A eutectic carbide strengthened tantalum alloy and a method for producing the same
By adding Nb, Mo, and W elements to tantalum alloys and generating dispersed eutectic carbides, the problems of insufficient strength and brittleness of tantalum alloys under ultra-high temperature conditions are solved, and a eutectic carbide-reinforced tantalum alloy with high strength and ductility is prepared, which is suitable for aerospace and defense industries.
Patent Information
- Application Number
- CN202311865265.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-29
AI Technical Summary
Existing tantalum alloys lack sufficient strength under ultra-high temperature conditions and suffer from room temperature brittleness, making it difficult to meet the high-temperature service requirements of aerospace and other fields.
By adding Nb, Mo, and W elements to tantalum alloys for solid solution strengthening, and by adding C element to generate dispersed eutectic carbides in situ, eutectic carbide-strengthened tantalum alloys are prepared using vacuum arc melting method. High-melting-point eutectic carbides are formed to improve strength, and the microstructure is adjusted to improve brittleness.
The ultra-high temperature strength and room temperature plasticity of tantalum alloys are significantly improved. The prepared eutectic carbide-reinforced tantalum alloy has a compressive strength of over 600 MPa at 1600℃ and excellent room temperature processing performance, making it suitable for aerospace and defense industries.
Smart Images

Figure CN117802376B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of tantalum alloy technology, and particularly relates to a eutectic carbide-strengthened tantalum alloy strengthened by introducing uniformly dispersed eutectic carbides and its preparation method. Background Technology
[0002] With the development of society and technology, the demand for high-performance, ultra-high temperature resistant structural materials in aerospace, missile weaponry, and other fields is becoming increasingly urgent. The service temperatures of components such as the engine hot end, nose cone, and wing leading edge of hypersonic aircraft have exceeded 1400℃. However, currently commonly used nickel-based high-temperature alloys, limited by their melting points, have a maximum operating temperature of only 1200℃, making it difficult to meet the requirements for service at temperatures above 1400℃. Ultra-high temperature ceramics and CC composites, which meet the temperature resistance requirements, face challenges such as difficult manufacturing, low damage tolerance, and low thermal shock resistance, thus limiting their further application. Refractory metals and their alloys, especially Ta-based alloys, possess characteristics such as high melting point (Ta's melting point is 2996℃), high high-temperature strength, and good thermal shock resistance, while also exhibiting excellent processing properties. Developing high-performance tantalum alloys is of great significance in meeting the urgent demand for ultra-high temperature structural materials.
[0003] Tantalum alloys possess high heat resistance and stress load capacity. With the addition of other refractory metals, their service temperature can reach over 1800℃, exhibiting good thermal shock resistance and high creep strength. Currently, researchers have developed a series of tantalum alloys with significant applications. For example, Ta-10W alloy has been used in the combustion chamber of the Agina spacecraft and the nose cone of missiles (operating at around 2500℃), as well as in the gas spoiler of rocket engine nozzles, the combustion chamber of Apollo spacecraft, and as a reinforcing structural material for space nuclear power plants. Ta-10W-2.5Hf alloy is used for nozzles in liquid rocket nozzles, and Ta-8W-2Hf alloy is used as a reinforcing structural material for encasing the heat source of space-based thermal engines. While the addition of refractory metals such as W and Hf enhances the high-temperature strength of these tantalum alloys through solid solution strengthening, the amount of these solid solution elements must be strictly controlled; otherwise, it will affect the room-temperature plasticity of the alloy. Furthermore, the improvement in mechanical properties through minute adjustments to the alloy composition is limited. The ultra-high temperature strength of existing tantalum alloys still needs further improvement.
[0004] Multi-principal high-entropy alloys are a new type of alloy material that has emerged in recent years. By redesigning the alloy composition through the concept of entropy regulation, the comprehensive performance of the alloy can be greatly improved. Refractory high-entropy alloys designed with multiple refractory metal elements can maintain a stable phase structure and excellent strength under high temperature conditions. For example, the ultimate compressive strength of NbMoTaW and NbMoTaWV refractory high-entropy alloys can reach 467MPa and 707MPa at 1400℃, respectively. However, they have serious room temperature brittleness problems. Summary of the Invention
[0005] This invention discloses a eutectic carbide-reinforced tantalum alloy and its preparation method, in order to solve any of the above-mentioned and other potential problems in the prior art.
[0006] To achieve the above objectives, the technical solution of the present invention is: a eutectic carbide-reinforced tantalum alloy, wherein the alloy composition system is Ta a Nb b Mo c W d C e a, b, c, d, and e are the atomic percentages of each element, where 40 ≤ a ≤ 60, 6 ≤ b ≤ 10, 6 ≤ c ≤ 10, 10 ≤ d ≤ 20, 0 < e ≤ 20, and a + b + c + d + e = 100.
[0007] The present invention also provides an in-situ preparation method of the above-mentioned eutectic carbide-reinforced tantalum alloy, comprising the following steps:
[0008] 1) Accurately weigh the required weights of Ta, Nb, Mo, W and C raw materials, and place them in the water-cooled copper crucible of the non-consumable vacuum arc melting furnace in the order of low melting point raw materials at the bottom and high melting point raw materials at the top.
[0009] 2) Perform vacuum arc melting. Evacuate the sample chamber until the vacuum level is higher than 5 × 10⁻⁶. -3 After Pa, high-purity argon gas with a purity of 99.999% is introduced as a protective gas and arc-ignition medium. The melting current is 350-450A to ensure that all raw materials can be completely melted. The melting is carried out 5-8 times, and the electric arc is maintained for at least 2 minutes during each melting process. Before each melting, the ingot is flipped and tilted at 40°-50° to finally obtain a refractory high-entropy alloy ingot with uniform composition.
[0010] As a preferred embodiment of the above technical solution, the eutectic carbide-reinforced tantalum alloy provided by the present invention further includes some or all of the following technical features:
[0011] Preferably, the Ta, Nb, Mo, and W raw materials in step 1) are elemental particles with a purity of over 99.9% for each element, and the C raw material is high-purity graphite.
[0012] Further optimization involves removing the oxide layer and impurities from the surfaces of Ta, Nb, Mo, and W elemental particles before smelting, ultrasonically cleaning them in ethanol or acetone, and then cutting the high-purity graphite into fine particles.
[0013] Further optimization revealed that by changing the C element content, the proportion of eutectic carbide structure in the microstructure was controlled. As the added C element content increased from 0 to 15 at% and then to 20 at%, the microstructure of the alloy changed from hypoeutectic to eutectic and then to hypereutectic, and the strength gradually increased.
[0014] To address the aforementioned problems, the present invention aims to provide a tantalum alloy with excellent room-temperature strength and ductility as well as ultra-high temperature strength. To address the insufficient ultra-high temperature strength of existing tantalum alloys, this invention utilizes the concept of entropy regulation to achieve solid solution strengthening by adding Nb, Mo, and W elements to the tantalum alloy. Furthermore, it strengthens the alloy by adding C element in situ to generate dispersed high-melting-point eutectic carbides, significantly improving the ultra-high temperature strength of the tantalum alloy. The strength and toughness of the eutectic structure are also coordinated to improve room-temperature brittleness. This eutectic carbide-strengthened tantalum alloy exhibits a compressive strength exceeding 600 MPa at 1600°C, making it suitable for applications in aerospace, defense, and other fields.
[0015] Another objective of this invention is to provide an in-situ preparation method for the above-mentioned eutectic carbide-reinforced tantalum alloy. This method uses high-purity elemental particles of each element as raw materials and prepares the alloy by vacuum arc melting. The method is simple and easy to operate. The eutectic carbides generated in-situ during the solidification process are uniformly dispersed in the prepared alloy, and the phase interface has excellent bonding strength.
[0016] Compared with the prior art, the technical solution of the present invention has the following advantages and beneficial effects:
[0017] 1. This invention adds refractory metal elements Mo, Nb and W to tantalum alloys for solid solution strengthening, and strengthens them by adding C element to generate high-strength, high-melting-point eutectic carbides in situ during solidification, thus obtaining a high-performance eutectic carbide-strengthened tantalum alloy, enriching the tantalum alloy and carbide-strengthened alloy system.
[0018] 2. This invention uses vacuum arc melting to prepare tantalum alloys. Compared with the method of preparing tantalum alloys by powder metallurgy, the process is simple and easy to operate, which can significantly shorten the preparation cycle. The eutectic reaction that occurs during solidification can lower the melting point, which is beneficial to the melting of high melting point elements. The prepared ingot has uniform composition and microstructure. Furthermore, this invention directly uses elemental particles of each element as raw materials, which is simple and easy to operate, has a high raw material utilization rate, and is suitable for further industrial promotion.
[0019] 3. In the eutectic carbide-reinforced tantalum alloy prepared by this invention, lamellar carbides are introduced in situ through a eutectic reaction during solidification, resulting in high reaction efficiency and uniform dispersion of the carbides. The two-phase interface is a semi-coherent interface with low interfacial energy and high interfacial bonding strength, effectively hindering dislocation slip in the alloy during deformation and achieving excellent strengthening effects. Simultaneously, the eutectic carbides are distributed in a network-like interwoven pattern, and the refractory high-entropy alloy phases between the eutectic carbides can inhibit crack propagation in the carbides, improving plasticity.
[0020] 4. The Ta-Nb-Mo-WC tantalum alloy system designed in this invention can adjust the microstructure of the alloy (exhibiting different hypoeutectic, eutectic, and hypereutectic microstructures) by changing the C content, thereby achieving adjustments to properties such as strength and plasticity. Among these, Ta... 48 Nb8Mo8W 16 C 20 The tantalum alloy has a room temperature compressive strength of 2488 MPa and a plastic strain of 6%. Its compressive strength at 1600℃ is as high as 738 MPa, which is significantly better than existing tantalum alloys and high-temperature alloys. It also has certain room temperature processing properties and has outstanding application potential in the field of ultra-high temperature structural materials.
[0021] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of the present invention more apparent and understandable, the following detailed description is provided in conjunction with preferred embodiments. Attached Figure Description
[0022] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings of the embodiments will be briefly described below.
[0023] Figure 1 This is a flowchart of a method for preparing a eutectic carbide-reinforced tantalum alloy according to the present invention.
[0024] Figure 2 This is a schematic diagram of the XRD analysis curves of the tantalum alloy phases prepared in Examples 1-4;
[0025] (a) XRD analysis results of the tantalum alloy phase composition of Ta57Nb9.5Mo9.5W19C5 prepared in Example 1;
[0026] (b) XRD analysis results of the tantalum alloy phase composition of Ta54Nb9Mo9W18C10 prepared in Example 2;
[0027] (c) XRD analysis results of the tantalum alloy phase composition of Ta51Nb8.5Mo8.5W17C15 prepared in Example 3;
[0028] (d) shows the XRD analysis results of the tantalum alloy phase composition of Ta48Nb8Mo8W16C20 prepared in Example 4;
[0029] Figure 3 This is a schematic diagram of the SEM observation results of the microstructure of the tantalum alloys prepared in Examples 2-4;
[0030] (a) SEM observation results of the microstructure of the Ta54Nb9Mo9W18C10 tantalum alloy prepared in Example 2;
[0031] (b) SEM observation results of the microstructure of the Ta51Nb8.5Mo8.5W17C15 tantalum alloy prepared in Example 3;
[0032] (c) The microstructure of the Ta48Nb8Mo8W16C20 tantalum alloy prepared in Example 4 is observed by SEM.
[0033] Figure 4 Schematic diagram of EBSD analysis results of the microstructure of the tantalum alloys prepared in Examples 2-4;
[0034] (a) EBSD analysis results of the microstructure of the Ta54Nb9Mo9W18C10 tantalum alloy prepared in Example 2;
[0035] (b) EBSD analysis results of the microstructure of the Ta51Nb8.5Mo8.5W17C15 tantalum alloy prepared in Example 3;
[0036] (c) EBSD analysis results of the microstructure of the Ta48Nb8Mo8W16C20 tantalum alloy prepared in Example 4;
[0037] Figure 5 This is a schematic diagram of the room temperature compressive stress-strain curves of the tantalum alloys prepared in Examples 1-4.
[0038] Figure 6 This is a schematic diagram of the high-temperature compressive stress-strain curves of the tantalum alloys prepared in Examples 2-3 at 1600℃. Detailed Implementation
[0039] The technical solution of the present invention will be further described below with reference to specific embodiments and accompanying drawings.
[0040] This invention discloses a eutectic carbide-reinforced tantalum alloy, which is strengthened by solid solution addition of refractory metal elements and further strengthened by eutectic carbides. The atomic percentage expression of the tantalum alloy composition is as follows: Ta a Nbb Mo c W d C e , where 40≤a≤60, 6≤b≤10, 6≤c≤10, 10≤d≤20, 0<e≤20, and a+b+c+d+e=100.
[0041] The tantalum alloy is composed of a high-entropy alloy phase with a body-centered cubic structure and a high-entropy carbide phase with a close-packed hexagonal structure. The high-entropy alloy phase is a solid solution composed of Ta, Nb, Mo and W elements, with Ta being the dominant element. The high-entropy carbide phase is a (Ta,Nb,Mo,W)2C solid solution containing Ta, Nb, Mo and W, with Ta being the dominant metal element.
[0042] In the tantalum alloy, as the C content increases, the volume fraction of the carbide phase increases. As the C content increases from 0 to 20 at%, the microstructure changes from hypoeutectic to eutectic and then to hypereutectic. At the same time, the room temperature strength increases and the room temperature plasticity decreases.
[0043] When a = 54, b = 9, c = 9, d = 18, and e = 10, the chemical formula of the eutectic carbide-reinforced tantalum alloy is Ta. 54 Nb9Mo9W 18 C 10 Its room temperature compressive strength is greater than 2500 MPa, its room temperature compressive plastic strain is greater than 10%, and its compressive strength at 1600℃ is 659 MPa.
[0044] When a = 51, b = 8.5, c = 8.5, d = 17, and e = 15, the chemical formula of the eutectic carbide-reinforced tantalum alloy is Ta. 51 Nb 8.5 Mo 8.5 W 17 C 15 Its room temperature compressive strength is greater than 2500 MPa, its room temperature compressive plastic strain is greater than 15%, and its compressive strength at 1600℃ is 632 MPa.
[0045] When a = 48, b = 8, c = 8, d = 16, and e = 20, the chemical formula of the eutectic carbide-reinforced tantalum alloy is Ta. 48 Nb8Mo8W 16 C 20 Its room temperature compressive strength is greater than 2500 MPa, its room temperature compressive plastic strain is 5%, and its 1600℃ compressive strength is 734 MPa.
[0046] When a = 57, b = 9.5, c = 9.5, d = 19, and e = 5, the chemical formula of the eutectic carbide-reinforced tantalum alloy is Ta. 57 Nb 9.5Mo 9.5 W 19 C5 has a room temperature compressive strength of nearly 2500 MPa, a room temperature compressive plastic strain of 14%, and a 1600℃ compressive strength of nearly 600 MPa.
[0047] like Figure 1 The present invention provides a method for in-situ preparation of eutectic carbide-reinforced tantalum alloy, comprising the following steps:
[0048] S1: Accurately weigh the required weights of Ta, Nb, Mo, W, and C raw materials.
[0049] S2: Place the low-melting-point raw materials into the water-cooled copper crucible of the non-consumable vacuum arc melting furnace in the order of low-melting-point raw materials at the bottom and high-melting-point raw materials at the top;
[0050] S3: Perform vacuum arc melting. Evacuate the sample chamber until the vacuum level exceeds 5 × 10⁻⁶. -3 After Pa, high-purity argon gas with a purity of 99.999% is introduced as a protective gas and arc-ignition medium. The melting current is 350-450A to ensure that all raw materials can be completely melted. The melting is carried out 5-8 times, and the electric arc is maintained for at least 2 minutes during each melting process. Before each melting, the ingot is flipped and tilted at 40°-50° to finally obtain a refractory high-entropy alloy ingot with uniform composition.
[0051] The Ta, Nb, Mo, and W raw materials mentioned in S1) are elemental particles with a purity exceeding 99.9% for each element. The C raw material is high-purity graphite. Before melting, the oxide layer and impurities on the surface of the Nb, Mo, Ta, W, and Zr elemental particles are removed, and they are ultrasonically cleaned in ethanol or acetone. The high-purity graphite is then cut into fine particles. When the C content is high, high-purity niobium foil and tantalum foil can be used for the Ta and Nb raw materials. The graphite particles are wrapped in niobium foil and tantalum foil and placed at the bottom of a water-cooled copper crucible.
[0052] Example 1:
[0053] Preparation of Ta 57 Nb 9.5 Mo 9.5 W 19 C5 composition eutectic carbide-reinforced tantalum alloy. The specific steps are as follows:
[0054] (1) Raw material preparation: The alloy smelting raw materials used in this invention are high-purity (≥99.9%) Ta, Nb, Mo and W elemental particles. The surface oxide scale of the raw materials is removed by means of grinding wheels, and they are cleaned by ultrasonic vibration in alcohol. The high-purity graphite is mechanically crushed into smaller particles, and C particles with a size of about 1 mm are screened out by metal sieve. 19.757 g of Ta particles, 1.691 g of Nb particles, 1.746 g of Mo particles, 6.691 g of W particles and 0.115 g of C particles are weighed (the atomic percentage of Ta / Nb / Mo / W / C is 57:9.5:9.5:19:5).
[0055] (2) Vacuum Arc Melting: Place the C particles at the bottom of the water-cooled crucible of the vacuum arc melting furnace, and then place the Ta, Nb, Mo, and W particles into the crucible in order of increasing melting point. Evacuate the sample chamber until the vacuum level is higher than 5 × 10⁻⁶. -3 After Pa, high-purity argon gas with a purity of 99.999% is introduced as a protective gas and arc-ignition medium. The melting current is 350-450A to ensure that all raw materials can be completely melted. The melting is carried out 5 times, and the electric arc is maintained for 3 minutes during each melting process. Before each melting, the ingot is flipped and tilted at 40°. Finally, it is rapidly cooled to room temperature to obtain a tantalum alloy ingot with uniform composition.
[0056] Figure 2 The curve (a) represents the Ta prepared in Example 1. 57 Nb 9.5 Mo 9.5 W 19 The XRD pattern of the C5 tantalum alloy shows that the prepared tantalum alloy is mainly composed of a refractory high-entropy alloy phase with a BCC structure and a small amount of carbide phase with an HCP structure. Figure 5 Figure (a) shows the compression curve of the alloy at room temperature. Figure 5 As shown in curve (a), the plastic strain of this alloy at room temperature is 14%, and its room temperature compressive strength is close to 2500 MPa.
[0057] Example 2:
[0058] Preparation of Ta 54 Nb9Mo9W 18 C 10 A eutectic carbide-reinforced tantalum alloy. The specific steps are as follows:
[0059] (1) Raw material preparation: The alloy smelting raw materials used in this invention are high-purity (≥99.9%) Ta, Nb, Mo and W elemental particles. The surface oxide scale of the raw materials is removed by means of grinding wheels, and they are cleaned by ultrasonic vibration in alcohol. The high-purity graphite is mechanically crushed into smaller particles, and C particles with a size of about 1 mm are screened out by metal sieve. 19.673 g of Ta particles, 1.684 g of Nb particles, 1.738 g of Mo particles, 6.663 g of W particles and 0.242 g of C particles are weighed (the atomic percentage of Ta / Nb / Mo / W / C is 54:9:9:18:10).
[0060] (2) Vacuum Arc Melting: Place the C particles at the bottom of the water-cooled crucible of the vacuum arc melting furnace, and then place the Ta, Nb, Mo, and W particles into the crucible in order of increasing melting point. Evacuate the sample chamber until the vacuum level is higher than 5 × 10⁻⁶. -3 After Pa, high-purity argon gas with a purity of 99.999% is introduced as a protective gas and arc-ignition medium. The melting current is 350-450A to ensure that all raw materials can be completely melted. The melting is carried out 5 times, and the electric arc is maintained for 3 minutes during each melting process. Before each melting, the ingot is flipped and tilted at 50°. Finally, it is rapidly cooled to room temperature to obtain a tantalum alloy ingot with uniform composition.
[0061] Figure 2 The curve (b) represents the Ta prepared in Example 1. 54 Nb9Mo9W 18 C 10 The XRD pattern of the tantalum alloy composition shows that the prepared tantalum alloy is mainly composed of a refractory high-entropy alloy phase with a BCC structure and a carbide phase with an HCP structure; observations were performed using SEM and EBSD, as shown in the image. Figure 3 (a) and Figure 4 As shown in (a), its microstructure is mainly a dendritic refractory high-entropy alloy phase, with carbide phases distributed between the dendrites; through Figure 5 As shown in curve (b), the plastic strain of this alloy at room temperature exceeds 10%, and the room temperature compressive strength is 2750 MPa. Figure 6 Figure (a) shows the engineering stress-strain curve of the alloy under ultra-high temperature compression at 1600℃, which shows that it has a compressive strength of 659MPa at 1600℃.
[0062] Example 3:
[0063] Preparation of Ta 51 Nb 8.5 Mo 8.5 W 17 C 15 A eutectic carbide-reinforced tantalum alloy. The specific steps are as follows:
[0064] (1) Raw material preparation: The alloy smelting raw materials used in this invention are high-purity (≥99.9%) Ta, Nb, Mo and W elemental particles. The surface oxide scale of the raw materials is removed by means of grinding wheels, and they are cleaned by ultrasonic vibration in alcohol. High-purity graphite is mechanically crushed into smaller particles, and carbon particles with a size of about 1 mm are screened out by metal sieve. 19.580 g of Ta particles, 1.676 g of Nb particles, 1.730 g of Mo particles, 6.631 g of W particles and 0.382 g of C particles are weighed (the atomic percentage of Ta / Nb / Mo / W / C is 51:8.5:8.5:17:15).
[0065] (2) Vacuum Arc Melting: Place the C particles at the bottom of the water-cooled crucible in the vacuum arc melting furnace, and then place the Nb particles, Mo particles, Ta particles, and W particles into the crucible in order of increasing melting point. Evacuate the sample chamber until the vacuum level is higher than 5 × 10⁻⁶. -3 After Pa, high-purity argon gas with a purity of 99.999% is introduced as a protective gas and arc-ignition medium. The melting current is 350-450A to ensure that all raw materials can be completely melted. The melting is carried out 8 times, and the electric arc is maintained for 2 minutes during each melting process. Before each melting, the ingot is flipped and tilted at 40°. Finally, it is rapidly cooled to room temperature to obtain a tantalum alloy ingot with uniform composition.
[0066] Figure 3 The curve (c) represents the Ta prepared in Example 2. 51 Nb 8.5 Mo 8.5 W 17 C 15 The XRD pattern of the tantalum alloy composition shows that the prepared tantalum alloy is mainly composed of a refractory high-entropy alloy phase with a BCC structure and a carbide phase with an HCP structure; its microstructure is mainly composed of a eutectic structure consisting of alternating micro / nano-scale lamellar alloy phases and carbide phases, such as... Figure 3 (b) and Figure 4 As shown in (b); this alloy composition has a compressive strength exceeding 2500 MPa at room temperature, while also possessing 16% plasticity, such as Figure 5 As shown in (c); Ta 51 Nb 8.5 Mo 8.5 W 17 C 15 The tantalum alloy exhibits a compressive strength exceeding 632 MPa at 1600°C, such as... Figure 6 As shown in (b).
[0067] Example 4:
[0068] Preparation of Ta 48 Nb8Mo8W16 C 20 Composition: Tantalum alloy. The specific steps are as follows:
[0069] (1) Raw material preparation: The alloy smelting raw materials used in this invention are high-purity (≥99.9%) Ta, Nb, Mo and W elemental particles. The surface oxide scale of each elemental particle is removed by means of grinding wheel, etc., and each elemental particle is cleaned by ultrasonic vibration in alcohol. High-purity graphite is mechanically crushed into smaller particles, and C particles with a size of about 3 mm are screened out by metal screening. 19.477 g of Ta particles, 1.667 g of Nb particles, 1.730 g of Mo particles, 6.596 g of W particles and 0.539 g of C particles are weighed (the atomic percentage of Ta / Nb / Mo / W / C is 48:8:8:16:20).
[0070] (2) Vacuum Arc Melting: Place the C particles at the bottom of the water-cooled crucible in the vacuum arc melting furnace, and then place the Nb particles, Mo particles, Ta particles, and W particles into the crucible in order of increasing melting point. Evacuate the sample chamber until the vacuum level is higher than 5 × 10⁻⁶. -3 After Pa, high-purity argon gas with a purity of 99.999% is introduced as a protective gas and arc-ignition medium. The melting current is 350-450A to ensure that all raw materials can be completely melted. The melting is carried out 6 times, and the arc is maintained for 2 minutes during each melting process. Before each melting, the ingot is flipped and tilted at 45°. Finally, it is rapidly cooled to room temperature to obtain a tantalum alloy ingot with uniform composition.
[0071] Figure 2 The middle curve (d) represents the Ta prepared in Example 3. 48 Nb8Mo8W 16 C 20 The XRD pattern of the tantalum alloy composition shows that the prepared refractory high-entropy alloy is mainly composed of a refractory high-entropy alloy phase with a BCC structure and a carbide phase with an HCP structure; observations were performed using SEM and EBSD, as shown in... Figure 3 (c) and Figure 4 As shown in (c), its microstructure mainly consists of primary carbide phases and eutectic carbide phases distributed in a network pattern between the primary phases; through Figure 5 As can be seen from the curve (d), the compressive strength of this alloy at room temperature is close to 2500 MPa, and the room temperature plasticity is 5%. Figure 6 (c) shows the engineering stress-strain curve of the alloy under ultra-high temperature compression at 1600℃, which shows that it has a compressive strength of 734MPa at 1600℃.
[0072] The foregoing has provided a detailed description of a eutectic carbide-reinforced tantalum alloy and its preparation method, as provided in the embodiments of this application. The descriptions of the embodiments above are merely for the purpose of helping to understand the method and core ideas of this application; furthermore, those skilled in the art will recognize that, based on the ideas of this application, there will be changes in the specific implementation methods and application scope. Therefore, the content of this specification should not be construed as a limitation of this application.
[0073] Certain terms are used in the specification and claims to refer to specific components. Those skilled in the art will understand that hardware manufacturers may use different names to refer to the same component. This specification and claims do not distinguish components based on differences in name, but rather on differences in function. The terms "comprising" and "including" used throughout the specification and claims are open-ended and should be interpreted as "comprising / including but not limited to". "Approximately" means that within an acceptable margin of error, those skilled in the art can solve the technical problem and substantially achieve the technical effect within a certain margin of error. The following descriptions in the specification are preferred embodiments for carrying out this application; however, these descriptions are for the purpose of illustrating the general principles of this application and are not intended to limit the scope of this application. The scope of protection of this application shall be determined by the appended claims.
[0074] It should also be noted that the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a product or system comprising a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a product or system. Without further limitation, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the product or system that includes said element.
[0075] It should be understood that the term "and / or" used in this article is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this article generally indicates that the preceding and following related objects have an "or" relationship.
[0076] The foregoing description illustrates and describes several preferred embodiments of this application. However, as previously stated, it should be understood that this application is not limited to the forms disclosed herein and should not be construed as excluding other embodiments. It can be used in various other combinations, modifications, and environments, and can be altered within the scope of the application concept described herein through the foregoing teachings or techniques or knowledge in related fields. Any modifications and variations made by those skilled in the art that do not depart from the spirit and scope of this application should be within the protection scope of the appended claims.
Claims
1. A eutectic carbide-reinforced tantalum alloy, characterized in that, The eutectic carbide-reinforced tantalum alloy is prepared by vacuum arc melting, and its chemical formula is: Ta a Nb b Mo c W d C e Where 40≤a≤60at%, 6≤b≤10at%, 6≤c≤10 at%, 10≤d≤20at%, 0<e≤20at%, and a+b+c+d+e=100%. The eutectic carbide-reinforced tantalum alloy has a body-centered cubic structure and a close-packed hexagonal structure. The body-centered cubic structure is a multi-principal-element alloy phase. The close-packed hexagonal structure is a high-entropy carbide phase. The multi-principal-element alloy phase is a solid solution composed of Ta, Nb, Mo, and W elements. The high-entropy carbide phase is a (Ta,Nb,Mo,W)₂C solid solution containing Ta, Nb, Mo, and W. Among them, the proportion of eutectic carbide structure in the microstructure is controlled by changing the C element content. As the added C element content increases from 0 to 15 at% and then to 20 at%, the microstructure of the alloy changes from hypoeutectic to eutectic and then to hypereutectic.
2. The eutectic carbide-reinforced tantalum alloy according to claim 1, characterized in that, When a=54, b=9, c=9, d=18, and e=10, the chemical formula of the eutectic carbide-reinforced tantalum alloy is Ta. 54 Nb9Mo9W 18 C 10 Its room temperature compressive strength is greater than 2500 MPa, its room temperature compressive plastic strain is greater than 10%, and its compressive strength at 1600℃ is 659 MPa.
3. The eutectic carbide-reinforced tantalum alloy according to claim 1, characterized in that, When a=51, b=8.5, c=8.5, d=17, and e=15, the chemical formula of the eutectic carbide-reinforced tantalum alloy is Ta. 51 Nb 8.5 Mo 8.5 W 17 C 15 Its room temperature compressive strength is greater than 2500 MPa, its room temperature compressive plastic strain is greater than 15%, and its compressive strength at 1600℃ is 632 MPa.
4. The eutectic carbide-reinforced tantalum alloy according to claim 1, characterized in that, When a=48, b=8, c=8, d=16, and e=20, the chemical formula of the eutectic carbide-reinforced tantalum alloy is Ta. 48 Nb8Mo8W 16 C 20 Its room temperature compressive plastic strain is 5%, and its compressive strength at 1600℃ is 734MPa.
5. The eutectic carbide-reinforced tantalum alloy according to claim 1, characterized in that, When a=57, b=9.5, c=9.5, d=19, and e=5, the chemical formula of the eutectic carbide-reinforced tantalum alloy is Ta. 57 Nb 9.5 Mo 9.5 W 19 C5; its room temperature compressive plastic strain is 14%.
6. A method for preparing the eutectic carbide-reinforced tantalum alloy as described in any one of claims 1-5, characterized in that, The method specifically includes the following steps: S1) Ingredients: Pre-treat the raw materials Ta, Nb, Mo, W and C to obtain raw materials Ta, Nb, Mo, W and C that meet the required proportions and quality. S2) Arrange the raw materials weighed in S1) in the order of low melting point raw materials at the bottom and high melting point raw materials at the top; S3) Alloy melting: The raw materials placed in S2) are subjected to multiple alloy melting processes under vacuum conditions and in an inert gas. Before each melting process, the ingot is flipped and tilted at 40°~60° to finally obtain a eutectic carbide-reinforced tantalum alloy.
7. The method according to claim 6, characterized in that, The eutectic carbide-reinforced tantalum alloy prepared by the method has a room temperature compressive strength greater than 2250 MPa, a room temperature compressive plastic strain of not less than 5%, and a compressive strength of not less than 600 MPa at 1600℃.
Citation Information
Patent Citations
High-temperature-resistant refractory high-entropy alloy and preparation method thereof
CN112609118A
Refractory high-entropy alloy powder material, preparation method and application of refractory high-entropy alloy powder material in additive manufacturing
CN114871425A