A printable thermal interface material and methods of making and using the same
By blending poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate] acrylate matrix with liquid metal thermally conductive filler, a low-modulus, high-adhesion printable thermal interface material was prepared, which solved the problems of insufficient thermal conductivity and flexibility of existing materials, and realized efficient heat dissipation and 3D printing applications.
Patent Information
- Application Number
- CN202311862805.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-29
AI Technical Summary
Existing thermal interface materials have shortcomings in terms of thermal conductivity, low modulus and high adhesion, making it difficult to effectively fill micro gaps, resulting in high contact thermal resistance, affecting heat dissipation efficiency, and insufficient flexibility and machinability in 3D printing applications.
A printable thermal interface material with low modulus and high adhesion is prepared by melt or solution blending of poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate matrix with liquid metal thermally conductive fillers (such as indium tin alloy, sodium potassium alloy, magnesium aluminum alloy or gallium indium alloy), and then using 3D printing technology to encapsulate integrated chip circuits.
It achieves a thermal interface material with low total thermal resistance, low contact thermal resistance, high thermal conductivity and excellent printability, which can effectively dissipate chip heat and maintain the chip temperature below 50°C, making it suitable for the precise packaging of integrated chip circuits.
Smart Images

Figure CN117801450B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of thermally conductive materials technology, and in particular to a printable thermal interface material, its preparation method, and its application. Background Technology
[0002] The information disclosed in the background section of this invention is intended only to enhance the understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.
[0003] With technological advancements, electronic devices are becoming increasingly integrated, miniaturized, and power-density. Excessive heat accumulation can significantly impact the performance and lifespan of electronic devices, making heat dissipation a growing concern. The contact surface between electronic devices and heat sinks is typically rough, and warping during operation can create tiny air-filled gaps. These gaps exhibit high thermal resistance, drastically affecting heat dissipation efficiency. Thermal interface materials are used to fill these microscopic gaps between electronic components and heat sinks to improve heat dissipation.
[0004] Patent CN 114573830 B (authorization announcement date: 2023.04.18) discloses a room temperature self-healing flexible organosilicon thermal interface material with self-adhesive properties, which has a thermal conductivity ≥1.8W / (mK), room temperature self-healing efficiency ≥90%, tensile strain ≥200%, and bonding strength ≥4MPa.
[0005] However, simply increasing thermal conductivity to a certain extent does not guarantee optimal heat transfer. Equally important is reducing the contact thermal resistance between thermal interface materials, electronic components, and heat sinks. Thermal interface materials must simultaneously possess high thermal conductivity, low modulus, and high adhesion to more effectively fill microscopic gaps, thereby significantly reducing contact thermal resistance. Therefore, developing a novel thermal interface material with high thermal conductivity, low thermal resistance, and high adhesion is crucial for the development of the electronics industry.
[0006] In recent years, with the advancement of 3D printing and chip technology, people have increasingly focused on using 3D printing to package integrated chip circuits. 3D printing is a crucial technology for the development of electronic packaging towards intelligence, versatility, and fine structures. 3D printing can achieve precise packaging based on the chip circuit structure. However, simultaneously possessing high thermal conductivity, low thermal resistance, high adhesion, and excellent printability remains a major challenge in the application of 3D printing technology in electronic packaging based on thermal interface materials. Currently, the most commonly used methods to improve thermal conductivity include: improving filler orientation through magnetic fields, hydrothermal reduction, constructing isolation structures, template guidance methods, ice templates, and infiltration methods. While these methods improve thermal conductivity to some extent, these composite thermal interface materials have significant drawbacks in terms of flexibility and processability.
[0007] Therefore, there is an urgent need for a high-performance printable thermal interface material to precisely encapsulate chip circuits and improve the above problems. Summary of the Invention
[0008] In view of this, the present invention provides a printable thermal interface material, its preparation method and application. The printable thermal interface material has high thermal conductivity, low thermal resistance, high adhesion and excellent printability, and has good application prospects.
[0009] In a first aspect, the present invention provides a printable thermal interface material comprising the following components in parts by weight: 15 to 25 parts of poly(2-[[(butylamino)carbonyl]oxy] ethyl acrylate matrix and 75 to 85 parts of liquid metal thermally conductive filler.
[0010] Preferably, the liquid metal thermally conductive filler is selected from any one of indium tin alloy, sodium potassium alloy, magnesium aluminum alloy or gallium indium alloy.
[0011] Preferably, the particle size of the liquid metal thermally conductive filler is 5–15 μm.
[0012] Secondly, the present invention provides a method for preparing the above-mentioned printable thermal interface material, comprising the following steps:
[0013] Using ethyl 2-[[(butylamino)carbonyl]oxy]acrylate as a monomer, a poly(2-[[(butylamino)carbonyl]oxy]acrylate precursor was obtained by free radical solution polymerization. The precursor was then precipitated, filtered, and dried to obtain the poly(2-[[(butylamino)carbonyl]oxy]acrylate matrix. The poly(2-[[(butylamino)carbonyl]oxy]acrylate matrix and a liquid metal thermally conductive filler were then melt-blended or solution-blended to obtain the final product.
[0014] Preferably, the solvent for the free radical solution polymerization is selected from one of N,N-dimethylacetamide, N,N-dimethylformamide, or N-methylpyrrolidone.
[0015] Preferably, the initiator for free radical solution polymerization is selected from one of the following: organic peroxide initiators, azo initiators, inorganic peroxide initiators, or redox initiators.
[0016] Preferably, the free radical solution polymerization time is 10-30 h; the temperature is 40-80 °C; and nitrogen and / or argon are introduced during the free radical solution polymerization process.
[0017] Preferably, the solvent used for precipitation is water; the drying temperature is 40–70°C, and the drying time is 15–24 hours.
[0018] Preferably, the melt blending temperature is 90–120°C and the time is 1–2 h; the melt blending process also includes ultrasonic dispersion for 20–40 min.
[0019] Preferably, the solvent used for blending the solution is ethyl acetate.
[0020] Thirdly, the present invention provides an application of the above-mentioned printable thermal interface material, wherein the application is to use the printable thermal interface material in the field of integrated chip circuits.
[0021] Preferably, the method of applying the printable thermal interface material to the field of integrated chip circuits is: encapsulating the integrated chip circuit with the printable thermal interface material using a 3D printing method.
[0022] Preferably, the 3D printing includes one of photopolymerization 3D printing, fused deposition modeling 3D printing, powder bonding 3D printing, or selective laser sintering 3D printing.
[0023] Preferably, the air pressure during the printing process is maintained at 10–100 kPa; the travel speed during the printing process is 10–50 mm / min; the temperature of the printing barrel is maintained at 80–100°C; the temperature at the nozzle is maintained at 90–120°C; and the ambient temperature during the printing process is 20–30°C.
[0024] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0025] In the printable thermal interface material provided by this invention, the poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate matrix provides low modulus and high adhesion to the thermal interface material through the action of long side chains and hydrogen bonds. The addition of liquid metal thermally conductive filler not only improves the thermal conductivity of the thermal interface material, but also reduces the contact thermal resistance between the thermal interface material and the chip. Therefore, the printable thermal interface material provided by this invention has low total thermal resistance, low contact thermal resistance, high thermal conductivity, low storage modulus and excellent printability, and can be applied to the field of integrated chip circuits in combination with 3D printing technology. Attached Figure Description
[0026] The accompanying drawings, which form part of this specification, are used to provide a further understanding of the invention. The illustrative embodiments and descriptions of the invention are used to explain the invention and do not constitute an undue limitation thereof. Obviously, those skilled in the art can obtain other drawings based on these drawings without any inventive effort.
[0027] Figure 1 This is a schematic diagram of the printable thermal interface material preparation process in Embodiment 2 of the present invention;
[0028] Figure 2 This is a schematic diagram of the 3D printed packaged chip of the present invention. Detailed Implementation
[0029] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0030] The present invention provides a printable thermal interface material comprising the following components in parts by weight: 15-25 parts of poly(2-[[(butylamino)carbonyl]oxy] ethyl acrylate matrix and 75-85 parts of liquid metal thermally conductive filler.
[0031] This invention uses poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate] as a matrix. The presence of its long side chains allows it to fully contact the substrate surface, which is a key step in wet interfacial adhesion. The NH and C=O groups play a role by forming hydrogen bonds with various surfaces, thereby endowing poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate] with excellent adhesion properties. Then, liquid metal thermally conductive filler is wrapped by the long side chains of the poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate] matrix, thereby improving the thermal conductivity and reducing the contact thermal resistance between the thermal interface material and the chip.
[0032] This invention uses liquid metal as a thermally conductive filler. Liquid metal has good flexibility, making it suitable as a filler for printing, and the resulting thermal interface material has low contact thermal resistance. In existing technologies, excessive solid fillers are often added to improve thermal conductivity. However, adding excessive solid fillers causes the composite material to harden, which not only increases contact thermal resistance and affects heat dissipation but also hinders printing. Furthermore, the poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate] matrix of this invention can effectively encapsulate the liquid metal, preventing leakage.
[0033] The comparison of the amounts of poly(2-[[(butylamino)carbonyl]oxy] ethyl acrylate matrix and liquid metal thermally conductive filler is crucial. If there is too little liquid metal thermally conductive filler, the improvement in thermal conductivity will not be significant and the heat dissipation effect will be poor; if there is too much liquid metal thermally conductive filler, it will be difficult to mix evenly with the polymer matrix and cannot be used normally.
[0034] The present invention does not impose any special restrictions on the type of liquid metal thermally conductive filler, and any liquid metal thermally conductive filler commonly used in the art can be used. The present invention preferably selects any one of indium tin alloy, sodium potassium alloy, magnesium aluminum alloy or gallium indium alloy.
[0035] In this invention, the particle size of the liquid metal thermally conductive filler is 5–15 μm.
[0036] The present invention also provides a method for preparing the above-mentioned printable thermal interface material, comprising the following steps:
[0037] Using ethyl 2-[[(butylamino)carbonyl]oxy]acrylate as a monomer, a poly(2-[[(butylamino)carbonyl]oxy]acrylate precursor was obtained by free radical solution polymerization. The precursor was then precipitated, filtered, and dried to obtain the poly(2-[[(butylamino)carbonyl]oxy]acrylate matrix. The poly(2-[[(butylamino)carbonyl]oxy]acrylate matrix and a liquid metal thermally conductive filler were then melt-blended or solution-blended to obtain the final product.
[0038] This invention does not impose any special restrictions on the solvent used for free radical solution polymerization, as long as it can dissolve ethyl 2-[[(butylamino)carbonyl]oxy]acrylate monomer and poly(2-[[(butylamino)carbonyl]oxy]acrylate. Preferably, the solvent is selected from N,N-dimethylacetamide, N,N-dimethylformamide or N-methylpyrrolidone.
[0039] This invention does not impose special restrictions on the type of initiator used in free radical solution polymerization; commonly used initiators for free radical solution polymerization can be selected. Preferably, the initiator is selected from one of the following: organic peroxide initiators, azo initiators, inorganic peroxide initiators, or redox initiators. Organic peroxide initiators include benzoyl peroxide, cumene hydroperoxide, etc.; azo initiators include azobisisobutyronitrile, azobisisoheptanenitrile, etc.; inorganic peroxide initiators include potassium persulfate, sodium persulfate, ammonium persulfate, etc.; redox initiators include ammonium persulfate / sodium bisulfite, potassium persulfate / sodium bisulfite, ammonium persulfate / ferrous sulfate, hydrogen peroxide / ferrous sulfate, etc.
[0040] In this invention, the free radical solution polymerization time is 10–30 h; the temperature is 40–80 °C; the polymerization time and temperature are related to the selected initiator, and those skilled in the art can adjust them appropriately according to the selected initiator. To avoid oxygen affecting the polymerization process, nitrogen and / or argon are introduced as protective gases during the free radical solution polymerization process of this invention to isolate oxygen.
[0041] In this invention, the solvent used for precipitation is water. Poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate) is insoluble in water but soluble in the solvent, therefore it can be precipitated in water to remove the solvent and unreacted monomers. After precipitation, water is removed by vacuum filtration. The vacuum filtration process can be repeated multiple times to thoroughly remove unreacted monomers and solvents, followed by drying. The drying temperature is 40–70°C, and the drying time is 15–24 hours.
[0042] In this invention, the melt blending temperature is 90–120°C, and the time is 1–2 hours; the melt blending process also includes ultrasonic dispersion for 20–40 minutes. At 90–120°C, both the liquid metal and poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate] melt, exhibiting high fluidity, thus allowing for better blending. Ultrasonic dispersion is used to ensure uniform dispersion of the liquid metal within the polymer matrix, guaranteeing good uniformity of the obtained printable interface material.
[0043] In this invention, the solvent for solution blending is ethyl acetate. After blending, the solvent is evaporated to dryness before subsequent applications.
[0044] This invention provides an application of the aforementioned printable thermal interface material, specifically its application in the field of integrated circuit chips. The method for applying the printable thermal interface material to integrated circuit chips involves encapsulating the integrated circuit chip using a 3D printing method.
[0045] Because the printable thermal interface material provided by this invention has low total thermal resistance, low contact resistance, and high thermal conductivity, it can effectively dissipate the heat of the chip and maintain its overall temperature below 50°C. Within this temperature range, poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate] can effectively encapsulate liquid metal, providing good safety.
[0046] This invention does not impose any special limitations on the 3D printing method; any commonly used 3D printing method in the field can be selected. This invention is selected from one of photopolymerization 3D printing, fused deposition modeling (FDM) 3D printing, powder bonding 3D printing, or selective laser sintering (SLS) 3D printing. The air pressure during the printing process is maintained at 10–100 kPa; the travel speed during the printing process is 10–50 mm / min; the temperature of the printing barrel is maintained at 80–100°C; the temperature at the nozzle is maintained at 90–120°C; and the ambient temperature during the printing process is 20–30°C.
[0047] The technical solution of the present invention will be further described below with reference to specific embodiments.
[0048] Example 1
[0049] This embodiment provides the preparation of a poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate matrix, comprising the following steps:
[0050] 2-[[(butylamino)carbonyl]oxy]ethyl acrylate was selected as the monomer for the poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate]acrylate matrix, N,N-dimethylacetamide was selected as the solvent, and 2,2-azobisisobutyronitrile was selected as the initiator. 10 g of 2-[[(butylamino)carbonyl]oxy]ethyl acrylate and 20 mL of N,N-dimethylacetamide were added to a 50 mL beaker, which was then placed in an oil bath. The oil bath temperature was set to 68 °C, and the mixture was stirred at 300 rpm for 1 h. 10 g of 2-[[(butylamino)carbonyl]oxy]ethyl acrylate, 20 mL of N,N-dimethylacetamide, and 15.2 mg of 2,2-azobisisobutyronitrile were added to a 100 mL two-necked flask, which was then placed in an oil bath. The oil bath temperature was set to 68 °C, and the mixture was stirred at 400 rpm while nitrogen gas was introduced. Stir for 24 hours until the poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate precursor is formed.
[0051] The obtained poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate) precursor was precipitated in 200 ml of deionized water. After multiple filtrations, the white precipitate was collected and added to a 25 ml beaker, which was then placed in a drying oven at 50°C. Drying was carried out for 24 hours until the material became transparent, yielding the poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate matrix.
[0052] Example 2
[0053] This embodiment provides a method for preparing a printable thermal interface material, as shown in the schematic diagram. Figure 1 As shown, it includes the following steps:
[0054] Gallium-indium alloy with a melting point of 16℃ was selected as the liquid metal thermally conductive filler. 20g of the liquid metal thermally conductive filler and 5g of poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate prepared in Example 1 were added to a 25ml beaker (the mass ratio of thermally conductive filler to matrix was 80:20). The beaker was placed in an oil bath. The oil bath temperature was set to 100℃, and the mixture was stirred with a glass rod for 10 minutes to achieve initial mixing, followed by ultrasonic dispersion for 30 minutes. The beaker was then placed in the oil bath again, and the temperature was set to 100℃. Stirring was continued for 1 hour until the liquid metal was uniformly dispersed in the poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate), thus obtaining the composite thermal interface material.
[0055] Example 3
[0056] The difference between this embodiment and embodiment 2 is that indium tin alloy is used instead of gallium indium alloy.
[0057] Example 4
[0058] The difference between this embodiment and embodiment 2 is that sodium-potassium alloy is used instead of gallium-indium alloy.
[0059] Example 5
[0060] The difference between this embodiment and embodiment 2 is that magnesium-aluminum alloy is used instead of gallium-indium alloy.
[0061] Comparative Example 1
[0062] The difference between this comparative example and Example 2 is that 17.5g of liquid metal thermally conductive filler and 7.5g of poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate] were added to a 25ml beaker (the mass ratio of thermally conductive filler to matrix was 70:30).
[0063] Comparative Example 2
[0064] The difference between this comparative example and Example 2 is that 15g of liquid metal thermally conductive filler and 10g of poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate] were added to a 25ml beaker (the mass ratio of thermally conductive filler to matrix was 60:40).
[0065] Comparative Example 3
[0066] The difference between this comparative example and Example 2 is that 12.5g of liquid metal thermally conductive filler and 12.5g of poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate] were added to a 25ml beaker (the mass ratio of thermally conductive filler to matrix was 50:50).
[0067] Comparative Example 4
[0068] The difference between this comparative example and Example 2 is that 22.5g of liquid metal thermally conductive filler and 2.5g of poly(2-[[(butylamino)carbonyl]oxy]ethyl acrylate] were added to a 25ml beaker (the mass ratio of thermally conductive filler to matrix was 90:10). The inventors found that under this ratio, the two could not be mixed evenly, making subsequent printing impossible.
[0069] Test case
[0070] Encapsulation experiments were conducted on the materials of Examples 1-4 and Comparative Example 1, and the steps are as follows:
[0071] The chip circuitry was packaged using fused deposition modeling (FDM) technology. A schematic diagram of the packaging is shown below. Figure 2 As shown, place the above material in a drying oven at 90℃ and heat for 30 minutes. Then add the material to the feed cylinder, adjusting the cylinder temperature to 90℃ and the nozzle temperature to 100℃. Adjust the printing air pressure to 40 kPa. Set the printer's travel speed to 40 mm / min. Package the circuit according to the specific location of the chip in the chip circuit.
[0072] The properties of the materials in Examples 1-2 and Comparative Examples 1-3 were measured, and the results are shown in Table 1.
[0073] Table 1. Material property test results of Examples 1-2 and Comparative Examples 1-3
[0074]
[0075] As can be seen from Table 1, when the mass ratio of thermally conductive filler to matrix is 80:20 (Example 2), it exhibits excellent performance, with a total thermal resistance of less than 1 cm. 2 ·KW -1 Moreover, the thermal conductivity is 3 W·m -1 ·K -1 The above properties indicate good thermal conductivity. When the thermally conductive filler accounts for less than 70 wt% of the total mass of the thermally conductive filler and the matrix, the thermal conductivity decreases significantly, all falling below 1 W·m. -1 ·K -1 Below that, and the total thermal resistance also exceeds 1cm. 2 ·KW -1 It can be seen that the mass ratio of thermally conductive filler to matrix has a significant impact on the thermal conductivity and heat dissipation performance of the material.
[0076] The contact thermal resistance and storage modulus of the thermal interface material in Example 2 were measured, and its contact thermal resistance was 0.25 cm. 2 ·KW -1 The low contact thermal resistance enables better heat dissipation performance; the storage modulus of the material is 31 kPa at a shear rate of 10 rad / s, indicating that the material is relatively soft and suitable as a printing material.
[0077] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A printable thermal interface material, characterized in that, It comprises the following components in parts by weight: 20-25 parts of poly(2-[[(butylamino)carbonyl]oxy] ethyl acrylate matrix and 75-80 parts of liquid metal thermally conductive filler.
2. The printable thermal interface material as described in claim 1, characterized in that, The liquid metal thermally conductive filler is selected from any one of indium tin alloy, sodium potassium alloy, magnesium aluminum alloy or gallium indium alloy, and the particle size of the liquid metal thermally conductive filler is 5~15μm.
3. The method for preparing the printable thermal interface material according to any one of claims 1 to 2, characterized in that, Includes the following steps: Using ethyl 2-[[(butylamino)carbonyl]oxy]acrylate as a monomer, a poly(2-[[(butylamino)carbonyl]oxy]acrylate precursor was obtained by free radical solution polymerization. The precursor was then precipitated, filtered, and dried to obtain the poly(2-[[(butylamino)carbonyl]oxy]acrylate matrix. The poly(2-[[(butylamino)carbonyl]oxy]acrylate matrix and a liquid metal thermally conductive filler were then melt-blended or solution-blended to obtain the final product.
4. The preparation method according to claim 3, characterized in that, The solvent for the free radical solution polymerization is selected from one of N,N-dimethylacetamide, N,N-dimethylformamide, or N-methylpyrrolidone.
5. The preparation method according to claim 3, characterized in that, The free radical solution polymerization time is 10~30h; the temperature is 40~80℃; nitrogen and / or argon are introduced during the free radical solution polymerization process.
6. The preparation method according to claim 3, characterized in that, The solvent used for precipitation is water; the drying temperature is 40~70℃, and the drying time is 15~24h.
7. The preparation method according to claim 3, characterized in that, The melt blending temperature is 90~120℃ and the time is 1~2h; the melt blending process also includes ultrasonic dispersion for 20~40min; the solvent for solution blending is ethyl acetate.
8. The application of the printable thermal interface material as described in any one of claims 1 to 2, characterized in that, The application is to use the printable thermal interface material in the field of integrated chip circuits.
9. The application as described in claim 8, characterized in that, The method for applying the printable thermal interface material to the field of integrated chip circuits is as follows: the printable thermal interface material is used to encapsulate the integrated chip circuit using a 3D printing method; the 3D printing includes one of photopolymerization 3D printing, fused deposition modeling 3D printing, powder bonding 3D printing, or selective laser sintering 3D printing.
10. The application as described in claim 9, characterized in that, The air pressure during printing is maintained at 10~100kPa; the travel speed during printing is 10~50mm / min; the temperature of the printing barrel is maintained at 80~100℃, the temperature of the nozzle is maintained at 90~120℃, and the ambient temperature during printing is 20~30℃.
Citation Information
Patent Citations
Soft light-cured 3D printing resin material and preparation method thereof
CN111471139A
High-performance thermal interface material based on polymerization shrinkage induced liquid metal self-assembly and preparation method of high-performance thermal interface material
CN115558413A