A method for determining the free carbon content of boron carbide
By combining primary and secondary oxidation with heat treatment, and utilizing an infrared heating device and a carbon dioxide detector, the cumbersome and inaccurate problems of free carbon detection in boron carbide have been solved, enabling rapid and accurate determination of free carbon content.
Patent Information
- Application Number
- CN202410021923.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-08
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-01-08
AI Technical Summary
Existing methods for detecting free carbon in boron carbide are cumbersome, time-consuming, and not precise enough. They cannot directly measure the free carbon content and suffer from large detection errors and low accuracy.
A method combining primary and secondary oxidation with heat treatment was adopted. Boron carbide samples were treated at different temperatures using an infrared heating device with automatic protection. After carbon dioxide was generated, it was rapidly detected online using a carbon dioxide infrared detector. The free carbon content was calculated using A/D conversion and calculation software.
It enables rapid and accurate detection of free carbon in boron carbide, with small detection error, short detection time, and results consistent with standard samples, making it suitable for quality control of boron carbide.
Smart Images

Figure CN117805052B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of gas elemental analysis and testing technology, specifically relating to a method for determining the free carbon content in boron carbide. Background Technology
[0002] Boron carbide, as a representative material of cemented carbide, is widely used in abrasive molds and high-hardness ceramics. In existing technologies, boron carbide powder is mostly produced by high-temperature sintering, high-speed airflow grinding, or ball milling, followed by step-by-step separation. The carbon element in boron carbide typically exists in two forms: free carbon and combined carbon. Free carbon is carbon existing in its elemental form. During the refining process of boron carbide powder, the free carbon content increases with the grinding time, severely affecting the quality of the boron carbide powder. The free carbon content has a certain impact on the performance of boron carbide alloys, therefore it needs to be strictly controlled.
[0003] Currently, methods for detecting free carbon in boron carbide, both domestically and internationally, can be divided into chemical methods and instrumental methods. Chemical methods primarily employ standard methods such as GB / T 2490 or GB / T 16555.2. The characteristic of chemical methods is that free carbon is determined through sample ashing; however, the analytical process is cumbersome, difficult to master, and involves waste liquid pollution and treatment. Furthermore, the detection time for a single sample is typically 5–8 hours, resulting in very low detection efficiency. Instrumental methods usually employ a tube furnace infrared absorber with computer-controlled temperature rise. For example, Chinese patent CN103063602A involves weighing an appropriate amount of sample and placing it into a tube furnace, slowly raising the furnace temperature from 100℃ to 900℃, maintaining constant temperature at both the high and low points, and then calculating the free carbon content using the weight difference. However, this instrumental method is an indirect measurement, not a direct measurement of free carbon content, and therefore has the drawback of significant error.
[0004] Existing instrumental methods also employ infrared carbon-sulfur analyzers for detection. These methods utilize high-frequency furnaces, which cannot precisely control temperature and can only test total carbon content, not directly measure free carbon content. Furthermore, to ensure sufficient carbide content during boron carbide detection, existing technologies typically add excess boron. Boron oxidizes at relatively low temperatures (around 300°C), forming an oxide film, resulting in slow release or incomplete oxidation of free carbon in the short term. This leads to low detection accuracy, and both existing technologies and instruments cannot directly detect the free carbon release rate. Summary of the Invention
[0005] The purpose of this invention is to provide a method for determining the free carbon content in boron carbide. The method provided by this invention can achieve rapid online detection with small detection error.
[0006] To achieve the objectives of this invention, the following technical solutions are provided:
[0007] A method for determining the free carbon content in boron carbide includes the following steps:
[0008] The boron carbide to be tested is subjected to a first-stage oxidation to obtain the first oxidation product; the temperature of the first-stage oxidation is 100-300℃.
[0009] The first oxidation product is mixed with water and subjected to heat treatment, followed by solid-liquid separation. The resulting solid material is dried to obtain pretreated boron carbide. The heat treatment temperature is 70–95°C.
[0010] The pretreated boron carbide is subjected to secondary oxidation to obtain pure boron carbide and carbon dioxide;
[0011] The amount of carbon dioxide generated is detected, and the content of free carbon in the boron carbide to be tested is obtained based on the amount of carbon dioxide generated.
[0012] Preferably, the primary oxidation time is 3 to 5 minutes.
[0013] Preferably, the first-stage oxidation is carried out in the presence of oxygen, and the oxygen flow rate for the first oxidation is 0.5 to 5 L / min.
[0014] Preferably, the temperature of the secondary oxidation is 650–950°C and the time is 0.5–5 min.
[0015] Preferably, the secondary oxidation is carried out in the presence of oxygen, and the oxygen flow rate for the second oxidation is 0.5 to 5 L / min.
[0016] Preferably, the instruments used for the primary oxidation and secondary oxidation are independent infrared heating devices with automatic protection.
[0017] Preferably, the heat treatment time is 0.5 to 15 minutes.
[0018] Preferably, the drying temperature is 105–130°C and the time is 1–60 min.
[0019] Preferably, the instrument for detecting the amount of carbon dioxide generated is a carbon dioxide infrared detector.
[0020] Preferably, the free carbon content in the boron carbide to be tested is 0.1–20 wt.%.
[0021] This invention provides a method for determining the free carbon content in boron carbide, comprising the following steps: subjecting the boron carbide to be tested to primary oxidation to obtain a first oxidation product; the temperature of the primary oxidation is 100–300°C; mixing the first oxidation product with water, performing heat treatment, followed by solid-liquid separation, and drying the resulting solid material to obtain pretreated boron carbide; subjecting the pretreated boron carbide to secondary oxidation to obtain pure boron carbide and carbon dioxide; detecting the amount of carbon dioxide generated, and determining the free carbon content in the boron carbide to be tested based on the amount of carbon dioxide generated. This invention oxidizes the free boron in the boron carbide to be tested into boron oxide through primary oxidation, removes potentially interfering boron through heat treatment, and finally converts the free carbon in the boron carbide into carbon dioxide through secondary oxidation. This facilitates the conversion of the collected carbon dioxide into a detection signal recognizable by hardware via a detector. The detection signal is converted by an AD converter and calculated by software, allowing for direct and accurate determination of the free carbon content and release rate in the boron carbide to be tested, thereby achieving rapid online detection of the free carbon content in boron carbide. Furthermore, the instruments used for the primary and secondary oxidation processes described in this invention are infrared heating devices with automatic protection, which can achieve precise heating of boron carbide. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1 This is a process flow diagram for determining the free carbon content in boron carbide according to the present invention. Detailed Implementation
[0024] This invention provides a method for determining the free carbon content in boron carbide, comprising the following steps:
[0025] The boron carbide to be tested is subjected to a first-stage oxidation to obtain the first oxidation product; the temperature of the first-stage oxidation is 100-300℃.
[0026] The first oxidation product was mixed with water and subjected to heat treatment. After solid-liquid separation, the resulting solid material was dried to obtain pretreated boron carbide.
[0027] The pretreated boron carbide is subjected to secondary oxidation to obtain pure boron carbide and carbon dioxide;
[0028] The amount of carbon dioxide generated is detected, and the content of free carbon in the boron carbide to be tested is obtained based on the amount of carbon dioxide generated.
[0029] This invention involves primary oxidation of boron carbide to obtain a first oxidation product. In this invention, method calibration is first performed, preferably by: determining a free carbon standard substance, and measuring the free carbon content in boron carbide according to the method described in this invention. The measured value is then calibrated using a single-point correction method. In this invention, the free carbon content of the national standard substance for boron carbide is preferably 0.436%, 0.932%, and 3.02%. In this invention, the free carbon content in the boron carbide to be tested is preferably 0.1–20 wt.%, more preferably 0.436–3.02 wt.%, and most preferably 0.932 wt.%. In this invention, the temperature of the primary oxidation is 100–300°C, preferably 200°C; the time is preferably 3–5 min. In this invention, the primary oxidation is preferably carried out in the presence of oxygen. In this invention, the oxygen flow rate for the primary oxidation is preferably 0.5–5 L / min, more preferably 1–3 L / min; the oxygen purity is preferably 99.5–99.999%, more preferably 99.999%. In this invention, the instrument used for the primary oxidation is preferably an infrared heating device with automatic protection; the infrared heating device with automatic protection is preferably the one with automatic protection described in Chinese Patent CN201621148446.X. In this invention, the free boron in the boron carbide to be tested is oxidized to boron oxide through primary oxidation.
[0030] After obtaining the first oxidation product, the present invention mixes the first oxidation product with water, performs heat treatment, and then performs solid-liquid separation. The resulting solid material is dried to obtain pretreated boron carbide. In the present invention, the water is preferably deionized water. In the present invention, the mass ratio of the first oxidation product to water is preferably 1:100 to 5000, more preferably 1:1000 to 2000. In the present invention, the temperature of the heat treatment is preferably 70 to 95°C, more preferably 85 to 90°C; the time is preferably 0.5 to 15 min, more preferably 5 to 10 min. In the present invention, the heat treatment is preferably carried out under stirring conditions; the stirring rate is preferably 60 to 600 r / min, more preferably 80 to 120 r / min. In the present invention, the heat treatment removes the boron oxide generated by the oxidation of free boron in the boron carbide to be tested after the first-stage oxidation.
[0031] The present invention does not specifically limit the method of solid-liquid separation; any method well known to those skilled in the art can be used. In the present invention, the drying temperature is preferably 105–130°C, more preferably 120°C; the drying time is preferably 1–60 min, more preferably 10–20 min.
[0032] In this invention, the first oxidation product is preferably weighed after drying. The weighing instrument used in this invention is preferably an electronic balance. The mass of the first oxidation product is denoted as m and is used as one of the parameters in subsequent calculations.
[0033] After obtaining pretreated boron carbide, the present invention performs secondary oxidation on the pretreated boron carbide to obtain pure boron carbide and carbon dioxide. In the present invention, the temperature of the secondary oxidation is preferably 650–950°C, more preferably 650–780°C; the time is preferably 0.5–5 min, more preferably 3 min. In the present invention, the secondary oxidation is preferably carried out in the presence of oxygen. In the present invention, the oxygen flow rate of the secondary oxidation is preferably 0.5–5 L / min, more preferably 1–3 L / min; the oxygen purity is preferably 99.5–99.999%, more preferably 99.999%. In the present invention, the instrument used for the secondary oxidation is preferably an infrared heating device with automatic protection; the infrared heating device with automatic protection is preferably the same as the device described above. In the present invention, the free carbon in the pretreated boron carbide is oxidized to carbon dioxide through secondary oxidation.
[0034] After obtaining pure boron carbide and carbon dioxide, this invention detects the amount of carbon dioxide generated, and obtains the content of free carbon in the boron carbide to be tested based on the amount of carbon dioxide generated. In this invention, the instrument used to detect the generation of carbon dioxide is preferably a carbon dioxide infrared detector; the carbon dioxide infrared detector is preferably a carbon dioxide pyroelectric sensor.
[0035] In this invention, after detecting the amount of carbon dioxide generated, the detection signal is converted by an A / D converter and calculated by calculation software. The preferred specific steps of the A / D conversion and calculation software calculation are as follows: a reference voltage is obtained as the starting point of the vertical axis Y, i.e., the horizontal line of Y = reference voltage is used as the zero line; when carbon dioxide gas passes through the carbon dioxide infrared detector, the voltage acquired by the carbon dioxide infrared detector changes, the carbon dioxide infrared detector records the voltage signal acquired in real time, and converts the analog signal into a digital signal through an A / D converter. The A / D converter then transmits the digital signal to a host computer, which is equipped with calculation software. The calculation software uses the version registered by the applicant, registration number 2023SR1028332; the calculation software plots points based on the detection signal, and finally obtains a time-voltage curve on the calculation software, then calculates the area S enclosed by the curve and the zero line. The free carbon content is proportional to S / m, where m is the weighed mass of the first oxidation product; after calibration using a standard sample, the free carbon content in the boron carbide to be tested can be determined.
[0036] To further illustrate the present invention, the method for determining the free carbon content in boron carbide provided by the present invention will be described in detail below with reference to the accompanying drawings and embodiments, but these should not be construed as limiting the scope of protection of the present invention.
[0037] Example 1
[0038] according to Figure 1 The process flow diagram describes the measurement of free carbon content in boron carbide, and the specific steps are as follows:
[0039] 0.2g of boron carbide to be tested (free carbon content of 0.436%) was placed in a crucible and pushed into an infrared heating device with automatic protection by a cylinder. Oxygen with a purity of 99.99% and an oxygen flow rate of 1L / min was introduced and oxidized at 250℃ for 5 minutes to obtain 0.22g of the first oxidation product, which was then removed.
[0040] 0.22g of the first oxidation product and 200g of water were mixed and placed in a hot reactor. The mixture was heat-treated at 95°C and a stirring rate of 80r / min for 10min. After filtration, the solid product was dried at 120°C for 10min. The mixture was weighed using an electronic balance to obtain 0.1118g of free carbon and boron carbide.
[0041] 0.1118g of the mixture was placed in a crucible and propelled into an infrared heating device with automatic protection using a cylinder. Oxygen with a purity of 99.99% and a flow rate of 1L / min was introduced, and secondary oxidation was performed at 850℃ for 5 minutes, oxidizing the free carbon in the mixture into carbon dioxide. The amount of carbon dioxide generated in the second oxidation product was detected using a carbon dioxide infrared detector. The specific steps were as follows: First, a reference voltage was obtained as the starting point of the ordinate Y, i.e., the horizontal line Y = reference voltage, which was used as the zero line; when carbon dioxide gas passed through the detector, the voltage obtained by the carbon dioxide infrared detector increased. The carbon dioxide infrared detector records the voltage signal acquired in real time and converts the analog signal into a digital signal through an A / D converter. The A / D converter then transmits the digital signal to the host computer, which contains calculation software (registration number 2023SR1028332). The calculation software plots points based on the detection signal and finally obtains a time-voltage curve. The area S enclosed by the curve and the zero line is then calculated. The free carbon content is directly proportional to S / m, where m is the weighed mass. After calibration using a standard sample, the free carbon content in the boron carbide to be tested can be determined.
[0042] The test results are shown in Table 1.
[0043] Table 1. Test results of free carbon in boron carbide as described in Example 1.
[0044]
[0045]
[0046] As shown in Table 1, the data obtained by this method are consistent with the indicated content of free carbon in the standard sample, and the detection time is about 30 minutes.
[0047] Example 2
[0048] 0.1g of boron carbide (free carbon content of 3.02%) to be tested was placed in a crucible and pushed into an infrared heating device with automatic protection by a cylinder. Oxygen with a purity of 99.99% and an oxygen flow rate of 3L / min was introduced and oxidized at 300℃ for 5 minutes to obtain 0.11g of the first oxidation product, which was then removed.
[0049] 0.11g of the first oxidation product and 150g of water were mixed and placed in a hot reactor. The mixture was heat-treated at 95°C and a stirring rate of 80r / min for 10min. After filtration, the solid product was dried at 120°C for 10min and weighed using an electronic balance to obtain 0.0835g of pretreated boron carbide.
[0050] 0.0835g of pretreated boron carbide was placed in a crucible and pushed into an infrared heating device with automatic protection by a cylinder. Oxygen with a purity of 99.99% and a flow rate of 3L / min was introduced, and secondary oxidation was carried out at 650℃ for 5min. The amount of carbon dioxide generated in the second oxidation product was detected by a carbon dioxide infrared detector, and the content of free carbon was calculated by calculation software. The calculation method was the same as in the example.
[0051] The test results are shown in Table 2.
[0052] Table 2 shows the test results of free carbon in boron carbide described in Example 2.
[0053]
[0054] As shown in Table 2, the test results are consistent with the labeled content in the standard sample, and the test time is 35 min.
[0055] Table 3. Total carbon and free carbon content in boron carbide standard samples
[0056]
[0057]
[0058] As shown in Table 3, the detection method provided by this invention has high measurement accuracy, with a maximum standard deviation of 0.007%, which is far below the requirements in the standard sample certificate (maximum standard deviation of 0.13%), and is suitable for the determination of boron carbide.
[0059] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, and not all embodiments. People can obtain other embodiments based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for determining the free carbon content in boron carbide, characterized in that, Includes the following steps: The boron carbide to be tested is subjected to a first-stage oxidation to obtain the first oxidation product; the temperature of the first-stage oxidation is 100~300℃. The first oxidation product is mixed with water and subjected to heat treatment, followed by solid-liquid separation. The resulting solid material is dried to obtain pretreated boron carbide. The heat treatment temperature is 70~95℃. The pretreated boron carbide is subjected to a secondary oxidation to obtain pure boron carbide and carbon dioxide; the temperature of the secondary oxidation is 650~950℃ and the time is 0.5~5min. The amount of carbon dioxide generated is detected, and the content of free carbon in the boron carbide to be tested is obtained based on the amount of carbon dioxide generated.
2. The method according to claim 1, characterized in that, The primary oxidation time is 3-5 minutes.
3. The method according to claim 1 or 2, characterized in that, The primary oxidation is carried out in the presence of oxygen, and the oxygen flow rate of the primary oxidation is 0.5~5 L / min.
4. The method according to claim 1, characterized in that, The secondary oxidation is carried out in the presence of oxygen, and the oxygen flow rate for the secondary oxidation is 0.5~5 L / min.
5. The method according to claim 1, characterized in that, The primary and secondary oxidation processes are performed using independent infrared heating devices with automatic protection.
6. The method according to claim 1, characterized in that, The heat treatment time is 0.5~15 min.
7. The method according to claim 1, characterized in that, The drying temperature is 105~130℃, and the time is 1~60min.
8. The method according to claim 1, characterized in that, The instrument used to detect the amount of carbon dioxide generated is a carbon dioxide infrared detector.
9. The method according to claim 1, characterized in that, The free carbon content in the boron carbide to be tested is 0.1~20 wt.%.
Citation Information
Patent Citations
Method for measuring free carbon and silicon carbide in silicon carbide deoxidizing agent
CN103063602A
Take infrared heating device of automatic protection
CN206136321U
Device and method for measuring content of free carbon in boron carbide
CN106645559A
Method for detecting content of free carbon in blast furnace fly ash
CN111721731A