.8μs, a cycle delay of 2s, and approximately 3000 scans.

[0176] The sample 1 H MAS NMR spectra were obtained on a Varian Infinityplus-400 spectrometer using a 4mm dual resonance probe, a Ф4mm ZrO2 rotor, a resonance frequency of 400.1MHz, a magic angle rotation speed of 10kHz, a pulse width of 3.57μs, a cycle delay of 1s, and approximately 4000 scans.

[0177] The reagents used in the following examples and comparative examples were all purchased through conventional channels.

[0178] Preparation Example 1

[0179] (1) 104g tetraethyl silicate (0.5mol), 65g tetrapropylammonium hydroxide (TPAOH, 0.08mol) aqueous solution with a concentration of 25% by weight and 140g water (7.8mol) were added sequentially into a 500mL beaker, placed on a magnetic stirrer with heating and stirring functions and mixed evenly. The mixture was stirred at 60℃ for 5 hours, and the evaporated water was replenished periodically to obtain a colorless and transparent silica gel solution.

[0180] (2) Add 9g of N-phenyl-3-aminopropyltrimethoxysilane (PHAPTMS, 0.035mol) and 3g of PEO-PPO-PEO triblock copolymer (P123, purchased from Inokai, weight average molecular weight 5800) to the mixture in step (1) and stir for 2 hours.

[0181] (3) The mixture obtained in step (2) was transferred to a stainless steel sealed reactor and crystallized at 170°C for 24 hours to obtain a sample. The sample was filtered, washed, dried at 110°C for 3 hours, and then calcined in a muffle furnace at 550°C for 3 hours to obtain intermediate product M-1.

[0182] (4) Mix 10g of M-1 sample, 20g of 25% by weight tetrapropylammonium hydroxide (TPAOH, 5g) aqueous solution and 40g of water evenly (the weight ratio of molecular sieve intermediate: second template agent: water is 1:0.5:5.5), transfer to a stainless steel sealed reactor, and crystallize at 170℃ for 24h to obtain the sample. Filter and wash the obtained sample, dry it at 110℃ for 3 hours, and then calcine it in a muffle furnace at 550℃ for 3 hours to obtain the multi-level porous Silicalite-1 molecular sieve sample CAT-1.

[0183] The structural parameter characterization results of CAT-1 are listed in Table 2;

[0184] TEM electron microscope images of CAT-1 are as follows Figure 1 As shown, the molecular sieve has a hierarchical porous structure with multiple cavities within the crystal, and the size of a single cavity structure is 10–90 nm.

[0185] TEM of intermediate product M-1 without dissolution and recrystallization, as shown in the image. Figure 9 As shown, Figure 9 and Figure 1 By comparison, it can be seen that Figure 1 The intermediate products, after being dissolved and recrystallized, created a large number of intracrystalline multi-cavity structures;

[0186] The XRD pattern of CAT-1 is as follows Figure 2 As shown, this indicates that CAT-1 is an MFI topology;

[0187] The products obtained by CAT-1 and Comparative Example 2 (prior art) 31 p-TMP MAS NMR spectrum as shown Figure 3 As shown, compared with the molecular sieve DCAT-2 obtained in Comparative Example 2, CAT-1 has a chemical shift of -5 ± 2 ppm. The presence of acid signals, and Lewis acid signals with chemical shifts at -34±2 ppm, indicates that the Silicalite-1 molecular sieve prepared using the method provided in this disclosure simultaneously possesses... The acid and Lewis acid properties, where N1 is 114450, N2 is 158051, and N3 is 545002, the values ​​of X1 and X2 calculated by formulas (1) to (2) are listed in Table 3;

[0188] SEM images of CAT-1 are as follows Figure 4 As shown, the molecular sieve particles have regular shapes and uniform sizes.

[0189] CAT-1 BET Figure 5 As shown, there is a clear hysteresis loop between the nitrogen adsorption and desorption curves, and the initial relative pressure (P / P0) at which the hysteresis loop appears is 0.45.

[0190] The infrared hydroxyl spectrum of CAT-1 is as follows: Figure 6 As shown, distinct silanol active centers can be observed, with the 3740 cm⁻¹ site being particularly prominent. -1 The spectral peak at position 3690 cm⁻¹ represents a terminal hydroxyl group, indicating a side reaction center. -1 The spectral peak at position 3500 cm⁻¹ is for the ortho-hydroxyl group; -1 The spectral peak at the position is a nested silanol, indicating the main reaction center;

[0191] CAT-1 29 Si MAS NMR spectrum as shown Figure 7 As shown in the figure, CAT-1 has peaks at chemical shifts of -103 ppm and -113 ppm. After integration, the peak area Q of the peak at chemical shift -103 ppm is calculated. 3 The peak area Q of the spectral peak with a chemical shift of -113 ppm is 239001. 4 The value of X3, calculated by formula (3), is 1407909 and is listed in Table 3.

[0192] CAT-1 1 HMAS NMR spectrum and its peak fractionation results are as follows Figure 8 As shown in the figure, spectral peaks are present at chemical shifts of 1.7 ppm, 2.0 ppm, 3.2 ppm, and 4.5 ppm, respectively, with corresponding peak areas A1 to A4 of 60728, 87324, 65689, and 36591, respectively. The total area A0 of A1 to A4 is 250332. X is calculated using equations (4-1) to (4-4). 4-1 ~X 4-4 Listed in Table 3.

[0193] Preparation of Comparative Example 1

[0194] The method used in Preparation Example 1 differs from that in that no silanizing agent or structural filler is added, and the resulting product is denoted as DCAT-1. The preparation conditions are listed in Table 1, and the characterization results of the resulting molecular sieve are listed in Tables 2 and 3.

[0195] Preparation of Comparative Example 2

[0196] This comparative example prepared conventional all-silica Silicalite-1 molecular sieves according to the method disclosed in patent CN1338427A, specifically including the following steps:

[0197] (1) Add 104g of tetraethyl silicate, 90g of 22.5% by weight tetrapropylammonium hydroxide (TPAOH) aqueous solution and 110g of water to a 500mL beaker, place it on a magnetic stirrer with heating and stirring functions and mix evenly. Stir at 75℃ for 5 hours, and replenish the evaporated water periodically to obtain a colorless and transparent silica gel solution.

[0198] (2) The above sol was transferred to a stainless steel sealed reactor and crystallized at 170°C for 2 days. After filtration and washing, it was dried at 120°C for 24 hours and then calcined in a muffle furnace at 550°C for 5 hours.

[0199] (3) 15g of the calcined product was mixed with 55g of a 22.5% by weight tetrapropylammonium hydroxide (TPAOH) aqueous solution, and crystallized at 170℃ for 1 day. The mixture was then filtered, washed, dried at 110℃ for 12 hours, and finally calcined in a muffle furnace at 550℃ for 4 hours. The resulting product was designated DCAT-2. The characterization results of the obtained molecular sieve are shown in Tables 2 and 3. The TEM image of DCAT-2 is shown below. Figure 12 As shown in the figure, DCAT-2 molecular sieve does not have an internal cavity structure.

[0200] Preparation Examples 2-9

[0201] The hierarchical porous Silicalite-1 molecular sieve catalyst was prepared according to the method of Preparation Example 1. The difference from Preparation Example 1 is that the ratio and synthesis conditions were changed to obtain hierarchical porous Silicalite-1 molecular sieve samples, which are denoted as CAT-2 to CAT-9. The preparation conditions are listed in Table 1, and the characterization results of the obtained molecular sieves are listed in Tables 2 and 3.

[0202] Preparation Example 10

[0203] Hierarchical porous Silialite-2 molecular sieves were prepared according to the method of Preparation Example 1, except that the template agent was changed to tetrabutylammonium hydroxide (TBAOH) to prepare the MEL topology, resulting in a hierarchical porous molecular sieve sample designated CAT-10. The preparation conditions are listed in Table 1, and the characterization results of the obtained molecular sieves are listed in Tables 2 and 3. The XRD pattern of CAT-10 is shown below. Figure 10 As shown, this indicates that CAT-10 is a MEL structure.

[0204] Preparation Example 11

[0205] Hierarchical porous β-zeolite was prepared according to the method of Preparation Example 1, except that the ratio and template agent were changed. Tetraethylammonium hydroxide (TEAOH) was used as the template agent to prepare the BEA topology, resulting in a hierarchical porous molecular sieve sample designated CAT-11. The preparation conditions are listed in Table 1, and the characterization results of the obtained molecular sieve are listed in Tables 2 and 3. The XRD pattern of CAT-11 is shown below. Figure 11 As shown, this indicates that CAT-11 is a BEA structure.

[0206] Preparation Example 12

[0207] The hierarchical porous Silicalite-1 molecular sieve was prepared according to the method of Preparation Example 1, except that:

[0208] The first hydrothermal crystallization treatment was carried out at a temperature of 130℃ for 4 days; the first calcination treatment was carried out at a temperature of 350℃ for 8 hours.

[0209] The second hydrothermal crystallization treatment was carried out at a temperature of 130℃ for 4 days; the second calcination treatment was carried out at a temperature of 350℃ for 8 hours.

[0210] The obtained multi-level porous Silicalite-1 molecular sieve sample is designated as CAT-12; the characterization results of the obtained molecular sieve are listed in Tables 2 and 3.

[0211] Table 1

[0212]

[0213]

[0214] In Table 1, TPAOH is tetrapropylammonium hydroxide, TBAOH is tetrabutylammonium hydroxide, and TEAOH is tetraethylammonium hydroxide; PHAPTMS is N-phenyl-3-aminopropyltrimethoxysilane, APTMS is 3-aminopropyltriethoxysilane, GCPMS is 3-glycidoxypropyl(dimethoxy)methylsilane, and TOMS is methyltrimethoxysilane; P123 is PEO-PPO-PEO triblock copolymer, and CTAB is hexadecyltrimethylammonium bromide. The reagents used in this disclosure can be obtained through conventional purchasing channels.

[0215] The water in the "water / silicon source" calculation in Table 1 also includes water from the first template agent aqueous solution; the water in the "water / molecular sieve" calculation also includes water from the second template agent aqueous solution.

[0216] Table 2

[0217]

[0218]

[0219] Table 3

[0220]

[0221] Reaction Example 1

[0222] This reaction example is used to illustrate the effect of cyano hydrolysis esterification of the method provided in this disclosure.

[0223] The molecular sieve samples prepared in the above preparation examples and comparative examples were used as catalysts for nitrile hydrolysis esterification. The evaluation apparatus was an atmospheric pressure continuous flow fixed-bed reactor with an inner diameter of 5 mm and a catalyst loading of 2 g. After loading the catalyst, it was pretreated for 3 hours under a nitrogen atmosphere at atmospheric pressure and 350 °C. The concentration of the feedstock hexanolyte was 10% by weight, and the solvent was methanol (molar ratio of hexanolyte to methanol was 1:10). The reaction conditions included a hexanolyte weight hourly space velocity (WHSV, hexanolyte flow rate in feed / catalyst weight in reactor) of 1 h⁻¹. -1 The reaction temperature was 380℃, the reaction pressure was 0.6MPa, the nitrogen flow rate was 4 L / h, and the reaction time was 12 h. The same catalytic reaction was repeated 5 times using the same catalyst.

[0224] The reaction products were collected after cooling, and the concentrations of each substance were quantitatively analyzed by gas chromatography. An Agilent 6890 gas chromatograph with an HP-5 column was used. The test conditions included: vaporization chamber temperature 250℃, detection chamber temperature 230℃, and a programmed column temperature ramp: 110℃ for 8 minutes, ramped to 230℃ at a rate of 15℃ / min, and then held for 14 minutes. The results are shown in Table 4.

[0225] Where the conversion rate of hexanolyte % = (moles of hexanolyte in the raw material - moles of hexanolyte in the product) / moles of hexanolyte in the raw material × 100%;

[0226] Selectivity of methyl hexanoate % = (moles of methyl hexanoate in the product) / (moles of hexanonitrile in the feed - moles of hexanonitrile in the product) × 100%;

[0227] The percentage decrease in hexanoic acid conversion rate = (hexanoic acid conversion rate after 1 reaction - hexanoic acid conversion rate after 5 reactions) / hexanoic acid conversion rate after 1 reaction × 100%;

[0228] The reduction rate of methyl hexanoate selectivity = (selectivity of methyl hexanoate after 1 reaction - selectivity of methyl hexanoate after 5 reactions) / selectivity of methyl hexanoate after 1 reaction × 100%.

[0229] Table 4

[0230]

[0231]

[0232] As can be seen from the table above, compared with the catalytic reaction using DCAT-1 and DCAT-2, the molecular sieves CAT-1 to CAT-12 prepared in this disclosure can achieve higher conversion rates of nitrile compounds and higher selectivity of ester products in the hydrolysis and esterification reaction of nitrile compounds; and the catalyst exhibits better catalytic stability under repeated reaction conditions.

[0233] Further comparison between CAT-1 and CAT-9 reveals that CAT-1, when prepared by reacting with raw materials in the following proportions during molecular sieve preparation: "the molar ratio of silicon source: first template agent: water: silanizing agent is 1:(0.02~0.3):(5~30):(0.03~0.15); the weight ratio of SiO2 to structural filler in the reaction mixture is (5~30):1" and "the weight ratio of molecular sieve intermediate, second template agent and water is 1:(0.1~1):(2~10)", yields CAT-1 molecular sieves with higher conversion rates of nitrile compounds and selectivity for ester products, and also exhibits better catalytic stability.

[0234] Further comparison of CAT-1 and CAT-12 shows that the molecular sieve CAT-1 prepared in Example 1 according to the preferred process conditions of this disclosure can achieve higher conversion rates of nitrile compounds and selectivity of ester products, as well as better catalyst reaction stability.

[0235] Comparative Example 1

[0236] This comparative reaction uses the method disclosed in existing technology CN101172253A to synthesize ester compounds, specifically including:

[0237] (1) 1 mol of 1-methylimidazolium was placed in a three-necked round-bottom flask, and tetrafluoroboric acid (40 wt%) was added in an equimolar ratio while stirring. The reaction temperature was controlled not to exceed 40 °C, and stirring was continued for 1 h to obtain a pale yellow liquid. Excess water was removed by vacuum distillation at 70 °C to obtain the ionic liquid 1-methylimidazolium tetrafluoroborate [Hmim]. + BF4 - .

[0238] (2) Mix 0.015 mol FeCl3 with 0.06 mol of ionic liquid [Hmim] + BF4 -After thorough mixing, the mixture was added to a 500 mL three-necked flask along with 1 mol of hexanoic acid and 1 mol of methanol. A water separator and temperature sensor were installed, and a reflux condenser was attached to the water separator. The mixture was heated while stirring until the reactants boiled and the reaction began (reaction temperature 92–105 °C). The azeotrope formed during the reaction was distilled off from the three-necked flask, condensed in the reflux condenser, and then returned to the water separator. The water in the azeotrope was separated from the organic phase, and the water was discharged from the water separator. The organic phase was returned to the three-necked flask to continue the reaction. After almost no water was released from the reflux, the ester product methyl hexanoate and the unreacted raw materials were distilled off. The conversion rate of hexanoic acid was determined to be 74 mol%, and the selectivity of methyl hexanoate was 85 mol%.

[0239] Comparing reaction Comparative Example 1 with reaction Example 1, it can be seen that the heterogeneous reaction method provided by this disclosure is simple to operate, and the catalyst is easy to separate, recover and reuse; moreover, the method provided by this disclosure does not use toxic and harmful solvents, making it more green and environmentally friendly.

[0240] Reaction Examples 2-3

[0241] The same reaction apparatus as in Reaction Example 1 was used, except that the reaction conditions were changed and the catalytic reaction was carried out according to the reaction conditions listed in Table 5 below. The reaction results are listed in Table 6.

[0242] Table 5

[0243]

[0244] Table 6

[0245]

[0246] As can be seen from Tables 5 and 6 above:

[0247] In reaction example 2, acrylonitrile was used as the reaction raw material and ethanol as the solvent. High conversion rate of nitrile compounds and selectivity of ester products were obtained in the hydrolysis and esterification reaction of nitrile compounds, indicating that the method provided in this disclosure has wide applicability to different types of nitrile compounds.

[0248] Comparing Reaction Example 3 with Reaction Example 1, it can be seen that when CAT-1 is used as the catalyst, Reaction Example 1 follows the following conditions: the molar ratio of nitrile compound to solvent is 1:(5-50); the reaction temperature is 350-400℃; the reaction time is 10-24h; the reaction pressure is 0.1-2MPa; and the weight hourly space velocity of the nitrile compound is 0.2-10h. -1 "The reaction was carried out under the reaction conditions, and the conversion rate of nitrile compounds and the selectivity of ester products obtained in Reaction Example 1 were higher."

[0249] The preferred embodiments of this disclosure have been described in detail above. However, this disclosure is not limited to the specific details of the above embodiments. Within the scope of the technical concept of this disclosure, various simple modifications can be made to the technical solutions of this disclosure, and these simple modifications all fall within the protection scope of this disclosure.

[0250] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, this disclosure will not describe the various possible combinations separately.

[0251] Furthermore, various different embodiments of this disclosure can be combined in any way, as long as they do not violate the spirit of this disclosure, they should also be regarded as the content disclosed in this disclosure.

Claims

1. A method for esterification of nitrile hydrolysis, characterized in that, Includes the following steps: A cyano hydrolysis esterification reaction is carried out by contacting nitriles with a catalyst; The catalyst is a hierarchical porous Silicalite-1 molecular sieve, which has multiple cavity structures within its crystals. The hierarchical porous Silicalite-1 molecular sieve has the following characteristics: 31 P MAS NMR characteristics: The peak intensity of the characteristic peak at a chemical shift of -5±1ppm for the hierarchical porous Silicalite-1 molecular sieve is denoted as N1; the peak intensity of the characteristic peak at a chemical shift of -34±1ppm for the hierarchical porous Silicalite-1 molecular sieve is denoted as N2; and the peak intensity of the characteristic peak at a chemical shift of -61±1ppm for the hierarchical porous Silicalite-1 molecular sieve is denoted as N3. As defined in equation (1), X1 can be any value between 0.10 and 0.30; X1 = N1 / N3 (1); and As defined in equation (2), X2 is any value between 0.15 and 0.45; X2=N2 / N3 (2); The hierarchical porous Silicalite-1 molecular sieve has the following characteristics: 29 Si MAS NMR characteristics: The peak area of ​​the chemical shift peak of the hierarchical porous Silicalite-1 molecular sieve in the range of -102 to -104 ppm is denoted as Q. 3 The peak area of ​​the spectral peak with a chemical shift in the range of -112 to -114 ppm is denoted as Q. 4 As defined in the following formula (3), X3 is any value between 2% and 30%: X3=Q 3 / Q 4 ×100% Equation (3).

2. The method according to claim 1, characterized in that, The nitrile compounds are selected from one or more of hydrocarbon nitrile compounds and aryl nitrile compounds and their derivatives.

3. The method according to claim 2, characterized in that, In the hydrocarbon nitrile compounds, the hydrocarbon group is selected from one or more of alkyl groups having 2 to 10 carbon atoms and alkenyl groups having 3 to 10 carbon atoms; in the aryl nitrile compounds and their derivatives, the aryl group is selected from one or more of aryl groups having 6 to 12 carbon atoms and heteroaryl groups having 5 to 15 carbon atoms.

4. The method according to claim 3, characterized in that, The hydrocarbon nitrile compounds are selected from one or more of acetonitrile, propionitrile, butyronitrile, valerate, hexanonitrile, heptanonitrile, octanonitrile, nonanonitrile, decanonitrile, acrylonitrile, butenonitrile, and hexenonitrile; the aryl nitrile compounds and their derivatives are selected from one or more of phthalonitrile, 4-cyanopyridine, cyclohexanenitrile, and 2-(3-methoxyphenyl)-2-methylpropionitrile.

5. The method according to claim 1, characterized in that, The method further includes: contacting a nitrile compound with a catalyst in the presence of a solvent to carry out the cyano hydrolysis esterification reaction.

6. The method according to claim 5, characterized in that, The solvent is selected from one or more of methanol, ethanol, propanol, butanol and hexanol.

7. The method according to claim 5, characterized in that, The molar ratio of the nitrile compound to the solvent is 1:(3~100).

8. The method according to claim 7, characterized in that, The molar ratio of the nitrile compound to the solvent is 1:(5~50).

9. The method according to claim 1, characterized in that, The conditions for the cyano hydrolysis esterification reaction include: a reaction temperature of 200–450 °C; a reaction time of 1–72 h; a reaction pressure of 0.1–3 MPa; and a weight hourly space velocity (WHSV) of 0.1–15 h⁻¹ for the nitrile compound. -1 .

10. The method according to claim 9, characterized in that, The conditions for the cyano hydrolysis esterification reaction include: a reaction temperature of 350–400 °C; a reaction time of 10–24 h; a reaction pressure of 0.1–2 MPa; and a weight hourly space velocity (WHSV) of 0.2–10 h⁻¹ for the nitrile compound. -1 .

11. The method according to claim 10, characterized in that, The reactor for the cyano hydrolysis esterification reaction is selected from any one of a fixed bed reactor, a batch reactor, a moving bed reactor, a suspended bed reactor, or a slurry bed reactor.

12. The method according to claim 1, characterized in that, In the hierarchical porous Silicalite-1 molecular sieve, the size of a single cavity structure is 5~150 nm.

13. The method according to claim 12, characterized in that, In the hierarchical porous Silicalite-1 molecular sieve, the size of a single cavity structure is 10~100nm.

14. The method according to claim 1, characterized in that, The volume of all the cavity structures accounts for 10-95% of the total volume of the molecular sieve.

15. The method according to claim 14, characterized in that, The volume of all the cavity structures accounts for 15-90% of the total volume of the molecular sieve.

16. The method according to claim 1, characterized in that, The shape of the cavity structure is selected from one or more of the following: sphere, cube, ellipsoid, and irregular cube.

17. The method according to claim 1, characterized in that, X1 is any value between 0.15 and 0.25; X2 is any value between 0.20 and 0.

35.

18. The method according to claim 1, characterized in that, X3 is any value between 5% and 25%.

19. The method according to claim 1, characterized in that, The hierarchical porous Silicalite-1 molecular sieve has the following characteristics: 1 HMAS NMR characteristics: The hierarchical porous Silicalite-1 molecular sieve 1 In the peak separation results of the 1~6 ppm chemical shift range of the H MAS NMR spectrum: the peak area of ​​the peak in the 1.6~1.8 ppm chemical shift range is recorded as A1, the peak area of ​​the peak in the 2.0~2.2 ppm chemical shift range is recorded as A2, the peak area of ​​the peak in the 3.1~3.3 ppm chemical shift range is recorded as A3, the peak area of ​​the peak in the 4.4~4.6 ppm chemical shift range is recorded as A4, and the sum of the peak areas of A1~A4 is recorded as A0. X is defined as follows (4-1) 4-1 Any value between 14% and 32% X 4-1 =A1 / A0×100% (4-1); X is defined as follows (4-2) 4-2 Any value between 23% and 41% X 4-2 =A2 / A0×100% (4-2); X is defined as follows (4-3) 4-3 Any value between 16% and 35% X 4-3 =A3 / A0×100% (4-3); X is defined as follows (4-4) 4-4 Any value between 4% and 20% X 4-4 =A4 / A0×100% (4-4).

20. The method according to claim 1, characterized in that, The multi-level porous Silicalite-1 molecular sieve includes molecular sieve particles composed of single crystals and / or molecular sieve particles composed of aggregates of multiple crystals.

21. The method according to claim 1, characterized in that, The molecular sieve particles have an average particle size of 0.1~2μm and a BET specific surface area of ​​300~650m². 2 / g; Microporous specific surface area is 200~550m² 2 / g; total pore volume is 0.2~0.7cm³. 3 / g; mesopore volume is 0.1~0.5cm³ 3 / g.

22. The method according to claim 1, characterized in that, The molecular sieve particles have an average particle size of 0.2~1.2μm and a BET specific surface area of ​​350~550m². 2 / g; Microporous specific surface area is 250~450m² 2 / g; total pore volume is 0.3~0.5cm³. 3 / g; mesopore volume is 0.2~0.4cm³ 3 / g.

23. The method according to claim 1, characterized in that, There is a hysteresis loop between the adsorption isotherm and desorption isotherm of the hierarchical porous Silicalite-1 molecular sieve at low temperature nitrogen adsorption.

24. The method according to claim 1, characterized in that, The hierarchical porous Silicalite-1 molecular sieve is prepared by a method including the following steps: S1. Mix the silicon source, the first template agent, water, the silanizing agent and the structural filler to obtain a reaction mixture, wherein the structural filler is an amphiphilic surfactant and / or a hard template agent; S2. The reaction mixture is subjected to a first hydrothermal crystallization treatment and a first calcination treatment in sequence to obtain a molecular sieve intermediate; S3. Mix the molecular sieve intermediate, the second template agent and water, and then perform a second hydrothermal crystallization treatment and a second calcination treatment in sequence.

25. The method according to claim 24, characterized in that, In step S1, the molar ratio of silicon source: first template agent: water: silanizing agent is 1:(0.01~2):(1~50):(0.02~0.2); the weight ratio of SiO2 to structural filler in the reaction mixture is (5~40):

1.

26. The method according to claim 25, characterized in that, In step S1, the molar ratio of silicon source: first template agent: water: silanizing agent is 1:(0.02~0.3):(5~30):(0.03~0.15).

27. The method according to claim 25, characterized in that, The weight ratio of SiO2 to structural filler in the reaction mixture is (5~30):

1.

28. The method according to claim 24, characterized in that, In step S1, the silicon source is selected from at least one of organosilicon grease, solid silica gel, fumed silica, and silica sol.

29. The method according to claim 28, characterized in that, In step S1, the silicon source is selected from at least one of silicone grease, solid silicone and silica.

30. The method according to claim 29, characterized in that, The silicon source is an organosilicone grease, and the organosilicone grease has the general formula shown in formula (A): (A); Where R a R b R c R d Each is independently selected from alkyl groups having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight-chain alkyl group.

31. The method according to claim 30, characterized in that, R a R b R c R d Each is independently selected from straight-chain alkyl groups having 1 to 4 carbon atoms or branched alkyl groups having 3 to 4 carbon atoms.

32. The method according to claim 31, characterized in that, The R a R b R c R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, or tert-butyl.

33. The method according to claim 30, characterized in that, The silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate, and dimethyl diethyl silicone grease.

34. The method according to claim 24, characterized in that, The first template agent in step S1 and the second template agent in step S3 are organic bases.

35. The method according to claim 34, characterized in that, The first template agent in step S1 and the second template agent in step S3 are each independently selected from at least one of quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines.

36. The method according to claim 35, characterized in that, The first and second template agents are each independently selected from at least one of quaternary ammonium bases having the structure shown in formula (B): (B); R1, R2, R3 and R4 are each selected from alkyl groups having 1 to 4 carbon atoms.

37. The method according to claim 36, characterized in that, R1, R2, R3 and R4 are straight-chain alkyl groups having 1 to 4 carbon atoms and branched alkyl groups having 3 to 4 carbon atoms.

38. The method according to claim 37, characterized in that, R1, R2, R3 and R4 are each selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.

39. The method according to claim 36, characterized in that, The first template agent and the second template agent are each independently tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide.

40. The method according to claim 24, characterized in that, In step S1, the silanizing agent has the general formula R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, alkyl, alkoxy, aromatic, mercapto, or amino group, and at least one of R5, R6, R7, and R8 is an alkyl, alkoxy, aromatic, mercapto, or amino group; the alkyl, alkoxy, mercapto, and amino groups each have an independent number of carbon atoms of C1 to C2. 18 .

41. The method according to claim 40, characterized in that, The silanizing agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane.

42. The method according to claim 41, characterized in that, The silanizing agent is selected from one or more of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane.

43. The method according to claim 24, characterized in that, In step S1, the structural filler is selected from one or more of hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, PEO-PPO-PEO triblock copolymer, mesoporous carbon, and natural cellulose.

44. The method according to claim 24, characterized in that, Step S1 includes: a. Mix the silicon source, the first template agent, and water to obtain a silicon hydrolysis sol; b. The silanizing agent and the structural filler are added to the hydrolyzed sol of the silicon, and the mixture is then used to obtain the reaction mixture.

45. The method according to claim 44, characterized in that, The mixing conditions in step a include stirring at 40~90℃ for 6~12 hours.

46. ​​The method according to claim 44, characterized in that, The mixing conditions in step b include stirring at 20~50℃ for 2~4 hours.

47. The method according to claim 44, characterized in that, The silicon source is an organosilicon grease. In step a, after mixing the silicon source, the first template agent and water, a hydrolysis and alcohol removal treatment is also included to obtain the silicon hydrolysate.

48. The method according to claim 47, characterized in that, The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 40~90℃ for 6~12h.

49. The method according to claim 48, characterized in that, The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 60~85℃ for 8~10h.

50. The method according to claim 24, characterized in that, In step S3, the weight ratio of the molecular sieve intermediate, the second template agent, and water is 1:(0.01~1.5):(1~15).

51. The method according to claim 50, characterized in that, In step S3, the weight ratio of the molecular sieve intermediate, the second template agent, and water is 1:(0.1~1):(2~10).

52. The method according to claim 24, characterized in that, The conditions for the first hydrothermal crystallization treatment in step S2 and the second hydrothermal crystallization treatment in step S3 each independently include: a hydrothermal crystallization time of 0.25 to 7 days and a hydrothermal crystallization temperature of 130 to 200°C.

53. The method according to claim 52, characterized in that, The hydrothermal crystallization time is 1-3 days, the hydrothermal crystallization temperature is 150-180℃, and the pressure is autogenous pressure; The conditions for the first roasting treatment in step S2 and the second roasting treatment in step S3 each independently include: a roasting temperature of 300~700℃ and a roasting time of 1~16h.

54. The method according to claim 53, characterized in that, The conditions for the first roasting treatment in step S2 and the second roasting treatment in step S3 each independently include: a roasting temperature of 400~600℃ and a roasting time of 2~5h.

Citation Information

Patent Citations

  • Esterification catalysts and esterification process of organic acid

    CN101172253A

  • Method for converting nitrile compounds into corresponding carboxylic acids and esters

    CN101641318A

  • Silicon molecular sieve and its synthesizing process

    CN1338427A