High-melting-point, high-temperature-resistant nickel-based alloy and high-temperature-resistant cladding layer

By using nickel-based alloy powder and laser or plasma cladding technology, the problems of thickness, bonding strength and durability of high-temperature oxidation coatings have been solved, achieving high melting point and long life high-temperature oxidation resistance.

CN117802358BActive Publication Date: 2026-11-20WUHU DIANJIN ELECTROMECHANICAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311545827.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-20
Publication Date
2026-11-20
Estimated Expiration
2043-11-20

AI Technical Summary

Technical Problem

Existing high-temperature resistant oxidation coatings suffer from problems such as insufficient thickness, low bonding strength, easy formation of pores and inclusions, and easy coating peeling. Furthermore, traditional processes are costly and have poor performance.

Method used

By using nickel-based alloy powder, spherical powders are prepared through supersonic gas atomization. Combined with laser or plasma cladding technology, cladding is carried out in an atmospheric or protective atmosphere. By controlling the alloy composition and process parameters, a high-melting-point, high-temperature resistant cladding layer is prepared.

Benefits of technology

The prepared cladding layer exhibits excellent high-temperature oxidation resistance under high-temperature conditions, has a long service life, a melting point above 1450℃, and a service life of more than 90 days in environments above 1300℃.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117802358B_ABST
    Figure CN117802358B_ABST
Patent Text Reader

Abstract

The application discloses a high-melting-point and high-temperature-resistant nickel-based alloy, which comprises the following components in percentage by weight: Cr 20-39%, Si 0.2-1.0%, Ni greater than or equal to 60%, C less than or equal to 0.05%, P less than or equal to 0.001%, and B less than or equal to 0.1%, and the sum of the weights of the components is 100%. The application also provides a high-temperature-resistant cladding layer obtained by cladding treatment using the nickel-based alloy powder as cladding material. The nickel-based alloy disclosed by the application mainly comprises nickel and chromium, and can obtain a high melting point at a relatively low Cr content. The cladding layer obtained by using the nickel-based alloy powder exhibits excellent high-temperature oxidation resistance and long protection life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nickel-based alloys, and particularly relates to a high-melting-point, high-temperature resistant nickel oxide-based alloy and a high-temperature resistant cladding layer. Background Technology

[0002] Protecting components operating under high temperatures is a major challenge in the industrial and aerospace sectors. Currently, most high-temperature resistant oxide coatings, both domestically and internationally, are produced using traditional processes such as spraying and welding. These traditional processes present several insurmountable problems, including: 1) achieving a sufficiently thick protective layer; 2) low bonding strength, leading to defects such as porosity and inclusions; and 3) a non-metallic bond between the coating and the base material, resulting in coating detachment and a short service life. Using laser or plasma cladding technology to manufacture high-temperature resistant oxide coatings can effectively solve these problems, significantly reducing the process requirements and costs.

[0003] In the field of high-temperature oxidation protection materials, the market currently mainly focuses on sprayed nickel-chromium alloy powder. This type of material is suitable for thermal spraying to prepare sprayed coatings. The preparation method of this type of powder mainly involves mixing, granulating, and sintering non-spherical powders to obtain spherical powders. The overall performance of this powder is not good enough, and it has the following problems: 1) Poor cladding formation. Adding other trace elements to the powder is beneficial for spraying formation, but it lowers the melting point; 2) The granulation and sintering process is too costly; 3) It cannot meet the long lifespan requirements of high-temperature protective coatings; 4) It is prone to large pores during laser cladding or plasma cladding.

[0004] Therefore, it is of great significance to develop high-temperature oxidation-resistant protective materials for cladding processes that have high-temperature oxidation resistance and stable performance. Summary of the Invention

[0005] To address the aforementioned technical problems, this invention provides a nickel-based alloy for cladding, which is mainly composed of nickel and chromium and can achieve a high melting point with a relatively low Cr content. The cladding layer obtained using this nickel-based alloy powder exhibits excellent high-temperature oxidation resistance and a long protective lifespan.

[0006] The specific solution of this invention is as follows:

[0007] One of the objectives of this invention is to provide a high-melting-point, high-temperature resistant nickel oxide-based alloy, comprising the following components by weight percentage: Cr 20-39%, Si 0.2-1.0%, Ni ≥ 60%, C ≤ 0.05%, P ≤ 0.001%, B ≤ 0.1%, with the sum of the weights of all components being 100%.

[0008] Preferably, the components comprise the following by weight percentage: Cr 20-39%, Si 0.2-1.0%, Ni 60-79.8%, C≤0.05%, P≤0.001%, B≤0.1%, and the sum of the weights of all components is 100%.

[0009] Preferably, the composition comprises the following components by weight percentage: Cr 20-39%, Si 0.2-1.0%, C≤0.05%, P≤0.001%, B≤0.1%, with the balance being Ni.

[0010] According to the inventor's previous research, increasing the Cr content is beneficial to improving the high-temperature oxidation resistance of the cladding layer. However, this invention achieves a high melting point and exhibits excellent high-temperature oxidation resistance by controlling the composition and components of the nickel-based alloy at a relatively low Cr content (20-39%).

[0011] Compared to the approach of adding both Si and B to nickel-based alloys, this invention eliminates B while controlling the Si content to 0.2-1.0% and the Ni content to ≥60%. This ensures the fluidity of the molten pool and the forming performance of the cladding layer in laser cladding and plasma cladding of nickel-based alloy powders, as well as the high melting point of the nickel-based alloy.

[0012] For other elements, such as C, P, and B, their content needs to be strictly controlled within a certain range to avoid lowering the alloy's melting point and limiting the upper limit of the coating's operating temperature.

[0013] The second objective of this invention is to provide a high-temperature resistant cladding layer, which is obtained by cladding treatment using any of the above-mentioned nickel-based alloy powders as the cladding material.

[0014] Preferably, the particle size of the nickel-based alloy powder is 50-150 μm.

[0015] The present invention limits the particle size of nickel-based alloy powder to 50-150μm because powder particles smaller than 50μm are easily blown away during the cladding process, resulting in low powder utilization efficiency; powder particles larger than 150μm are difficult to melt during the cladding process, which affects the formation of the cladding layer.

[0016] The preparation method of the nickel-based alloy powder is not specifically limited, but includes, but is not limited to, supersonic gas atomization, as long as spherical nickel-based alloy powder is obtained. The supersonic gas atomization method specifically includes: (1) adding pure nickel, pure chromium and pure silicon into a vacuum melting furnace in proportion and stirring electromagnetically to obtain a uniform alloy liquid; (2) using supersonic gas atomization process to prepare spherical alloy powder from the alloy liquid; the gas flow rate is 300-400m / s.

[0017] Supersonic atomization can effectively break down highly viscous nickel-based alloys, achieving a powder recovery rate of up to 60%.

[0018] Preferably, the cladding process is laser cladding or plasma cladding.

[0019] Preferably, the cladding is carried out under atmospheric conditions or a protective atmosphere; the protective atmosphere is an Ar-CO2 mixture or an Ar-O2 mixture.

[0020] Preferably, in the Ar-CO2 mixture, the volume percentage of Ar is ≥90%; in the Ar-O2 mixture, the volume percentage of Ar is ≥97%.

[0021] For the nickel-based alloy composition described in this invention, cladding is preferably performed under atmospheric conditions. Under atmospheric conditions, Si in the Ni-based alloy is preferentially oxidized and floats to the surface, thereby achieving the purpose of Si removal from the cladding layer. Thus, by matching this process design with the alloy composition, adding Si to the alloy composition, and then removing Si using the process, the flowability of the nickel-based alloy powder is ensured, and the melting point and high-temperature oxidation resistance of the obtained cladding layer are further improved.

[0022] For applications with special performance requirements, cladding can be performed under a protective atmosphere. Specifically, the protective atmosphere is an Ar-CO2 mixture or an Ar-O2 mixture. In the mixture, a small amount of O2 or CO2 has certain oxidizing properties. The small amount of oxidizing gas preferentially reacts with Si to eliminate Si. At the same time, since the amount of oxidizing gas is small, it will not cause large-scale oxidation of the cladding layer. This achieves the goal of effectively removing Si from the cladding layer while avoiding large-scale oxidation of the cladding layer.

[0023] Preferably, the parameters for laser cladding are: laser power of 1100-1800W, scanning speed of 4.5-5.5mm / s, laser spot with a diameter of 1.5-3mm, overlap rate of 20-40%, air flow rate of 2-5L / min, and powder feeding voltage of 10-20V.

[0024] Preferably, the parameters for plasma cladding are: current of 150-200A, both plasma gas and protective gas are Ar, plasma gas flow rate of 0.1-0.5L / min, protective gas flow rate of 10-15L / min, and powder feeding speed of 0.5-1.5Kg / h.

[0025] The beneficial effects of this invention are:

[0026] The nickel-based alloy provided by this invention has both a high melting point and good cladding performance. The cladding layer prepared using this alloy powder has a melting point higher than 1450℃ and a service life of more than 90 days in an environment above 1300℃, and has good high-temperature oxidation resistance. Attached Figure Description

[0027] Figure 1 This is a photograph of the cladding layer obtained in Example 1 after 90 days of use at 1300°C.

[0028] Figure 2 This is a photograph of the cladding layer obtained in Example 3 after 100 days of use at 1300°C.

[0029] Figure 3 A photograph of the cladding layer obtained in Comparative Example 1 after 20 days of use at 1300℃.

[0030] Figure 4 A photograph of the cladding layer obtained in Comparative Example 2 after 32 days of use at 1300℃.

[0031] Figure 5 The image shows the actual product of the cladding layer of Comparative Example 3 after 90 days of use in an environment of 1300℃. Detailed Implementation

[0032] The following embodiments describe the preparation process of nickel-based alloy powder, specifically as follows: pure nickel, pure chromium, and pure silicon are added into a vacuum melting furnace in proportion, and electromagnetic stirring is used during the melting process to obtain a uniform alloy liquid; the alloy liquid is then prepared into spherical alloy powder using a supersonic gas atomization process, wherein the gas flow rate is 350 m / s.

[0033] The technical solution of the present invention will be described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustrative purposes only and are not intended to limit the scope of the present invention.

[0034] Example 1

[0035] A nickel-based alloy comprising the following components by weight percentage: Cr 33%, Si 0.8%, C≤0.05%, P≤0.001%, B≤0.1%, with the balance being Ni.

[0036] A high-temperature resistant cladding layer is prepared on the surface of a pipe fitting using a laser cladding process, with the nickel-based alloy powder described in this embodiment as the cladding material and a mixed gas of 97% Ar + 3% O2 ​​by volume as the protective atmosphere. The cladding layer has a thickness of 1.3 mm.

[0037] The nickel-based alloy powder has a particle size of 50-150μm; the laser cladding parameters are: laser power of 1500W, scanning speed of 4.8mm / s, laser spot with a diameter of 1.5mm, overlap rate of 25%, gas flow rate of 3L / min, and powder feeding voltage of 12V.

[0038] The cladding layer obtained in this embodiment does not exhibit problems such as ablation or burn marks after 90 days of use in a gas combustion environment at 1300℃. Figure 1 As shown.

[0039] Example 2

[0040] A nickel-based alloy comprising the following components by weight percentage: Cr 35%, Si 0.9%, C≤0.05%, P≤0.001%, B≤0.1%, with the balance being Ni.

[0041] A high-temperature resistant cladding layer is prepared on the surface of a pipe fitting using the nickel-based alloy powder described in this embodiment as the cladding material, a mixed gas of 98% Ar + 2% O2 as the protective atmosphere, and a plasma cladding process to obtain a cladding layer with a thickness of 2 mm.

[0042] The nickel-based alloy powder has a particle size of 50-150μm; the plasma cladding parameters are: current 180A, both plasma gas and protective gas are Ar, powder feeding speed 0.6Kg / h, plasma gun oscillation amplitude 12mm, overlap rate 25%, protective gas flow rate 15L / min, and plasma gas flow rate 0.3L / min.

[0043] The cladding layer obtained in this embodiment will not exhibit problems such as ablation or burn marks after 100 days of use in a gas environment at 1300°C.

[0044] Example 3

[0045] A nickel-based alloy comprising the following components by weight percentage: Cr 20%, Si 0.9%, C≤0.05%, P≤0.001%, B≤0.1%, with the balance being Ni.

[0046] A high-temperature resistant cladding layer is prepared on the surface of a pipe fitting using the nickel-based alloy powder described in this embodiment as the cladding material, and the cladding is carried out in an atmospheric environment. The cladding layer has a thickness of 1.5 mm.

[0047] The nickel-based alloy powder has a particle size of 50-150μm; the laser cladding parameters are: laser power of 1500W, scanning speed of 4.8mm / s, laser spot with a diameter of 3mm, overlap rate of 25%, gas flow rate of 3L / min, and powder feeding voltage of 12V.

[0048] The cladding layer obtained in this embodiment exhibited minor ablation and burn marks after 100 days of use in a gas combustion environment at 1300°C. Figure 2 As shown.

[0049] Comparative Example 1

[0050] The NiCr20 coating material used in the market contains the following components by weight percentage: Cr: 20%, with the balance being Ni.

[0051] A protective coating was prepared using supersonic flame spraying, with a thickness of 0.3 mm. Due to limitations of this process, it is difficult to prepare a protective layer thicker than 0.3 mm. The coating forms a semi-metallurgical bond with the substrate, but the bond strength is lower than that of the cladding layer.

[0052] Because this material is designed for supersonic spraying, its use in laser cladding results in severe porosity, poor forming performance, and uneven laser cladding surface, making normal laser cladding production impossible.

[0053] After 20 days of use in a gas-fired environment at 1300℃, the coating peeled off, and the substrate was severely ablated. (See attached image.) Figure 3 As shown. This is because the sprayed coating is porous and the coating and the substrate are not metallurgically bonded, resulting in large-area delamination due to temperature fluctuations during use.

[0054] Comparative Example 2

[0055] The high-temperature oxidation-resistant powder alloy is made from commercially available materials and comprises the following components by weight percentage:

[0056] Cr: 23–29%; Mo: 14–21%; W: 5–12%; Fe: 6–17%; Co: 3–10%; V: 0.1–0.8%; Mn: 0.5–2%; Si: 0.2–2%; Y₂O₃: 0.1–0.5%; Hf: 0.1–0.5%; La₂O₃: 0.1–0.5%; Ce: 0.1–0.5%; Ni: balance.

[0057] The cladding layer of this alloy was prepared using the laser cladding process described in Example 1, resulting in a cladding layer thickness of 1.5 mm. When used in a pulverized coal combustion environment at 1300°C, the workpiece's service life was 32 days. Surface ablation occurred, and burn scars appeared in areas with high pulverized coal contact. See the actual image below. Figure 4 As shown.

[0058] Comparative Example 3

[0059] A cladding layer, using the nickel-based alloy powder described in Example 1 as the cladding material and pure Ar as the protective atmosphere, is prepared on the surface of a pipe fitting using a laser cladding process to obtain a cladding layer with a thickness of 1.3 mm; wherein the particle size of the nickel-based alloy powder is 50-150 μm; and the laser cladding parameters are the same as in Example 1.

[0060] Because pure argon protection prevented the elimination of Si in the cladding layer, it lowered the melting point of the cladding layer. After 90 days of use in a 1300℃ pulverized coal ablation environment, a small amount of ablation formed on its surface, but it did not ablate to the substrate. Figure 5 As shown.

[0061] Comparative Example 4

[0062] A nickel-based alloy comprising the following components by weight percentage: Cr 33%, B 0.8%, C≤0.05%, P≤0.001%, with the balance being Ni.

[0063] A cladding layer, using the nickel-based alloy powder described in this comparative example as the cladding material, and a mixed gas of 97% Ar + 3% O2 ​​by volume as the protective atmosphere, is prepared on the surface of the pipe using a laser cladding process to obtain a cladding layer with a thickness of 1.3 mm; wherein, the particle size of the nickel-based alloy powder is 50-150 μm; the laser cladding parameters are the same as in Example 1.

[0064] Because B has a significant impact on the melting point of nickel-based materials, the cladding layer will melt when used in environments above 1300℃, and its service life is 10 days.

[0065] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A high-temperature resistant cladding layer, characterized in that, The cladding layer is obtained by cladding with nickel-based alloy powder as the cladding material; cladding is carried out under atmospheric conditions or a protective atmosphere; the protective atmosphere is an Ar-CO2 mixture or an Ar-O2 mixture; the high-temperature resistant cladding layer does not contain Si. The nickel-based alloy powder is composed of the following components by weight percentage: Cr 20~39%, Si 0.2~1.0%, C≤0.05%, P≤0.001%, B≤0.1%, with the balance being Ni; the cladding process is laser cladding or plasma cladding. When using laser cladding, the parameters are as follows: laser power of 1100-1800 W, scanning speed of 4.5-5.5 mm / s, laser spot diameter of 1.5-3 mm, overlap rate of 20-40%, gas flow rate of 2-5 L / min, and powder feeding voltage of 10-20 V. When plasma cladding is used, the parameters are as follows: current is 150-200 A, both plasma gas and protective gas are Ar, plasma gas flow rate is 0.1-0.5 L / min, protective gas flow rate is 10-15 L / min, and powder feeding speed is 0.5-1.5 Kg / h.

2. The high-temperature resistant cladding layer according to claim 1, characterized in that, The particle size of the nickel-based alloy powder is 50-150 μm.

3. The high-temperature resistant cladding layer according to claim 1 or 2, characterized in that, In an Ar-CO2 mixture, the volume percentage of Ar is ≥90%; in an Ar-O2 mixture, the volume percentage of Ar is ≥97%.

Citation Information

Patent Citations

  • Corrosion-resistant anti-oxidation low-wear wear-resisting ball and preparation method thereof

    CN106811673A

  • Nickel-based alloy powder for protecting waste incineration boiler and preparation method of coating

    CN116159993A