Epitaxial wafer of light emitting diode and method of manufacturing the same
By introducing a composite buffer layer structure of SiC layer, graphene layer and three-dimensional AlInGaN nucleation layer into the epitaxial wafer of light-emitting diode, the problems of high dislocation density and high stress in the epitaxial layer are solved, thereby improving crystal quality and luminous efficiency.
Patent Information
- Application Number
- CN202311844131.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-29
AI Technical Summary
When growing wurtzite gallium nitride thin films on single-crystal silicon substrates, there are problems such as high dislocation density and high stress in the epitaxial layer, which leads to cracks and poor crystal quality, affecting the luminous efficiency of light-emitting diodes.
A composite buffer layer structure is adopted, including a SiC layer, a graphene layer and a three-dimensional AlInGaN nucleation layer. By growing these layers sequentially on the substrate, the dislocation density is reduced and stress is released, thereby improving the crystal quality.
This effectively reduces the dislocation density of the epitaxial layer, decreases crack formation, and improves the crystal quality of the GaN epitaxial layer, thereby enhancing the luminous efficiency of the light-emitting diode.
Smart Images

Figure CN117810327B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of laser diode technology, and in particular to an epitaxial wafer of a light-emitting diode and its fabrication method. Background Technology
[0002] Over the past three decades, gallium nitride (GaN)-based light-emitting diodes (LEDs) have made significant progress. Compared to traditional lighting methods, GaN-based LEDs have advantages such as low energy consumption, long lifespan, fast response speed, and small size, and have been widely used in liquid crystal display (LCD) backlighting, large-screen displays, and general lighting, greatly improving people's daily lives.
[0003] Fabricating wurtzite gallium nitride (GaN) films on single-crystal silicon substrates is a special case. Silicon substrates belong to the cubic crystal system, while wurtzite GaN belongs to the hexagonal crystal system. The reason wurtzite GaN films can grow on single-crystal silicon substrates is because silicon... <111> In this direction, a similar lattice structure can be provided for hexagonal crystal system growth. Typically, silicon-based gallium nitride (GaN) epitaxial films are prone to cracking and high dislocation density due to the enormous tensile stress they endure. Therefore, heteroepitaxial growth of GaN on a substrate often employs an AlN buffer layer technique. However, this also presents the following problems: First, the large lattice mismatch between the AlN layer and the silicon substrate still generates a large number of dislocations, while the GaN epitaxial layer is subjected to high tensile stress; second, when the high temperature of epitaxial layer growth on the substrate decreases to room temperature, the even greater thermal mismatch between GaN and the silicon substrate causes the GaN epitaxial layer to be subjected to even greater tensile stress, resulting in a large number of cracks. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to provide an epitaxial wafer of a light-emitting diode and a method for preparing the same, which can reduce the dislocation density of the epitaxial layer, release the stress between the substrate and the GaN epitaxial layer, improve the crystal quality of the GaN epitaxial layer, and thus improve the luminous efficiency of the light-emitting diode.
[0005] To address the aforementioned technical problems, the first aspect of the present invention provides an epitaxial wafer for a light-emitting diode, comprising a substrate, and further comprising a composite buffer layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer sequentially stacked on the substrate, wherein the composite buffer layer comprises a SiC layer, a graphene layer, and a three-dimensional AlInGaN nucleation layer grown on the substrate.
[0006] As an improvement to the above scheme, the thickness of the SiC layer is 1–100 nm;
[0007] The thickness of the graphene layer is 10–100 nm;
[0008] The thickness of the three-dimensional AlInGaN nucleation layer is 0.1–1 μm, the Al composition is 0.05–0.5, and the In composition is 0.01–0.1.
[0009] As an improvement to the above scheme, after the graphene layer is grown, it is subjected to nitrogen plasma treatment. The treatment temperature of the nitrogen plasma pretreatment is 800-1000℃ and the treatment pressure is 50-100 torr.
[0010] As an improvement to the above scheme, the thickness ratio of the SiC layer to the graphene layer is 1:(0.8~2).
[0011] As an improvement to the above scheme, the substrate is a Si substrate.
[0012] As an improvement to the above scheme, the growth atmosphere of the SiC layer is CH3Cl3Si and H2, the volume ratio of trichloromethylsilane (CH3Cl3Si) to H2 is 1:(1~20), the growth temperature is 1000~1200℃, and the growth pressure is 10~100 torr.
[0013] As an improvement to the above scheme, the growth radio frequency power of the graphene layer is 15-22W, the chamber pressure is 50-100 torr, the growth temperature is 800-1000℃, and the growth atmosphere is methane (CH4) and H2, with a volume ratio of CH4 to H2 of 1:(1-20).
[0014] As an improvement to the above scheme, the growth temperature of the three-dimensional AlInGaN nucleation layer is 800-1000℃, and the growth pressure is 50-500 torr.
[0015] Accordingly, a second aspect of the present invention provides a method for fabricating an epitaxial wafer of the light-emitting diode, comprising:
[0016] (1) Select a substrate;
[0017] (2) A composite buffer layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially grown on the substrate, wherein the composite buffer layer includes a SiC layer, a graphene layer, and a three-dimensional AlInGaN nucleation layer grown on the substrate.
[0018] As an improvement to the above scheme, after the graphene layer is grown, it is subjected to nitrogen plasma treatment, followed by the growth of a three-dimensional AlInGaN nucleation layer.
[0019] Implementing this invention has the following beneficial effects:
[0020] In this invention, a composite buffer layer is provided between the substrate and the undoped GaN layer to provide nucleation sites for subsequent GaN growth. The composite buffer layer specifically includes a SiC layer, a graphene layer, and a three-dimensional AlInGaN nucleation layer grown on the substrate. This can reduce the dislocation density of the epitaxial layer, release the stress between the substrate and the GaN epitaxial layer, reduce the probability of crack formation in the GaN epitaxial layer, improve the crystal quality of the GaN epitaxial layer, and thus improve the luminous efficiency of the light-emitting diode. Attached Figure Description
[0021] Figure 1 : A schematic diagram of the structure of an epitaxial wafer for a light-emitting diode according to the present invention;
[0022] Figure 2 : A schematic diagram of the structure of the multi-quantum well layer of this invention;
[0023] Figure 3 : A flowchart of the method for fabricating the epitaxial wafer of the light-emitting diode of the present invention;
[0024] Figure reference numerals: 100-substrate; 200-composite buffer layer; 210-SiC layer; 220-graphene layer; 230-three-dimensional AlInGaN nucleation layer; 300-undoped GaN layer; 400-N-type GaN layer; 500-multiple quantum well layer; 600-electron blocking layer; 700-P-type GaN layer. Detailed Implementation
[0025] To make the objectives, technical solutions, and advantages of the present invention clearer, specific embodiments will be described in further detail below.
[0026] To resolve the above issues, please refer to [link / reference]. Figure 1 and Figure 2 The present invention provides an epitaxial wafer for a light-emitting diode, comprising a substrate 100, and further comprising a composite buffer layer 200, an undoped GaN layer 300, an N-type GaN layer 400, a multiple quantum well layer 500, an electron blocking layer 600, and a P-type GaN layer 700 sequentially stacked on the substrate 100, wherein the composite buffer layer 200 comprises a SiC layer 210, a graphene layer 220, and a three-dimensional AlInGaN nucleation layer 230 grown on the substrate 100.
[0027] In this invention, by sequentially stacking SiC layer 210, graphene layer 220 and three-dimensional AlInGaN nucleation layer 230 in the buffer layer from bottom to top, the dislocation density of the epitaxial layer can be effectively reduced, the stress of the substrate 100 and the GaN epitaxial layer can be released, the generation of cracks in the GaN epitaxial layer can be reduced, and the crystal quality of the GaN epitaxial layer can be improved, thereby improving the luminous efficiency of the light-emitting diode.
[0028] The SiC layer 210 prevents the introduced NH3 from reacting with the surface of the substrate 100, and also prevents the substrate 100 from reacting with Ga, thus preventing the "Ga remelting" phenomenon that corrodes the substrate 100 and the epitaxial layer, thereby reducing the defect density of the GaN epitaxial layer. The graphene layer 220 has a good lattice match with the SiC layer 210, and there is a strong interaction between the two, which can change the nucleation density, form effective nucleation sites, promote the subsequent nucleation and growth of GaN, and reduce the dislocation density at the fusion boundary and the stress in the epitaxial layer. Then, a three-dimensional AlInGaN nucleation layer 230 is set on top of it. The migration barrier of GaN on the three-dimensional AlInGaN nucleation layer 230 is low, which can form low-density nucleation islands, which is beneficial to reduce dislocations in the crystal. It can also release the stress caused by the lattice mismatch between the nitride film and the substrate 100 and the thermal stress caused by the mismatch of the coefficient of thermal expansion, and provide nucleation centers with the same orientation as the substrate 100. Furthermore, during the transition from three-dimensional to two-dimensional growth, the penetrating dislocations in the crystal bend and close, thereby reducing the dislocation density in the GaN epitaxial film and further improving the crystal quality of GaN.
[0029] Preferably, the thickness of the SiC layer 210 is 1 to 100 nm, with exemplary thicknesses being 1 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, and 100 nm, but not limited to these. If the SiC layer 210 is too thin, the blocking effect on the reaction between the introduced NH3 and the substrate 100, and between the substrate 100 and Ga, will be weak, damaging the structure of the substrate 100 and the epitaxial layer. If the SiC layer 210 is too thick, it will lead to stress mismatch and easy cracking.
[0030] Preferably, the thickness of the graphene layer 220 is 10–100 nm, with exemplary thicknesses of 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, and 100 nm, but not limited to these. If the thickness of the graphene layer 220 is too thin, there will be fewer effective nucleation sites, which is not conducive to the subsequent deposition of GaN. If the thickness of the graphene layer 220 is too thick, it will reduce its conductivity, increase the operating voltage of the LED, and reduce its luminous efficiency.
[0031] Furthermore, the thickness ratio of the SiC layer 210 to the graphene layer 220 is 1:(0.8-2), with exemplary ratios of 1:0.8, 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, and 1:2, but not limited to these. By controlling the thickness ratio of the SiC layer 210 to the graphene layer 220, it is easier to control the degree of reaction between the Si atoms in the SiC layer 210 and the C atoms in the graphene layer 220 to form strong covalent bonds, which serve as effective nucleation sites and are beneficial for the subsequent nucleation and growth of GaN. If the reaction is too intense, it will lead to a decrease in carrier mobility.
[0032] In some preferred embodiments, after the graphene layer 220 is grown, it is subjected to nitrogen plasma treatment to obtain a nitrided graphene layer 220. This process creates defects on the graphene surface, partially etching the surface. In addition to incorporating into the graphene lattice, N atoms also form bonds with C atoms in the etched areas, forming out-of-plane N-sp atoms on the graphene surface. 3 C-bonds serve as effective nucleation sites, further promoting the subsequent nucleation and growth of GaN.
[0033] Preferably, the thickness of the three-dimensional AlInGaN nucleation layer 230 is 0.1 to 1 μm, and exemplary thicknesses are 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, and 1 μm, but are not limited thereto.
[0034] Furthermore, the Al composition in the three-dimensional AlInGaN nucleation layer 230 is 0.05 to 0.5, with exemplary values of 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, and 0.5, but not limited thereto; and the In composition is 0.01 to 0.1, with exemplary values of 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, and 0.1, but not limited thereto.
[0035] Accordingly, please refer to Figure 3 The present invention also provides a method for fabricating an epitaxial wafer of a light-emitting diode, comprising:
[0036] (1) Provide a substrate 100
[0037] (2) A composite buffer layer, an undoped GaN layer 300, an N-type GaN layer 400, a multi-quantum well layer 500, an electron blocking layer 600, and a P-type GaN layer 700 are grown on the substrate 100, wherein the composite buffer layer 200 includes a SiC layer 210, a graphene layer 220, and a three-dimensional AlInGaN nucleation layer 230 grown on the substrate 100.
[0038] Specifically, the method for fabricating the epitaxial wafer of the light-emitting diode includes:
[0039] S01, Provide a substrate 100;
[0040] Preferably, the substrate 100 can be selected from one of the following: sapphire substrate 100, SiO2 sapphire composite substrate 100, Si substrate 100, silicon carbide substrate 100, gallium nitride substrate 100, and zinc oxide substrate 100; more preferably, it is a Si substrate 100. The Si substrate 100 selected in this invention has advantages over the sapphire substrate 100, which has high hardness, poor thermal conductivity, and poor electrical properties, due to its large size and low cost. Furthermore, it simplifies the substrate 100 thinning process and reduces costs.
[0041] S02. Deposit a composite buffer layer 200 on the substrate 100. The composite buffer layer 200 includes a SiC layer 210, a graphene layer 220, and a three-dimensional AlInGaN nucleation layer 230.
[0042] Preferably, the SiC layer 210 is grown by CVD in a growth atmosphere of CH3Cl3Si and H2, with a volume ratio of CH3Cl3Si to H2 of 1:(1 to 20), such as 1:1, 1:3, 1:5, 1:7, 1:9, 1:11, 1:13, 1:15, 1:17, 1:19, or 1:20, but not limited thereto.
[0043] Furthermore, the growth temperature of the SiC layer 210 is 1000–1200°C, exemplarily 1000°C, 1050°C, 1100°C, 1150°C, and 1200°C, but not limited thereto. The growth pressure is 10–100 torr, exemplarily 10 torr, 20 torr, 30 torr, 40 torr, 50 torr, 60 torr, 70 torr, 80 torr, 90 torr, and 100 torr, but not limited thereto.
[0044] Preferably, the graphene layer 220 is grown using PECVD technology in a growth atmosphere of methane (CH4) and H2, with a volume ratio of CH4 to H2 of 1:(1 to 20), such as 1:1, 1:2, 1:4, 1:6, 1:8, 1:10, 1:12, 1:14, 1:16, 1:18, or 1:20, but not limited thereto.
[0045] Furthermore, the growth radio frequency power of the graphene layer 220 is 15-22W, exemplarily 15W, 16W, 17W, 18W, 19W, 20W, 21W, 225W, but not limited thereto; the cavity pressure is 50-100 torr, exemplarily 50 torr, 55 torr, 60 torr, 65 torr, 70 torr, 75 torr, 80 torr, 85 torr, 90 torr, 95 torr, 100 torr, but not limited thereto; and the growth temperature is 800-1000℃, exemplarily 800℃, 850℃, 900℃, 950℃, 1000℃, but not limited thereto.
[0046] In some preferred embodiments, after the graphene layer 220 is grown, it is subjected to nitrogen plasma treatment. The nitrogen plasma pretreatment temperature is 800-1000°C and the treatment pressure is 50-100 torr.
[0047] Preferably, the growth temperature of the three-dimensional AlInGaN nucleation layer 230 is 800-1000℃, exemplarily 800℃, 850℃, 900℃, 950℃, and 1000℃, but not limited thereto, and the growth pressure is 50-500 torr, exemplarily 50 torr, 100 torr, 150 torr, 200 torr, 250 torr, 300 torr, 350 torr, 400 torr, 450 torr, and 500 torr, but not limited thereto.
[0048] S03, Deposit an undoped GaN layer 300 on the composite buffer layer 200;
[0049] Preferably, the thickness of the undoped GaN layer 300 is 1–5 μm, the growth temperature is 1050–1200 °C, and the growth pressure is 100–600 torr. The undoped GaN layer 300 has a higher growth temperature and lower pressure, resulting in GaN crystals of superior quality. Furthermore, as the GaN thickness increases, compressive stress is released through stacking faults, reducing line defects, improving crystal quality, and lowering reverse leakage current. However, increasing the GaN layer thickness consumes a significant amount of Ga source material, greatly increasing the epitaxial cost of LEDs. Therefore, currently, LED epitaxial wafers are typically grown with undoped GaN to a thickness of 2–3 μm, which not only saves production costs but also provides GaN material with high crystal quality.
[0050] S04. Deposit an N-type GaN layer 400 on the undoped GaN layer 300;
[0051] Preferably, the thickness of the N-type GaN layer 400 is 2–3 μm, the growth temperature is 1050–1200 °C, the pressure is 100–600 torr, and the Si doping concentration is 1 × 10⁻⁶.19 ~5×10 19 atoms / cm 3 The N-type GaN layer 400 provides sufficient electrons for LED light emission, and the resistivity of the N-type GaN layer 400 is higher than that of the transparent electrode on the P-type GaN. Therefore, sufficient Si doping can effectively reduce the resistivity of the N-type GaN layer 400. In addition, sufficient thickness of N-type GaN can effectively release stress and improve the luminous efficiency of the LED.
[0052] S05, Deposit a multi-quantum-well layer 500 on the N-type GaN layer 400;
[0053] Preferably, the multiple quantum well layer 500 is composed of alternating stacked InGaN quantum well layers and AlGaN quantum barrier layers, with 6 to 12 stacking periods. The InGaN quantum well layer has a thickness of 2 to 5 nm, an In composition of 0.2 to 0.3%, a growth temperature of 790 to 810 °C, and a growth pressure of 50 to 300 torr. The AlGaN quantum barrier layer has a thickness of 5 to 15 nm, an Al composition of 0.01 to 0.1%, a growth temperature of 800 to 900 °C, and a growth pressure of 50 to 300 torr. Multiple quantum wells are regions where electrons and holes recombine. A well-designed structure can significantly increase the overlap of electron and hole wave functions, thereby improving the luminous efficiency of the LED device.
[0054] S06. Deposit an electron blocking layer 600 on the multi-quantum-well layer 500;
[0055] Preferably, the electron blocking layer 600 is an AlInGaN electron blocking layer 600 with a thickness of 10-40 nm, wherein the Al content is 0.005-0.1, the In content is 0.01-0.2, the growth temperature is 900-1000 °C, and the growth pressure is 100-300 torr.
[0056] S07. Deposit a P-type GaN layer 700 on the electron blocking layer 600;
[0057] Preferably, the thickness of the p-type GaN layer 700 is 10–50 nm, and the Mg doping concentration is 1 × 10⁻⁶. 19 ~1×10 21 atoms / cm 3 The growth temperature is 900–1050℃, and the growth pressure is 100–600 torr. Excessive Mg doping concentration will damage the crystal quality, while insufficient doping concentration will affect the hole concentration.
[0058] In summary, the epitaxial wafer of the present invention can reduce the dislocation density of the epitaxial layer, release the stress between the substrate 100 and the GaN epitaxial layer, reduce the generation of cracks in the GaN epitaxial layer, improve the crystal quality of the GaN epitaxial layer, and improve the luminous efficiency of the light-emitting diode.
[0059] It should be noted that in this invention, high-purity NH3 is used as the N source, trimethylgallium (TMGa) or triethylgallium (TEGa) is used as the gallium source, trimethylindium (TMIn) is used as the indium source, trimethylaluminum (TMAl) is used as the aluminum source, silane (SiH4) is used as the Si source, magnesium pyrocene (CP2Mg) is used as the dopant Mg source, and CH3Cl3Si is used as the C source for epitaxial growth.
[0060] The present invention will be further described below with reference to specific embodiments:
[0061] Example 1
[0062] This embodiment provides an epitaxial wafer for a light-emitting diode, including a substrate 100, and further including a composite buffer layer 200, an undoped GaN layer 300, an N-type GaN layer 400, a multiple quantum well layer 500, an electron blocking layer 600, and a P-type GaN layer 700 sequentially stacked on the substrate 100. The composite buffer layer 200 includes a SiC layer 210, a graphene layer 220, and a three-dimensional AlInGaN nucleation layer 230 grown on the substrate 100.
[0063] It is prepared by the following method:
[0064] S01, Provide a Si substrate 100;
[0065] S02, SiC layer 210, graphene nitride layer 220 and three-dimensional AlInGaN nucleation layer 230 are sequentially deposited on Si substrate 100;
[0066] A SiC layer 210 with a thickness of 50 nm was grown on a Si substrate 100 using CVD technology. The growth atmosphere was CH3Cl3Si and H2 with a volume ratio of 1:10, the growth temperature was 1100℃, and the growth pressure was 50 torr. Subsequently, a graphene layer 220 was grown on the SiC layer 210 using PECVD technology. The growth atmosphere was CH4 and H2 with a volume ratio of 1:10, the RF power was 17 W, the chamber pressure was 75 torr, the growth temperature was 900℃, and the thickness was 45 nm. Finally, a three-dimensional AlInGaN nucleation layer 230 with a thickness of 0.6 μm, an Al composition of 0.3%, an In composition of 0.05%, was deposited on the graphene layer 220 at a growth temperature of 950℃ and a growth pressure of 150 torr.
[0067] S03, Deposit an undoped GaN layer 300 on the three-dimensional AlInGaN nucleation layer 230;
[0068] The thickness of the undoped GaN layer 300 is 2.5 μm, the growth temperature is 1100℃, and the growth pressure is 150 torr.
[0069] S04. Deposit an N-type GaN layer 400 on the undoped GaN layer 300;
[0070] The thickness of the N-type GaN layer 400 is 2.5 μm, and the Si doping concentration is 2.5 × 10⁻⁶. 19 atoms / cm 3 The growth temperature is 1120℃ and the growth pressure is 100 torr.
[0071] S05. Deposit a multi-quantum-well layer 500 on the N-type GaN layer 400;
[0072] The multi-quantum-well layer 500 consists of alternating stacked InGaN quantum well layers and AlGaN quantum barrier layers, with a stacking period of 10. The InGaN quantum well layer has a thickness of 3.5 nm, an In composition of 0.22, a growth temperature of 795 °C, and a growth pressure of 200 torr. The AlGaN quantum barrier layer has a thickness of 9.8 nm, an Al composition of 0.05, a growth temperature of 855 °C, and a growth pressure of 200 torr.
[0073] S06. Deposit an electron blocking layer 600 on the multi-quantum well layer 500;
[0074] The electron blocking layer 600 is an AlInGaN layer with a thickness of 15 nm, wherein the Al composition is 0.05 and the In composition is 0.01, the growth temperature is 965℃, and the growth pressure is 200 Tor.
[0075] S07. Deposit a P-type GaN layer 700 on the electron blocking layer 600;
[0076] The thickness of the p-type GaN layer 700 is 15 nm, and the Mg doping concentration is 2 × 10⁻⁶. 20 atoms / cm 3 The growth temperature was 985℃ and the growth pressure was 200 torr.
[0077] Example 2
[0078] This embodiment provides an epitaxial wafer for a light-emitting diode, which is basically the same as that in Embodiment 1, except that:
[0079] The thickness of the graphene layer 220 is 35 nm.
[0080] Example 3
[0081] This embodiment provides an epitaxial wafer for a light-emitting diode, which is basically the same as that in Embodiment 1, except that:
[0082] Subsequently, a graphene layer 220 was grown on the SiC layer 210 using PECVD technology. The growth atmosphere was CH4 and H2 with a volume ratio of 1:10. The radio frequency power was 17W, the chamber pressure was 75 torr, and the growth temperature was 900℃. The graphene was then pretreated with nitrogen plasma to form a nitrided graphene layer 220 with a thickness of 45nm.
[0083] Comparative Example 1
[0084] This comparative example provides an epitaxial wafer for a light-emitting diode, which is basically the same as that in Example 3, except that:
[0085] The buffer layer is an AlN buffer layer with a thickness of 15nm.
[0086] Comparative Example 2
[0087] This comparative example provides an epitaxial wafer for a light-emitting diode, which is basically the same as that in Example 3, except that:
[0088] The composite buffer layer 200 includes a graphene layer 220 and a three-dimensional AlInGaN nucleation layer 230 grown on the substrate 100.
[0089] Comparative Example 3
[0090] This comparative example provides an epitaxial wafer for a light-emitting diode, which is basically the same as that in Example 3, except that:
[0091] The composite buffer layer 200 includes a SiC layer 210 and a three-dimensional AlInGaN nucleation layer 230 grown on the substrate 100.
[0092] Comparative Example 4
[0093] This comparative example provides an epitaxial wafer for a light-emitting diode, which is basically the same as that in Example 3, except that:
[0094] The composite buffer layer 200 includes a SiC layer 210 and a graphene layer 220 grown on the substrate 100.
[0095] Performance testing:
[0096] The epitaxial wafers of the light-emitting diodes obtained in Examples 1-3 and Comparative Examples 1-4 were fabricated into 10mil*24mil chips using the same chip process conditions. 300 LED chips were randomly selected from each chip and tested at 120mA / 60mA. The test results are shown in the table below. The improvement in luminous efficiency was calculated based on Comparative Example 1.
[0097] Table 1. Test results of Examples 1-3 and Comparative Examples 1-4
[0098] Light efficiency improvement (%) XRD 002 / 102 Example 1 2.8 90 / 180 Example 2 3.3 88 / 173 Example 3 5 85 / 165 Comparative Example 1 / 105 / 195 Comparative Example 2 1.5 95 / 182 Comparative Example 3 1 100 / 193 Comparative Example 4 1.2 97 / 190
[0099] The experimental data above show that optimizing the structure of the composite buffer layer, which includes a SiC layer, a graphene layer, and a three-dimensional AlInGaN nucleation layer grown on the substrate, can reduce the dislocation density of the epitaxial layer, release the stress between the substrate and the GaN epitaxial layer, reduce the generation of cracks in the GaN epitaxial layer, improve the crystal quality of the GaN epitaxial layer, and improve the luminous efficiency of the light-emitting diode.
[0100] The above description is merely a preferred embodiment of the present invention and should not be construed as limiting the scope of the invention. Therefore, any equivalent variations made in accordance with the claims of the present invention are still within the scope of the present invention.
Claims
1. An epitaxial wafer for a light-emitting diode, comprising a substrate, characterized in that, It also includes a composite buffer layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer sequentially stacked on the substrate, wherein the composite buffer layer includes a SiC layer, a graphene layer, and a three-dimensional AlInGaN nucleation layer grown on the substrate. The thickness of the SiC layer is 1~100nm; The thickness of the graphene layer is 10~100nm; The thickness of the three-dimensional AlInGaN nucleation layer is 0.1~1μm, the Al composition is 0.05~0.5, and the In composition is 0.01~0.
1. After the graphene layer is grown, it is subjected to nitrogen plasma treatment. The nitrogen plasma pretreatment temperature is 800~1000℃ and the treatment pressure is 50~100 torr.
2. The epitaxial wafer of the light-emitting diode as described in claim 1, characterized in that, The thickness ratio of the SiC layer to the graphene layer is 1:(0.8~2).
3. The epitaxial wafer of the light-emitting diode as described in claim 1, characterized in that, The substrate is a Si substrate.
4. The epitaxial wafer of the light-emitting diode as described in claim 1, characterized in that, The growth atmosphere of the SiC layer is CH3Cl3Si and H2, the volume ratio of CH3Cl3Si to H2 is 1:(1~20), the growth temperature is 1000~1200℃, and the growth pressure is 10~100 torr.
5. The epitaxial wafer of the light-emitting diode as described in claim 1, characterized in that, The growth radio frequency power of the graphene layer is 15~22W, the chamber pressure is 50~100 torr, the growth temperature is 800~1000℃, and the growth atmosphere is CH4 and H2 with a volume ratio of CH4 to H2 of 1:(1~20).
6. The epitaxial wafer of the light-emitting diode as described in claim 1, characterized in that, The growth temperature of the three-dimensional AlInGaN nucleation layer is 800~1000℃, and the growth pressure is 50~500 torr.
7. A method for fabricating an epitaxial wafer of a light-emitting diode as described in any one of claims 1 to 6, characterized in that, include: (1) Select a substrate; (2) A composite buffer layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially grown on the substrate, wherein the composite buffer layer includes a SiC layer, a graphene layer, and a three-dimensional AlInGaN nucleation layer grown on the substrate.
8. The method for fabricating an epitaxial wafer of a light-emitting diode as described in claim 7, characterized in that, After the graphene layer is grown, it undergoes nitrogen plasma treatment, followed by the growth of a three-dimensional AlInGaN nucleation layer.
Citation Information
Patent Citations
Light emitting diode epitaxial wafer and preparation method thereof
CN116387426A