By introducing reduced graphene oxide-supported silica and acidified conductive carbon black-cobalt copper hybrid into polyurethane foam to form a conductive network, the antistatic and high-temperature resistance problems of polyurethane foam are solved, the stability and safety of the material are improved, and its application range is expanded.
Patent Information
- Application Number
- CN202311726737.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-15
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-15
AI Technical Summary
Existing polyurethane foam materials have shortcomings in terms of antistatic properties and high temperature resistance. Traditional methods result in poor material stability, strong odor, unstable raw material storage, and the isocyanates used are highly toxic, which limits their application range.
Reduced graphene oxide supported on silica (RGO@SiO₂) is used as a high-temperature resistant filler and combined with acidified conductive carbon black-cobalt copper hybrid (oCB-Co-Cu) to form a conductive network, which enhances the high-temperature resistance and antistatic properties of polyurethane foam.
It improves the high temperature resistance and antistatic stability of polyurethane foam, reduces surface resistance, and is a safe and non-toxic material that combines the excellent properties of traditional polyurethane foam, thus broadening its application range.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of organic polymer synthesis technology, and relates to a method for preparing polyurethane polymer materials. Specifically, this relates to a high-temperature resistant and antistatic polyurethane foam material and its preparation method. Background Technology
[0002] Foamed plastics possess characteristics such as lightweight, heat insulation, sound absorption, and shock absorption, and have a wide range of applications in daily production and life. For example, polyurethane (PU) foam, the earliest developed and applied material, is widely used in refrigeration, decoration, construction, packaging, and automotive industries due to its large production volume and mature technology. PU foam accounts for approximately 70% of PU products, with a wide variety of products and increasing production. The PU foaming process involves reacting isocyanates with polyols to produce polymers with repeating units of carbamate, forming a plastic foam material under the action of a foaming agent. In the mid-20th century, Germany first successfully developed PU foam. Later, the American company Wyandotte proposed using inexpensive petrochemical products, such as propylene oxide, to replace polyols, significantly reducing the production cost of PU foam. PU foam essentially inherits all the advantages of the matrix while also possessing the excellent properties of foamed plastics, namely relatively light weight, heat insulation, sound absorption, shock absorption, electrical insulation, high specific strength, and high flexibility. Furthermore, traditional polyurethane foam is a polymer material with poor electrical conductivity, typically with a surface resistivity of around 10 ohms. 12 ~10 15 The Ω range is prone to electrostatic effects, and the isocyanate mostly used in its preparation is TDI (toluene diisocyanate), which is highly toxic, greatly limiting its application range. Therefore, it is essential to develop antistatic, low-temperature resistant, safe, and non-toxic polyurethane foam.
[0003] Traditional methods to improve the antistatic properties of polyurethane foam include adding antistatic agents or physically impregnating conductive fillers. However, adding antistatic agents can lead to poor long-term antistatic performance because small molecules tend to precipitate out of the polymer matrix. While physical impregnation can effectively reduce the surface resistivity of polyurethane, its stability is poor. Both methods result in numerous problems such as excessive odor in the foam, poor storage stability of raw materials, and migration of antistatic agents. Summary of the Invention
[0004] The purpose of this invention is to provide a method for preparing polyurethane foam materials with high-temperature resistance and antistatic properties. First, reduced graphene oxide (RGO@SiO2) with surface-grown silica is prepared as a high-temperature resistant filler. Then, cobalt-copper hybrid modified acidified conductive carbon black (oCB-Co-Cu) is prepared as a conductive filler and added to the polyurethane foam system to obtain a high-temperature resistant and antistatic polyurethane foam. This significantly improves the high-temperature resistance, antistatic properties, and antistatic stability of the foam without altering its structure.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: A high-temperature resistant and antistatic polyurethane foam material is composed of the following raw materials in parts by weight: 40-60 parts of polyether polyol, 40-60 parts of polypropylene glycol, 0-20 parts of polymer polyol (where the total weight of polyether polyol, polypropylene glycol, and polymer polyol is 100 parts), 0.4-0.6 parts of amine catalyst, 0.4-0.6 parts of tin catalyst, 0.8-1.2 parts of surfactant, 0.4-0.5 parts of blowing agent, 0.4-0.6 parts of co-blowing agent, 1-5 parts of cell opener, 3-7 parts of high-temperature resistant filler, 3-7 parts of antistatic hybrid filler, and 70-90 parts of diphenylmethane diisocyanate (MDI).
[0006] The high-temperature resistant filler is reduced graphene oxide supported on silica (RGO@SiO2); the antistatic hybrid filler is oxidized conductive carbon black-cobalt copper oxide (oCB-Co-Cu); the polyether polyol is polyether polyol GLR-2000 produced by Shanghai Gaoqiao Petrochemical Co., Ltd.; the base polyether polyol is polypropylene glycol (PPG) with a molecular weight of 3000; the polymer polyol is polymer polyol (POP); the amine catalyst is triethylenediamine A-33 catalyst; the tin catalyst is tin isooctanoate T-9; the surfactant is L 6002; the pore-opening agent is pore-opening agent 1900h; the foaming agent is deionized water; and the diphenylmethane diisocyanate is MDI-8002.
[0007] The high-temperature resistant filler is reduced graphene oxide supported on silicon dioxide (RGO@SiO2). The preparation process is as follows: Graphene oxide is prepared using the modified Hummers method. 0.5g of the prepared graphene oxide is weighed and added to a 250mL beaker. 100mL of ethanol solution is added and ultrasonically dispersed for 1h. Then, 1mL of hydrazine hydrate, 4mL of ammonia, and 2mL of tetraethyl orthosilicate are weighed and stirred for half an hour. The mixture is then poured into a hydrothermal reactor and reacted at 180℃ for 12h. Afterward, RGO@SiO2 is obtained by vacuum filtration and freeze-drying.
[0008] The antistatic hybrid filler is oxidized conductive carbon black-cobalt copper oxide (oCB-Co-Cu). Its preparation process is as follows: (1) The preparation process of acidified conductive carbon black is as follows: Weigh 50 mL of mixed acid (35 mL of concentrated sulfuric acid + 15 mL of concentrated nitric acid) into a 100 mL beaker, add 2 g of conductive carbon black to the mixed acid and react for 5 h to obtain acidified conductive carbon black, and then dry it at 60 °C after centrifugation of diluted solution to obtain oCB.
[0009] (2) Preparation of antistatic hybrid filler oCB-Co-Cu: Weigh 2g oCB and add it to a 250mL beaker. Weigh 100mL of deionized water, and then weigh 5g of urea, 0.9g of CuCl2 and 3g of CoCl2·6H2O and add them to the solution. After stirring for 1h, add it to a hydrothermal reactor and react at 140℃ for 12h. After vacuum filtration and drying, OCB-Co-Cu is obtained.
[0010] This invention also provides a method for preparing high-temperature resistant and antistatic polyurethane foam, comprising the following steps: (1) Add polyether polyol, polypropylene glycol and polymer polyol to a container in proportion, and then add high temperature resistant filler, antistatic hybrid filler, amine catalyst, tin catalyst, surfactant, foaming agent, foaming agent and cell opening agent according to the formula. Stir for 2-3 minutes in a stirrer with a speed of 1500 r / min. This is recorded as component A. (2) Add diphenylmethane diisocyanate (MDI) to another container in proportion and stir for 10-30 s under a stirrer with a speed of 1000 r / min. This is called component B. (3) Increase the rotation speed of component A to 2500-3000 r / min, then pour component B into the container containing component A, stir for 10-15 s under high speed mixer, wait for the system to turn black and lighten, pour the system into the mold, control the mold temperature to 60±0.5 ℃, cut after 24-72 h to obtain the product.
[0011] The beneficial effects of this invention are as follows: With a rationally designed production formula and process, using non-toxic water as a foaming agent and relatively safe diphenylmethane diisocyanate to prepare polyurethane foam, it has health and environmental benefits while retaining the characteristics of traditional polyurethane foam.
[0012] When nano-silica is added to a polyurethane system as a standalone raw material, its bonding is weak. Adding too much to a polyurethane foam can cause foam collapse, while adding too little fails to achieve the desired high-temperature resistance and reinforcement. However, by growing silica on reduced graphene oxide (RGO), the high-temperature resistance of both RGO and SiO2 can be utilized simultaneously, and it can bond tightly with the polyurethane system, improving its high-temperature resistance. Furthermore, by acidifying the carbon black surface and then dispersing cobalt-copper hybrids within it, conductivity and heat resistance are further enhanced. Combined with reduced graphene oxide, a conductive network is formed, thus solving to some extent the problem of carbon black particle dispersion in the polymer matrix and addressing the challenges of high-temperature resistance, antistatic properties, and antistatic stability in polyurethane foam. Attached Figure Description
[0013] Figure 1 Infrared spectra of RGO and RGO@SiO2; Figure 2 XRD patterns of CB and CB-CoCu; Figure 3 The image shows the EDS energy dispersive spectroscopy (EDS) analysis of CB-CoCu. Figure 4 Add SEM images of RGO and CB-CoCu. Detailed Implementation
[0014] The present invention will be further described in detail below with reference to specific embodiments, but the present invention is not limited to the following specific embodiments.
[0015] Example 1 (3 parts high-temperature resistant filler, 7 parts antistatic filler) Preparation of high-temperature resistant filler RGO@SiO2: Graphene oxide was prepared using a modified Hummers method. 0.5 g of the prepared graphene oxide was weighed and added to a 250 mL beaker. 100 mL of ethanol solution was added and ultrasonically dispersed for 1 h. Then, 1 mL of hydrazine hydrate, 4 mL of ammonia, and 2 mL of tetraethyl orthosilicate were weighed and stirred for half an hour. The mixture was then poured into a hydrothermal reactor and reacted at 180 °C for 12 h. After that, it was vacuum filtered and freeze-dried to obtain RGO@SiO2.
[0016] Preparation of antistatic hybrid filler oCB-Co-Cu: (1) The preparation process of acidified conductive carbon black is as follows: Weigh 50 mL of mixed acid (35 mL concentrated sulfuric acid + 15 mL concentrated nitric acid) into a 100 mL beaker, add 2 g of conductive carbon black to the mixed acid and react for 5 h to obtain acidified conductive carbon black. After diluting the solution and centrifuging, dry at 60 °C to obtain oCB.
[0017] (2) Preparation of antistatic hybrid filler oCB-Co-Cu: Weigh 2g of oCB and add it to a 250mL beaker. Weigh 100mL of deionized water, and then weigh 5g of urea, 0.9g of CuCl2, and 3g of CoCl2·6H2O and add them to the solution. After stirring for 1h, add the solution to a hydrothermal reactor and react at 140℃ for 12h. After vacuum filtration and drying, oCB-Co-Cu is obtained.
[0018] Preparation of high-temperature resistant and antistatic polyurethane foam: Weigh the following raw materials in parts by weight: 40 parts of polyether polyol, 40 parts of polypropylene glycol, 20 parts of polymer polyol (of which the total weight of polyether polyol, polypropylene glycol, and polymer polyol is 100 parts), 0.4 parts of amine catalyst, 0.4 parts of tin catalyst, 0.8 parts of surfactant, 0.4 parts of water, 0.4 parts of dichloromethane, 2 parts of pore-opening agent, 3 parts of high-temperature resistant filler, 7 parts of antistatic hybrid filler, and 70 parts of diphenylmethane diisocyanate (MDI).
[0019] Add polyether polyol, polypropylene glycol, and polymer polyol to a container in proportion, and then add high-temperature resistant filler, antistatic filler, amine catalyst, tin catalyst, surfactant, foaming agent, co-foaming agent, and cell opener according to the formula. Stir for 2-3 minutes in a mixer at 1500 r / min. This is recorded as component A. 70 parts of diphenylmethane diisocyanate (MDI) were added to another container, denoted as component B; Increase the rotation speed of component A to 2500-3000 r / min, then pour component B into the container containing component A. Mix under high speed for 10-15 seconds until the system turns white. Pour the system into a mold and control the mold temperature at 60±0.5℃. Cut after 24-72 hours to obtain the product.
[0020] Example 2 (5 parts high-temperature resistant filler and 5 parts antistatic filler) (1) Preparation of high-temperature resistant filler RGO@SiO2: Same as in Example 1, (2) Preparation of antistatic hybrid filler oCB-Co-Cu: Same as in Example 1, (3) Preparation of high-temperature resistant and antistatic polyurethane foam: Weigh the following raw materials in parts by weight: 40 parts of polyether polyol, 40 parts of polypropylene glycol, 20 parts of polymer polyol (of which the total weight of polyether polyol, polypropylene glycol, and polymer polyol is 100 parts), 0.4 parts of amine catalyst, 0.4 parts of tin catalyst, 0.8 parts of surfactant, 0.4 parts of water, 0.4 parts of dichloromethane, 2 parts of pore-opening agent, 3 parts of high-temperature resistant filler, 7 parts of antistatic hybrid filler, and 70 parts of diphenylmethane diisocyanate (MDI).
[0021] Add polyether polyol, polypropylene glycol, and polymer polyol to a container in proportion, and then add high-temperature resistant filler, antistatic filler, amine catalyst, tin catalyst, surfactant, foaming agent, co-foaming agent, and cell opener according to the formula. Stir for 2-3 minutes in a mixer at 1500 r / min. This is recorded as component A. 70 parts of diphenylmethane diisocyanate (MDI) were added to another container, denoted as component B; Increase the rotation speed of component A to 2500-3000 r / min, then pour component B into the container containing component A. Mix under high speed for 10-15 seconds until the system turns white. Pour the system into a mold and control the mold temperature at 60±0.5℃. Cut after 24-72 hours to obtain the product.
[0022] Example 3 (7 parts high-temperature resistant filler and 3 parts antistatic filler) (1) Preparation of high-temperature resistant filler RGO@SiO2: Same as in Example 1, (2) Preparation of antistatic hybrid filler oCB-Co-Cu: Same as in Example 1, (3) Preparation of high-temperature resistant and antistatic polyurethane foam: Weigh the following parts by weight of raw materials: 40 parts of polyether polyol, 40 parts of polypropylene glycol, 20 parts of polymer polyol (of which the total weight of polyether polyol, polypropylene glycol, and polymer polyol is 100 parts), 0.4 parts of amine catalyst, 0.4 parts of tin catalyst, 0.8 parts of surfactant, 0.4 parts of water, 0.4 parts of dichloromethane, 2 parts of pore-opening agent, 3 parts of high-temperature resistant filler, 7 parts of antistatic hybrid filler, and 70 parts of diphenylmethane diisocyanate (MDI).
[0023] Add polyether polyol, polypropylene glycol, and polymer polyol to a container in proportion, and then add high-temperature resistant filler, antistatic filler, amine catalyst, tin catalyst, surfactant, foaming agent, co-foaming agent, and cell opener according to the formula. Stir for 2-3 minutes in a mixer at 1500 r / min. This is recorded as component A. Add 70 parts of diphenylmethane diisocyanate (MDI) to another container, denoted as component B; Increase the rotation speed of component A to 2500-3000 r / min, then pour component B into the container containing component A. Mix under high speed for 10-15 seconds until the system turns white. Pour the system into a mold and control the mold temperature at 60±0.5℃. Cut after 24-72 hours to obtain the product.
[0024] Comparative Example 1 (no high-temperature resistant filler, no antistatic hybrid filler) Preparation of polyurethane foam: Weigh the following raw materials in parts by weight: 40 parts of polyether polyol, 40 parts of polypropylene glycol, 20 parts of polymer polyol (of which the total weight of polyether polyol, polypropylene glycol, and polymer polyol is 100 parts), 0.4 parts of amine catalyst, 0.4 parts of tin catalyst, 0.8 parts of surfactant, 0.4 parts of water, 0.4 parts of dichloromethane, 2 parts of pore-opening agent, and 70 parts of diphenylmethane diisocyanate (MDI).
[0025] Add polyether polyol, polypropylene glycol, and polymer polyol to a container in proportion, then add amine catalyst, tin catalyst, surfactant, foaming agent, co-foaming agent, and cell opener according to the formula. Stir for 2-3 minutes in a mixer at 1500 r / min. This is recorded as component A. Add 70 parts of diphenylmethane diisocyanate (MDI) to another container, denoted as component B; Increase the rotation speed of component A to 2500-3000 r / min, then pour component B into the container containing component A. Mix under high speed for 10-15 seconds until the system turns white. Pour the system into a mold and control the mold temperature at 60±0.5℃. Cut after 24-72 hours to obtain the product.
[0026] Comparative Example 2 (Conductive carbon black only) Preparation of polyurethane foam: Weigh the following raw materials in parts by weight: 40 parts of polyether polyol, 40 parts of polypropylene glycol, 20 parts of polymer polyol (of which the total weight of polyether polyol, polypropylene glycol, and polymer polyol is 100 parts), 0.4 parts of amine catalyst, 0.4 parts of tin catalyst, 0.8 parts of surfactant, 0.4 parts of water, 0.4 parts of dichloromethane, 2 parts of pore-opening agent, 10 parts of conductive carbon black, and 70 parts of diphenylmethane diisocyanate (MDI).
[0027] Add polyether polyol, polypropylene glycol, and polymer polyol to a container in proportion, then add amine catalyst, tin catalyst, surfactant, foaming agent, co-foaming agent, and cell opener according to the formula. Stir for 2-3 minutes in a mixer at 1500 r / min. This is recorded as component A. Add 70 parts of diphenylmethane diisocyanate (MDI) to another container, denoted as component B; Increase the rotation speed of component A to 2500-3000 r / min, then pour component B into the container containing component A. Mix under high speed for 10-15 seconds until the system turns white. Pour the system into a mold and control the mold temperature at 60±0.5℃. Cut after 24-72 hours to obtain the product.
[0028] Comparative Example 3 (graphene oxide only) Preparation of polyurethane foam: Weigh the following raw materials in parts by weight: 40 parts of polyether polyol, 40 parts of polypropylene glycol, 20 parts of polymer polyol (of which the total weight of polyether polyol, polypropylene glycol, and polymer polyol is 100 parts), 0.4 parts of amine catalyst, 0.4 parts of tin catalyst, 0.8 parts of surfactant, 0.4 parts of water, 0.4 parts of dichloromethane, 2 parts of pore-opening agent, 10 parts of graphene oxide, and 70 parts of diphenylmethane diisocyanate (MDI).
[0029] Add polyether polyol, polypropylene glycol, and polymer polyol to a container in proportion, then add amine catalyst, tin catalyst, surfactant, foaming agent, co-foaming agent, and cell opener according to the formula. Stir for 2-3 minutes in a mixer at 1500 r / min. This is recorded as component A. Add 70 parts of diphenylmethane diisocyanate (MDI) to another container, denoted as component B; Increase the rotation speed of component A to 2500-3000 r / min, then pour component B into the container containing component A. Mix under high speed for 10-15 seconds until the system turns white. Pour the system into a mold and control the mold temperature at 60±0.5℃. Cut after 24-72 hours to obtain the product.
[0030] Comparative Example 4 (High-Temperature Resistant Filler Only) Preparation of high-temperature resistant filler: Same as in Example 1.
[0031] Preparation of polyurethane foam: Weigh the following raw materials in parts by weight: 40 parts of polyether polyol, 40 parts of polypropylene glycol, 20 parts of polymer polyol (of which the total weight of polyether polyol, polypropylene glycol, and polymer polyol is 100 parts), 0.4 parts of amine catalyst, 0.4 parts of tin catalyst, 0.8 parts of surfactant, 0.4 parts of water, 0.4 parts of dichloromethane, 2 parts of pore-opening agent, 10 parts of high-temperature resistant filler, and 70 parts of diphenylmethane diisocyanate (MDI).
[0032] Add polyether polyol, polypropylene glycol, and polymer polyol to a container in proportion, then add amine catalyst, tin catalyst, surfactant, foaming agent, co-foaming agent, and cell opener according to the formula. Stir for 2-3 minutes in a mixer at 1500 r / min. This is recorded as component A. Add 70 parts of diphenylmethane diisocyanate (MDI) to another container, denoted as component B; Increase the rotation speed of component A to 2500-3000 r / min, then pour component B into the container containing component A. Mix under high speed for 10-15 seconds until the system turns white. Pour the system into a mold and control the mold temperature at 60±0.5℃. Cut after 24-72 hours to obtain the product.
[0033] Comparative Example 5 (Antistatic filler only) Preparation of antistatic hybrid filler: Same as in Example 1.
[0034] 40 parts of polyether polyol, 40 parts of polypropylene glycol, 20 parts of polymer polyol (of which the total weight of polyether polyol, polypropylene glycol, and polymer polyol is 100 parts), 0.4 parts of amine catalyst, 0.4 parts of tin catalyst, 0.8 parts of surfactant, 0.4 parts of water, 0.4 parts of dichloromethane, 2 parts of pore-opening agent, 10 parts of antistatic hybrid filler, and 70 parts of diphenylmethane diisocyanate (MDI).
[0035] Add polyether polyol, polypropylene glycol, and polymer polyol to a container in proportion, then add amine catalyst, tin catalyst, surfactant, foaming agent, co-foaming agent, and cell opener according to the formula. Stir for 2-3 minutes in a mixer at 1500 r / min. This is recorded as component A. Add 70 parts of diphenylmethane diisocyanate (MDI) to another container, denoted as component B; Increase the rotation speed of component A to 2500-3000 r / min, then pour component B into the container containing component A. Mix under high speed for 10-15 seconds until the system turns white. Pour the system into a mold and control the mold temperature at 60±0.5℃. Cut after 24-72 hours to obtain the product.
[0036] Performance testing The sponges obtained in Examples 1-3 and Comparative Examples 1-5 were cut into different sizes. According to the requirements of national standards GB / T 6344-2008 "Determination of Tensile Strength and Elongation at Break of Flexible Foam Polymer Materials", GB / T 10807-2006 "Determination of Hardness of Flexible Foam Polymer Materials (Indentation Method)", and GB / T 9640-2008 "Accelerated Aging Test Method for Flexible and Rigid Foam Polymer Materials", the foam density and tear strength of the sponge products were tested. The tensile strength, elongation at break, compression set, antistatic properties, and the rate of change of these three properties after heat storage (170 ℃, 24 h) were also tested. The test results of the obtained sponges are shown in Table 1.
[0037] Table 1 shows that the high-temperature resistant and antistatic polyurethane foam materials described in this invention (Examples 1-3) not only exhibit a physical and mechanical property change rate of no more than 5% after being treated at 170℃ for 140 hours, demonstrating a significant improvement in high-temperature resistance compared to the foams in Comparative Examples 1-3; but also, according to high-resistivity meter tests, their surface resistance is greatly reduced, reaching antistatic levels, and remains essentially unchanged after 30 days; furthermore, the mechanical properties are also improved through comparison. Using the single-variable method, Comparative Examples 4 and 5 show that adding only the antistatic hybrid filler and the high-temperature resistant filler does not result in better antistatic performance than adding them together. However, when both are added simultaneously, the surface resistance decreases directly, proving that their synergistic effect forms a dense conductive network within the polyurethane foam system. Comparative Examples 2 and 3 show that the unmodified filler has little impact on the foam, and its performance improvement effect is average. Therefore, in summary, the high-temperature resistant filler prepared by growing SiO2 on the RGO surface can be tightly bonded to the foam to improve its thermodynamic properties. CN-CoCu, which forms a cobalt-copper hybrid filler with acidified CB, can further improve the conductivity of CB. When added to the foam system, it works synergistically with RGO-SiO2 to not only improve the high-temperature resistance, but also improve the antistatic properties and antistatic stability.
[0038] Depend on Figure 1 The infrared spectrum shows that, due to the presence of SiO2, the antistatic hybrid material exhibits high activity at 467 cm⁻¹. −1 580cm −1 796 cm −1 and 1093cm −1 The appearance of a peak nearby indicates that SiO2 has been successfully grown on the RGO surface. Figure 2XRD analysis shows that the diffraction peaks of the CoCu hybrid material are located at 16.5°, 24.42°, and 32.73°, as shown in the figure, corresponding to the characteristic diffraction peaks of the (003), (006), and (009) crystal planes, respectively. This indicates that the CB-CuCo hybrid material was successfully prepared. Figure 3 The images show the scanning electron microscope (SEM) image and EDS spectrum of CB-CoCu. As can be seen from the images, the metal ions in the hybrid material are evenly distributed and have good bonding with the hybrid material formed by CB, thereby further enhancing the antistatic properties. Figure 4 The scanning electron microscope (SEM) images show that there are many pores, thin pore walls, high porosity, and a uniform and dense pore structure with a pore size of approximately 200 μm. As shown in Table 1, the RGO-SiO2, which is tightly bonded to the polyurethane matrix at high temperatures, along with carbon black and metal particles, all contribute to enhancing structural stability, resulting in the CB-CuCo hybrid material.
[0039] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention should be included in the scope of the present invention.
Claims
1. A high-temperature resistant and antistatic polyurethane foam material, characterized in that: The raw materials, by weight parts, are: 40-60 parts polyether polyol, 40-60 parts polypropylene glycol, 0-20 parts polymer polyol, 0.4-0.6 parts amine catalyst, 0.4-0.6 parts tin catalyst, 0.8-1.2 parts surfactant, 0.4-0.5 parts foaming agent, 0.4-0.6 parts co-foaming agent, 1-5 parts cell opener, 3-7 parts high-temperature resistant filler, 3-7 parts antistatic hybrid filler, and 70-90 parts diphenylmethane diisocyanate; wherein the total weight parts of polyether polyol, polypropylene glycol, and polymer polyol are 100 parts. The high-temperature resistant filler is reduced graphene oxide supported on silicon dioxide (RGO@SiO2), and its preparation process is as follows: graphene oxide is prepared using a modified Hummers method; 0.5 g of the prepared graphene oxide is added to 100 mL of ethanol, ultrasonically dispersed for 1 h, 1 mL of hydrazine hydrate, 4 mL of ammonia and 2 mL of tetraethyl orthosilicate are added, stirred for 0.5 h, hydrothermally reacted at 180 °C for 12 h, vacuum filtered, and freeze-dried to obtain RGO@SiO2; The antistatic hybrid filler is oxidized conductive carbon black-cobalt copper (oCB-Co-Cu), and its preparation process is as follows: (1) Preparation of acidified conductive carbon black: Mix 35 mL of concentrated sulfuric acid and 15 mL of concentrated nitric acid, add 2 g of conductive carbon black, react for 5 h, centrifuge, and dry at 60 °C to obtain oCB; (2) Preparation of oCB-Co-Cu: Add 2g oCB, 5g urea, 0.9g CuCl2 and 3g CoCl2·6H2O to 100mL of deionized water, stir for 1h, hydrothermally react at 140℃ for 12h, filter under vacuum, and dry to obtain oCB-Co-Cu; The polyether polyol is GLR-2000; the polypropylene glycol has a molecular weight of 3000.
2. The high-temperature resistant and antistatic polyurethane foam material according to claim 1, characterized in that: The polymer polyol is POP.
3. The high-temperature resistant and antistatic polyurethane foam material according to claim 1, characterized in that: The amine catalyst is triethylenediamine A-33; the tin catalyst is tin isooctanoate T-9.
4. The high-temperature resistant and antistatic polyurethane foam material according to claim 1, characterized in that: The surfactant is L-6002; the pore-opening agent is pore-opening agent 1900h; and the foaming agent is deionized water.
5. The high-temperature resistant and antistatic polyurethane foam material according to claim 1, characterized in that: The diphenylmethane diisocyanate mentioned is MDI-8002.
6. A method for preparing the high-temperature resistant and antistatic polyurethane foam material as described in any one of claims 1-5, characterized in that: Polyether polyol, polypropylene glycol, and polymer polyol are mixed evenly. Then, high-temperature resistant filler, antistatic hybrid filler, amine catalyst, tin catalyst, surfactant, foaming agent, co-foaming agent, and cell opener are added in sequence and stirred evenly. Diphenylmethane diisocyanate is then added and stirred at high speed. The mixture is poured into a mold and, after complete curing, demolded and cut to obtain the high-temperature resistant and antistatic polyurethane foam material.
7. The method according to claim 6, characterized in that: Includes the following steps: (1) Mix polyether polyol, polypropylene glycol and polymer polyol, add high temperature resistant filler, antistatic hybrid filler, amine catalyst, tin catalyst, surfactant, foaming agent, foaming agent and cell opening agent, stir at 1500 r / min for 2-3 min, and record it as component A; (2) Stir the diphenylmethane diisocyanate at 1000 r / min for 10-30 s and denote it as component B; (3) Increase the rotation speed of component A to 2500-3000 r / min, add component B, stir at high speed for 10-15 s, pour into mold, control the mold temperature at 60±0.5 ℃, cut after 24-72 h to obtain the product.
Citation Information
Patent Citations
High-temperature-resisting polyurethane foam and preparation method thereof