Preparation method and application of melamine boric acid modified chitosan / zinc borate double-coated red phosphorus flame retardant
By preparing a melamine-boric acid modified chitosan/zinc borate double-coated red phosphorus flame retardant, the flammability problem of polyethylene materials was solved, achieving high-efficiency flame retardancy and good compatibility, which is suitable for LLDPE/EVA cable materials.
Patent Information
- Application Number
- CN202410017823.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-05
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-01-05
AI Technical Summary
Existing polyethylene materials are flammable and generate a large amount of heat. Commonly used flame retardants, such as halogenated compounds, release harmful gases, while red phosphorus flame retardants are unstable and difficult to apply effectively in cable materials.
An organic-inorganic dual-coated red phosphorus flame retardant was prepared by using melamine-boric acid modified chitosan and zinc borate as the encapsulation material and red phosphorus as the core material. The synergistic effect of chitosan and zinc borate was utilized to improve the instability and surface properties of red phosphorus.
The prepared flame retardant has good thermal stability and high flame retardant efficiency, and can achieve UL94 V-0 rating in LLDPE/EVA cable materials, preventing melt dripping and reducing dense smoke emissions, while maintaining good compatibility and dispersibility.
Smart Images

Figure CN117820730B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of flame retardant technology of polymer materials, specifically relating to the preparation and application of a melamine-boric acid modified chitosan / zinc borate double-coated red phosphorus flame retardant. Background Technology
[0002] Power cables are a crucial component for energy transmission. Due to their complex working environment, flammable insulation materials, and operating conditions, fires involving power cables are common. Polyethylene (PE) materials are widely used in the wire and cable industry for manufacturing sheaths, underlays, and insulation layers due to their excellent processing, insulation, and mechanical properties. However, PE materials are highly flammable and generate a large amount of heat, easily producing numerous molten droplets. Their limiting oxygen index is only 17-22%, so flame-retardant treatment is essential when PE materials are used as wire and cable sheaths, underlays, and insulation layers. Flame retardants used with PE typically include halogenated, nitrogen-based, phosphorus-based, and metal hydroxides. With the development of environmental and health concepts, halogenated flame retardants are gradually being phased out due to the release of harmful gases during combustion. Green, harmless, halogen-free, and low-toxicity flame retardants have become a research hotspot in recent years.
[0003] Red phosphorus (RP) is a phosphorus-based flame retardant with good flame retardant effect and high flame retardant efficiency. However, red phosphorus is chemically unstable, and it usually needs to be modified when used as a flame retardant.
[0004] This invention proposes to prepare an organic-inorganic dual-coated red phosphorus flame retardant by using melamine-boric acid modified chitosan and zinc borate as the encapsulation material and red phosphorus as the core material. This flame retardant utilizes both the environmentally friendly material chitosan and the inorganic flame retardant zinc borate to improve the instability and surface properties of red phosphorus, and fully leverages the good flame-retardant synergistic effect between red phosphorus, melamine-boric acid modified chitosan, and zinc borate. It is expected to be applied in LLDPE / EVA cable materials and achieve good flame-retardant effects. Summary of the Invention
[0005] The purpose of this invention is to provide a preparation and application of a melamine-boric acid modified chitosan / zinc borate double-coated red phosphorus flame retardant. The resulting flame retardant has advantages such as high flame retardant efficiency, good smoke suppression effect, good thermal stability, and good compatibility with matrix materials, and has broad application prospects in LLDPE / EVA cable materials.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A method for preparing a melamine-boric acid modified chitosan / zinc borate double-coated red phosphorus flame retardant includes the following steps: (1) Chitosan (CS) is dissolved in a dilute acid solution of a certain concentration and a chitosan solution is obtained by magnetic stirring and ultrasonic vibration; (2) Prepare a 1 mol / L hydrochloric acid solution with concentrated hydrochloric acid, weigh a certain amount of melamine (Mel) and add it to an appropriate amount of deionized water, and stir it with a magnetic force to form a suspension. Heat it to 90°C and slowly add the prepared hydrochloric acid solution to the suspension to obtain a transparent melamine hydrochloric acid solution. (3) Add an appropriate amount of borax to the melamine hydrochloric acid solution obtained in step (2) and react at 90°C for 1 hour to obtain a melamine borate suspension. (4) Slowly add the chitosan solution obtained in step (1) to the melamine borate suspension obtained in step (3), and react at 90°C for 12 hours to obtain melamine borate modified chitosan suspension. (5) Add a certain amount of red phosphorus and an appropriate amount of dispersant to the melamine boric acid modified chitosan suspension obtained in step (4), and increase the magnetic stirring speed to make the red phosphorus evenly dispersed in the suspension. (6) Add a mixture of zinc salt and zinc oxide to the suspension obtained in step (5), react at 90°C for 7 hours, add an appropriate amount of ammonia water, adjust the pH value to neutral, let it stand for a certain period of time, vacuum filter, dry the filtered product, crush it, and pass it through a 200-mesh sieve to obtain a white powder product, which is the melamine boric acid modified chitosan / zinc borate double-coated red phosphorus flame retardant.
[0007] Further, the acid mentioned in step (1) is one or more of acetic acid, citric acid, and hydrochloric acid, the mass percentage concentration of the dilute acid solution is 1-2 wt%, and the amount used is 100 mL / 2 g chitosan.
[0008] Further, in step (2), the amount of melamine used is 6.3-18.9g / 10g chitosan, the amount of deionized water used is 200mL / 10g melamine, the amount of hydrochloric acid solution used is 50mL / 6.3g melamine, and the magnetic stirring speed is 300-500rpm.
[0009] Furthermore, the amount of borax used in step (3) is 19.1 g / 6.3 g melamine.
[0010] Further, in step (5), the amount of red phosphorus used is 2-8g / 4g chitosan, the dispersant is one or more of sodium dodecylbenzenesulfonate, sodium hexametaphosphate, and sodium dodecyl sulfate, the amount of dispersant used is 1-2 wt% of the amount of red phosphorus used, and the stirring speed is 600-800 rpm.
[0011] Further, the zinc salt mentioned in step (6) is one or more of zinc sulfate, zinc nitrate, and zinc chloride, and the amount of zinc salt used is: Zn in the zinc salt 2+ When prepared with borax at a molar ratio of 2:5, the amount of zinc oxide used is: zinc oxide to zinc salt (Zn) 2+The mixture is prepared at a molar ratio of 1:7, aged for 12-24 hours, dried at 60-80℃ for 12-24 hours.
[0012] Application: The melamine-boric acid modified chitosan / zinc borate double-coated red phosphorus flame retardant described above is used in LLDPE / EVA cable materials.
[0013] Chitosan (CS), also known as deacetylated chitin, is a polysaccharide polymer obtained from chitin through deacetylation. It is a white powder and a renewable raw material. In flame retardants, chitosan acts as a gas source, releasing N2 and NH3 when heated, thus diluting flammable gases. Furthermore, in dilute acid solutions, chitosan's positive charge and charge density are enhanced, leading to electrostatic attraction with negatively charged flame retardants. This provides the necessary conditions for chitosan to be used as a shell-coated red phosphorus flame retardant. Zinc borate (ZB) is an environmentally friendly non-halogenated flame retardant with good dispersibility, low specific gravity, small particle size, non-toxicity, low water solubility, and high thermal stability. Besides being used alone as a flame retardant, zinc borate can also act as a synergist for red phosphorus. When used together, they promote char formation, isolate oxygen, and hinder the volatilization of flammable gases.
[0014] This invention proposes to prepare an organic-inorganic dual-coated red phosphorus flame retardant by using melamine-boric acid modified chitosan and zinc borate as the encapsulation material and red phosphorus as the core material. This flame retardant utilizes both the environmentally friendly material chitosan and the inorganic flame retardant zinc borate to improve the instability and surface properties of red phosphorus, and fully leverages the good flame-retardant synergistic effect between red phosphorus, melamine-boric acid modified chitosan, and zinc borate. It is expected to be applied in LLDPE / EVA cable materials and achieve good flame-retardant effects.
[0015] The significant advantages of this invention are: (1) The preparation of melamine boric acid modified chitosan / zinc borate double-coated red phosphorus flame retardant is completed in the aqueous phase. The preparation process is simple, the raw materials are widely available, and it is easy to realize industrial production.
[0016] (2) The flame retardant prepared by the present invention has good thermal stability and dispersibility, and can give full play to the good flame retardant synergistic effect between red phosphorus, melamine boric acid modified chitosan and zinc borate. It has high flame retardant efficiency. When the addition amount in LLDPE / EVA cable material is 24wt%, the flame retardant level can reach UL94 V-0 level, and it can effectively prevent melt dripping and reduce dense smoke emission. Attached Figure Description
[0017] Figure 1 This is a process flow diagram of the present invention; Figure 2 These are the FT-IR images of the flame retardants used in Examples 1 and 2; Figure 3 This is a SEM image of the char layer after combustion of the sample prepared in Example 1; Figure 4 This is a SEM image of the char layer after combustion of the sample prepared in Example 2; Figure 5 This is a SEM image of the char layer after combustion of the sample prepared in Example 1; Figure 6 This is a SEM image of the carbon layer after combustion of the sample prepared in Example 2. Detailed Implementation
[0018] To make the content of this invention easier to understand, the technical solution of this invention will be further described below with reference to specific embodiments, but this invention is not limited thereto.
[0019] Example 1: Weigh 2g of acetic acid into a beaker and add deionized water to prepare a 1wt% acetic acid solution. Add 4g of chitosan to the acetic acid solution and stir magnetically until the chitosan is completely dissolved. Weigh 6.3g (0.05mol) of melamine and 200mL of deionized water and pour them into a three-necked flask equipped with a magnetic stirrer and a reflux condenser. Under stirring at 300 rpm, raise the temperature of the water bath to 90℃ and add 50mL of 1mol / L hydrochloric acid until the solution becomes clear, forming a melamine hydrochloric acid solution. Weigh 19.1g (0.05mol) of borax and add it to the melamine hydrochloric acid solution. React at 90℃ for 1h to form suspension A. Slowly add the chitosan dissolved in the acetic acid solution dropwise to the three-necked flask containing suspension A using a separatory funnel, and increase the stirring speed to 700rpm. React at 90℃ for 12h to form suspension B. 0.12 g of sodium dodecylbenzenesulfonate and 6 g of red phosphorus were weighed and added to suspension B, and dispersed evenly at 700 rpm. 6.1 g (0.021 mol) of zinc sulfate heptahydrate and 0.25 g (0.003 mol) of zinc oxide were then weighed and added to the three-necked flask containing suspension B. The reaction was carried out at the same temperature and speed for 7 hours. The pH of the reaction suspension was adjusted to neutral with an appropriate amount of ammonia, aged for 12 hours, and then vacuum filtered. The filtered product was dried in a 70°C oven for 12 hours, crushed, and passed through a 200-mesh sieve to obtain melamine-boric acid modified chitosan / zinc borate double-coated red phosphorus flame retardant.
[0020] Example 2: Weigh 3g of citric acid into a beaker and add deionized water to prepare a 1wt% citric acid solution. Add 6g of chitosan to the citric acid solution and stir magnetically until the chitosan is completely dissolved. Weigh 6.3g (0.05mol) of melamine and 200mL of deionized water and pour them into a three-necked flask equipped with a magnetic stirrer and a reflux condenser. Under stirring at 300rpm, raise the temperature of the water bath to 90℃ and add 50mL of 1mol / L hydrochloric acid until the solution becomes clear, generating a melamine hydrochloric acid solution. Weigh 19.1g (0.05mol) of borax and add it to the melamine hydrochloric acid solution. React at 90℃ for 1h to form suspension A. Slowly add the chitosan dissolved in acetic acid solution dropwise to the three-necked flask containing suspension A using a separatory funnel, and increase the stirring speed to 700rpm. React at 90℃ for 12h to form suspension B. 0.16 g of sodium hexametaphosphate and 8 g of red phosphorus were weighed and added to suspension B, and dispersed evenly at 700 rpm. 6.25 g (0.021 mol) of zinc nitrate hexahydrate and 0.25 g (0.003 mol) of zinc oxide were then weighed and added to the three-necked flask containing suspension B. The reaction was carried out at the same temperature and speed for 7 hours. The pH of the reaction suspension was adjusted to neutral with an appropriate amount of ammonia water, aged for 12 hours, and then vacuum filtered. The filtered product was dried in a 70℃ oven for 12 hours, crushed, and passed through a 200-mesh sieve to obtain melamine-boronic acid modified chitosan / zinc borate double-coated red phosphorus flame retardant.
[0021] Pure LLDPE / EVA splines: 50 parts by weight of LLDPE and 50 parts by weight of EVA were extruded and granulated using a twin-screw extruder and then injection molded to produce flame retardant test specimens (length × width × thickness = 130 mm × 10 mm × 3.2 mm) and mechanical property test specimens. The vertical burning test rating was UL94 NR, with an LOI value of 17.2%, exhibiting significant dripping, a melt flow rate of 2.2 g / 10 min, an elongation at break of 657.2%, a tensile strength of 12.7 MPa, and an impact strength of 62.8 kJ / m². 2 The residual char rate of the flame-retardant sample after full carbonization in a muffle furnace at 800℃ was 0.8%.
[0022] Application Example 1: 24 parts of the flame retardant obtained in Example 1 were weighed and mixed with 38 parts of LLDPE and 38 parts of EVA (by weight). The mixture was then extruded and granulated using a twin-screw extruder and injection molded to obtain flame retardant performance test specimens (length × width × thickness = 130 mm × 10 mm × 3.2 mm) and mechanical property test specimens. Compared with LLDPE / EVA, its vertical burning test rating reached UL94 V-0, the LOI value increased to 29.7%, there was no dripping phenomenon, the melt flow rate was 2.1 g / 10 min, the elongation at break was 535.5%, the tensile strength was 14.7 MPa, and the impact strength was 63.5 kJ / m. 2 The residual char rate of the flame-retardant sample after full carbonization in a muffle furnace at 800 °C was 17.4%.
[0023] Application Example 2: 24 parts of the flame retardant obtained in Example 2 were weighed and mixed with 38 parts of LLDPE and 38 parts of EVA (by weight). The mixture was then extruded and granulated using a twin-screw extruder and injection molded to obtain flame retardant performance test specimens (length × width × thickness = 130 mm × 10 mm × 3.2 mm) and mechanical property test specimens. Compared with LLDPE / EVA, its vertical burning test rating reached UL94 V-0, the LOI value increased to 30.3%, there was no dripping phenomenon, the melt flow rate was 2.2 g / 10 min, the elongation at break was 525.5%, the tensile strength was 15.1 MPa, and the impact strength was 64.5 kJ / m. 2 The residual char rate of the flame-retardant sample after full carbonization at 800 °C in a muffle furnace was 17.8%.
[0024] Comparative Application Example 1 12 parts of commercially available microencapsulated red phosphorus flame retardant and 12 parts of zinc borate flame retardant were weighed and mixed with 38 parts of LLDPE and 38 parts of EVA (by weight). The mixture was then extruded and granulated using a twin-screw extruder and injection molded to obtain flame retardant performance test specimens (length × width × thickness = 130 mm × 10 mm × 3.2 mm) and mechanical property test specimens. Compared with LLDPE / EVA, its vertical burning test rating was UL94V-2, the LOI value increased to 26.9%, the melt flow rate was 2.1 g / 10min, the elongation at break was 219.7%, the tensile strength was 10.2 MPa, and the impact strength was 48.9 kJ / m². 2 The residual char rate of the flame-retardant sample after full carbonization at 800 °C in a muffle furnace was 15.6%.
[0025] Comparative Application Example 2 24 parts of a self-made melamine-boric acid modified chitosan / zinc borate flame retardant (red phosphorus and dispersant were not added in Example 1, but the rest were the same as in Example 1) were weighed and mixed with 38 parts of LLDPE and 38 parts of EVA (by weight). The mixture was then extruded and granulated using a twin-screw extruder and injection molded to obtain flame retardant performance test specimens (length × width × thickness = 130 mm × 10 mm × 3.2 mm) and mechanical property test specimens. The specimens were not self-extinguishing after being lit. Compared with LLDPE / EVA, its vertical burning test rating was UL94NR, the LOI value was increased to 23.2%, the melt flow rate was 1.9 g / 10min, the elongation at break was 368.2%, the tensile strength was 13.2 MPa, and the impact strength was 61.2 kJ / m. 2 The residual char rate of the flame-retardant sample after full carbonization in a muffle furnace at 800 °C was 14.7%.
[0026] The test results above show that commercially available red phosphorus flame retardants and zinc borate have low flame retardant efficiency in LLDPE / EVA cable materials. Furthermore, due to the poor compatibility between the flame retardants and the matrix resin, the tensile strength, impact strength, and elongation at break of the flame-retardant composite material are significantly reduced. The flame-retardant sample with self-made melamine-boric acid modified chitosan / zinc borate lacks an acid source (P), resulting in very low flame retardant efficiency and failing to achieve the desired flame retardant effect when used in LLDPE / EVA cable materials. In contrast, the organic / inorganic dual-coated red phosphorus flame retardant prepared in this invention exhibits high flame retardant efficiency in LLDPE / EVA cable materials due to the good synergistic flame retardant effect between red phosphorus, melamine-boric acid modified chitosan, and zinc borate. Moreover, the flame retardant prepared in this invention has good compatibility and dispersibility in the LLDPE / EVA matrix, thus having minimal impact on the mechanical properties of the composite material.
[0027] Figure 2 These are the FT-IR spectra of chitosan, flame retardant 1 prepared in Example 1, and flame retardant 2 prepared in Example 2. As can be seen from the spectra, the prepared flame retardants show a high FT-IR index at 3350 cm⁻¹. -1 The absorption peak of the NH stretching vibration of melamine appeared nearby; at 1187 cm⁻¹ -1 The characteristic absorption peak at 802 cm⁻¹ is the internal bending vibration peak of BOH. -1 The characteristic absorption peak that appears is B. (3) -O external bending vibration peak; wavenumber 537 cm⁻¹ -1 This is the Zn-O stretching vibration peak. The above analysis indicates that the melamine-boric acid modified chitosan / zinc borate double-coated red phosphorus flame retardant was successfully prepared.
[0028] Figures 3-6The images show SEM images of Application Example 1, Application Example 2, Comparative Application Example 1, and Comparative Application Example 2. As can be seen from the images, the samples prepared in Application Example 1 and Application Example 2 formed a uniform and dense char layer after combustion, providing excellent heat and oxygen insulation and exhibiting superior flame-retardant effects. However, the char layer of the sample prepared in Comparative Application Example 1 showed certain micro-cracks after combustion, and the flame-retardant sample prepared in Comparative Application Example 2 showed small pores in its char layer. Neither could provide complete heat and oxygen insulation, resulting in poor flame-retardant effects.
[0029] To make the content of this invention easier to understand, the technical solutions of this invention have been further explained above in conjunction with specific embodiments. However, this invention is not limited thereto. All equivalent changes or modifications made in accordance with the spirit and essence of this invention are within the scope of protection of this invention.
Claims
1. A method for preparing a melamine-boric acid modified chitosan / zinc borate double-coated red phosphorus flame retardant, characterized in that: Includes the following steps: (1) Chitosan is dissolved in a dilute acid solution of a certain concentration, and a chitosan solution is obtained by magnetic stirring and ultrasonic vibration; (2) Prepare a 1 mol / L hydrochloric acid solution with concentrated hydrochloric acid, weigh a certain amount of melamine and add it to an appropriate amount of deionized water, and stir it with a magnetic force to form a suspension. Heat it to 90°C and slowly add the prepared hydrochloric acid solution to the suspension to obtain a transparent melamine hydrochloric acid solution. (3) Add an appropriate amount of borax to the melamine hydrochloric acid solution obtained in step (2) and react at 90°C for 1 hour to obtain a melamine borate suspension. (4) Slowly add the chitosan solution obtained in step (1) to the melamine borate suspension obtained in step (3), and react at 90°C for 12 hours to obtain melamine borate modified chitosan suspension. (5) Add a certain amount of red phosphorus and an appropriate amount of dispersant to the melamine boric acid modified chitosan suspension obtained in step (4), and increase the magnetic stirring speed to make the red phosphorus evenly dispersed in the suspension. (6) Add a mixture of zinc salt and zinc oxide to the suspension obtained in step (5), react at 90°C for 7 hours, add an appropriate amount of ammonia water, adjust the pH value to neutral, let it stand for a certain period of time, vacuum filter, dry the filtered product, crush it, and pass it through a 200-mesh sieve to obtain a white powder product, which is melamine boric acid modified chitosan / zinc borate double-coated red phosphorus flame retardant; The amount of melamine used in step (2) is 6.3-18.9 g / 10 g chitosan; The amount of borax used in step (3) is 19.1 g / 6.3 g melamine; The amount of red phosphorus used in step (5) is 2-8g / 4g chitosan.
2. The preparation method according to claim 1, characterized in that: The acid mentioned in step (1) is one or more of acetic acid, citric acid, and hydrochloric acid. The mass percentage concentration of the dilute acid solution is 1-2 wt%, and the amount used is 100 mL / 2 g chitosan.
3. The preparation method according to claim 1, characterized in that: In step (2), the amount of deionized water used is 200 mL / 10 g melamine, the amount of hydrochloric acid solution used is 50 mL / 6.3 g melamine, and the magnetic stirring speed is 300-500 rpm.
4. The preparation method according to claim 1, characterized in that: The dispersant mentioned in step (5) is one or more of sodium dodecylbenzenesulfonate, sodium hexametaphosphate, and sodium dodecyl sulfate. The amount of dispersant used is 1-2 wt% of the amount of red phosphorus used, and the stirring speed is 600-800 rpm.
5. The preparation method according to claim 1, characterized in that: The zinc salt mentioned in step (6) is one or more of zinc sulfate, zinc nitrate, and zinc chloride, and the amount of zinc salt used is: Zn in the zinc salt 2+ When prepared with borax at a molar ratio of 2:5, the amount of zinc oxide used is: zinc oxide to zinc salt (Zn) 2+ The mixture is prepared at a molar ratio of 1:7, aged for 12-24 hours, dried at 60-80℃ for 12-24 hours.
6. A melamine-boric acid modified chitosan / zinc borate double-coated red phosphorus flame retardant prepared by the preparation method according to any one of claims 1-5.
7. The application of the melamine-boric acid modified chitosan / zinc borate double-coated red phosphorus flame retardant as described in claim 6 in LLDPE / EVA cable materials.
Citation Information
Patent Citations
Melamine-modified lignin / magnesium aluminum hydroxide double-coated red phosphorus flame retardant and application thereof in cable materials
CN109054099A
High-flame-retardant low-release cable material and preparation method thereof
CN116693967A