Liquid crystalline polyester composition, process for its preparation and use thereof

By combining liquid crystal polyester composition with carbon fiber and hollow glass microspheres, the anisotropy and density of the materials are controlled, solving the problem of inconsistent acoustic performance of liquid crystal polyester materials during injection molding, and realizing low-cost, high-performance acoustic diaphragm molding.

CN117820828BActive Publication Date: 2026-11-20ZHUHAI WANTONG SPECIAL ENG PLASTICS CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311622560.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-30
Publication Date
2026-11-20
Estimated Expiration
2043-11-30

AI Technical Summary

Technical Problem

Due to the strong anisotropy of existing liquid crystal polyester materials during injection molding, the acoustic performance of speaker products is inconsistent in different directions, causing resonance and distortion. Furthermore, existing composite material molding processes are costly and complex to assemble.

Method used

A liquid crystal polyester composition is used, comprising liquid crystal polyester, carbon fiber and hollow glass microspheres. By controlling the retention length of the carbon fiber and the particle size and compressive strength of the hollow glass microspheres, combined with polyarylate, a low-density, low-anisotropy material is formed, which is suitable for injection molding of audio diaphragms.

Benefits of technology

This achieves low density and low anisotropy of the speaker diaphragm, improving the consistency of acoustic performance and reducing production costs and processing difficulty.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A liquid crystal polyester composition comprises the following components by weight parts: liquid crystal polyester 38-70 parts; carbon fiber 10-20 parts; hollow glass microsphere 10-20 parts; wherein the average retention length of the carbon fiber is 120-150 microns, the diameter range of the hollow glass microsphere is D50=22-28 microns, D90=37-43 microns, the density is 0.40-0.44 g / cm3, and the compressive strength is 7000-9000 Psi; further comprising polyarylate, the content of the polyarylate is 1-15% of the sum of the weight parts of the carbon fiber and the hollow glass microsphere; the polyarylate is bisphenol A type polyarylate, terephthalic acid accounts for 40-60 mol% of dicarboxylic acid units, and m-xylylene dicarboxylic acid accounts for 40-60 mol% of dicarboxylic acid units. The liquid crystal polyester composition has the advantages of good mechanical properties, good thin-wall forming property, low anisotropy and low density, and is suitable for injection molding of acoustic diaphragm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer materials technology, and in particular to a liquid crystal polyester composition, its preparation method, and its application. Background Technology

[0002] LCP materials have highly ordered rod-like molecular chains, with numerous benzene rings and biphenyl structures within the monomers. The molten molecular chains exhibit liquid crystal properties. During injection molding, the high-speed flow of the melt and the extremely rapid cooling rate in the thin-walled mold easily lead to high orientation of the molecular chains. These highly oriented structures result in LCP materials having extremely high tensile modulus in the flow direction, while simultaneously exhibiting lower tensile modulus in the vertical direction, demonstrating anisotropy.

[0003] To achieve a more uniform sound field, loudspeaker products are often shaped like rotating bodies, such as hemispheres, circles, and cones. However, excessive anisotropy can cause inconsistent absorption and vibration in different directions, leading to resonance or noise and causing distortion. Under high-frequency sound wave stimulation, the acoustic defects caused by this anisotropy are amplified, thus reducing the listening experience.

[0004] Patent application CN112351375A discloses a sound mold device with a sandwich structure formed by multi-layer honeycomb panels. By obtaining the properties of low-density, high-rigidity composite materials, it can reduce and suppress distortion and coloration of the sound diaphragm. This process has drawbacks such as the inability to form a single piece, high production cost, and significant impact from assembly results. Summary of the Invention

[0005] The purpose of this invention is to provide a liquid crystal polyester composition with good mechanical properties, good thin-wall formability, low anisotropy, and low density, which is suitable for injection molding of audio diaphragms.

[0006] This invention is achieved through the following technical solution: A liquid crystal polyester composition, characterized in that, by weight, it comprises the following components: 38-70 parts of liquid crystal polyester; 10-20 parts carbon fiber; 10-20 parts of hollow glass microspheres; The carbon fiber has an average retention length of 120-150 micrometers, the hollow glass microspheres have a diameter range of D50=22-28 micrometers and D90=37-43 micrometers, a density of 0.40-0.44 g / cm³, and a compressive strength of 7000-9000 Psi. It also includes polyarylate, the content of which is 1-15% of the sum of the weight parts of carbon fiber and hollow glass microspheres. The polyarylate is a bisphenol A type polyarylate, with terephthalic acid accounting for 40-60 mol% of the dicarboxylic acid units and isophthalic acid accounting for 40-60 mol% of the dicarboxylic acid units.

[0007] This liquid crystal polyester is obtained by polymerizing at least two or more of the following monomers: terephthalic acid, biphenyl, 6-hydroxy-2-naphthoic acid, p-hydroxybenzoic acid, and acetaminophen, through a polycondensation reaction followed by thickening. Preferably, the repeating units of the liquid crystal polyester are derived from p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid.

[0008] The liquid crystal polyester of the present invention is at a temperature greater than 20°C and 1000 -s The melt viscosity under shear rate conditions is 10-50 Pa·s, at 20°C above the melting point, 1000 -s Under shear rate conditions, the test method was based on the determination method of ISO 11443-2021, and the equipment used was a Goettfert high-pressure capillary rheometer, RG20, 1mm test die.

[0009] Preferably, the content of polyarylate is 3-8% of the sum of the weight parts of carbon fiber and hollow glass microspheres.

[0010] More preferably, the content of polyarylate is 5-6% of the sum of the weight parts of carbon fiber and hollow glass microspheres.

[0011] Preferably, in the polyarylate, terephthalic acid accounts for 51-54 mol of the dicarboxylic acid units, and isophthalic acid accounts for 46-49 mol of the dicarboxylic acid units.

[0012] The polyarylate used to achieve the technical objective of this invention can be a commercially available product or a self-made raw material. For self-made materials, the following method can be used: After thoroughly drying bisphenol A diacetate, terephthalic acid, and isophthalic acid at 80-100℃, add them to a reaction vessel in a certain proportion. Vacuum the vessel and purge with nitrogen to ensure all air is expelled. Slowly heat to 110-130℃ and hold for 20-40 minutes to remove moisture. Under nitrogen protection, slowly heat to 230-250℃ and hold until acetic acid distills out. Maintain the vacuum and react until no more acetic acid distills out. Then, rapidly heat to 330-340℃, vacuum the vessel, and stir. Stop stirring after a period of time. During the reaction, the pressure inside the vessel must be maintained at 0.5-0.8 atmospheres.

[0013] The polyarylate of this invention is subjected to a temperature of 335°C and 1000°C. -s Melt viscosity under shear rate conditions: 900-1000 Pa·s, 1000 -s Under shear rate conditions, the test method was based on the determination method of ISO 11443-2021, and the equipment used was a Goettfert high-pressure capillary rheometer, RG20, 1mm test die.

[0014] Preferably, the average retained length of the carbon fiber is 130-140 micrometers. The average length of the carbon fiber that can achieve the purpose of this invention is 4-13 mm. There are no special requirements for the average diameter of the carbon fiber, which is between 4-9 micrometers.

[0015] Preferably, the diameter range of the hollow glass microspheres is D50 = 24-26 micrometers and D90 = 39-41 micrometers. The test method is in accordance with GB / T 19077-2016.

[0016] Depending on actual needs, 0-2 parts of an auxiliary agent may be added, wherein the auxiliary agent is selected from at least one of antioxidants and lubricants. In the technical solution of this invention, the liquid crystal polyester accounts for not less than 45 wt% of the weight of the liquid crystal polyester composition.

[0017] The method for preparing the liquid crystal polyester composition of the present invention includes the following steps: mixing the components evenly according to the formula, granulating by extrusion through a twin-screw extruder, wherein the screw temperature range is 260-310℃ and the rotation speed is 200-600 rpm, to obtain the liquid crystal polyester composition.

[0018] According to existing technology, the retained length of carbon fibers can be adjusted by adjusting the length of the raw carbon fibers and the screw speed.

[0019] The liquid crystal polyester composition of the present invention is used for injection molding of audio diaphragms. For injection molding of audio diaphragms, the liquid crystal polyester composition needs to have a minimum flow length of 25 mm, low anisotropy (transverse / longitudinal stretch difference percentage less than 45%), a density less than 1.20 g / cm³, and preferably higher mechanical properties.

[0020] The present invention has the following beneficial effects: Conventional fiber-reinforced liquid crystal polyester compositions typically use glass fibers. However, this invention has found that wear between the glass fibers and hollow glass microspheres during processing can easily cause the hollow glass microspheres to break, resulting in increased density and high anisotropy. This invention, by controlling the retention length of carbon fibers in the composition, can also achieve low anisotropy at low density while obtaining suitable modulus and thin-wall formability.

[0021] Meanwhile, by exploring the particle size, compressive strength, and density of hollow glass microspheres, this application can reduce the breakage rate of hollow glass microspheres, thereby not only obtaining a liquid crystal polyester composition with high density, but also further reducing anisotropy. Detailed Implementation

[0022] The present invention will now be described in detail with reference to specific embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.

[0023] The raw materials used in this invention are sourced from the following sources: Liquid crystal polyester A: derived from p-hydroxybenzoic acid / 6-hydroxy-2-naphthoic acid, Ueno A5000.

[0024] Liquid crystal polyester B: p-hydroxybenzoic acid / biphenyl / terephthalic acid / isophthalic acid, Polyplastics A950.

[0025] Liquid crystal polyester C: p-hydroxybenzoic acid / 6-hydroxy-2-naphthoic acid / biphenyl / terephthalic acid / acetaminophen, Vicryst R8500.

[0026] Carbon fiber 5-7 mm, purchased from Toho, number average fiber length: 5-7 mm; Carbon fiber 7-9 mm, purchased from Toho, number average fiber length: 7-9 mm; Carbon fiber 3-5 mm, purchased from Toho, number average fiber length: 3-5 mm; Carbon fiber 10-12 mm, purchased from Toho, number average fiber length: 10-12 mm; The hollow glass microspheres below were purchased from Saint-Lite, and raw materials of different particle sizes were obtained through screening (density was tested according to GB / T 21782.3-2008, and compressive strength was tested according to JC / T 2285-2014).

[0027] Hollow glass microspheres A: D50=25 micrometers, D90=40 micrometers, density 0.42g / cm³, compressive strength 8000Psi; Hollow glass microspheres B: D50=22 micrometers, D90=37 micrometers, density 0.43g / cm³, compressive strength 8000Psi; Hollow glass microspheres C: D50=28 micrometers, D90=43 micrometers, density 0.41g / cm³, compressive strength 8000Psi; Hollow glass microspheres: D50=18 micrometers, D90=33 micrometers, density 0.44g / cm³, compressive strength 8000Psi; Hollow glass microspheres E: D50=35 micrometers, D90=46 micrometers, density 0.40g / cm³, compressive strength 8000Psi; Hollow glass microspheres F: D50=30 micrometers, D90=50 micrometers, density 0.38g / cm³, compressive strength 5500Psi; Hollow glass microspheres G: D50=20 micrometers, D90=30 micrometers, density 0.48g / cm³, compressive strength 16000Psi.

[0028] The following is the preparation process for polyarylates: Bisphenol A diacetate, terephthalic acid, and isophthalic acid are thoroughly dried at 90°C and then added to a reaction vessel in a specific ratio. A vacuum is then created and nitrogen is introduced to ensure the removal of air from the vessel. The temperature is slowly raised to 120°C and held for 30 minutes to remove moisture. Under nitrogen protection, the temperature is slowly raised to 240°C and held until acetic acid distills out. The vacuum is maintained, and the reaction continues until no more acetic acid distills out. The temperature is then rapidly raised to 330°C, and the mixture is stirred under vacuum. Stirring is stopped after a certain period of time. The pressure inside the vessel must be maintained at 0.6 atmospheres throughout the reaction.

[0029] Polyarylate A: Bisphenol A / terephthalic acid accounts for 41 mol% of the dicarboxylic acid units, and isophthalic acid accounts for 59 mol% of the dicarboxylic acid units. It is self-made.

[0030] Polyarylate B: Bisphenol A / terephthalic acid accounts for 59 mol% of the dicarboxylic acid units, and isophthalic acid accounts for 41 mol% of the dicarboxylic acid units; self-made.

[0031] Polyarylate C: Bisphenol A / terephthalic acid accounts for 51 mol% of the dicarboxylic acid units, and isophthalic acid accounts for 49 mol% of the dicarboxylic acid units; self-made.

[0032] Polyarylate D: Bisphenol A / terephthalic acid accounts for 54 mol% of the dicarboxylic acid units, and isophthalic acid accounts for 46 mol% of the dicarboxylic acid units; self-made.

[0033] Polyarylate E: Bisphenol A / terephthalic acid accounts for 70 mol% of the dicarboxylic acid units, and isophthalic acid accounts for 30 mol% of the dicarboxylic acid units, prepared in-house.

[0034] Polyarylate F: Bisphenol A / terephthalic acid accounts for 30 mol% of the dicarboxylic acid units, and isophthalic acid accounts for 70 mol% of the dicarboxylic acid units, prepared in-house.

[0035] Preparation method of liquid crystal polyester composition in the examples and comparative examples: According to the formula, the components are mixed evenly and extruded and granulated by a twin-screw extruder. The screw temperature range is 260-310℃ and the rotation speed is 200-600 rpm to obtain the liquid crystal polyester composition.

[0036] Test methods: (1) Test method for carbon fiber retention length in liquid crystal polyester composition: hot press to 0.3 mm film at a melting point above 20°C, and measure the fiber using a microscope.

[0037] (2) Flowability: At an injection temperature above 20℃, an injection pressure of 50 MPa, and an injection speed of 50%, a thin-walled sample with a width of 5 mm and a thickness of 0.4 mm was injection molded, and the flowability was judged based on the flow length.

[0038] (3) Anisotropy: For injection molding of 100×800mm square plates, cut strips along the flow direction and vertical direction and conduct tensile strength tests. The test standard is ISO527-1:2019. The percentage difference between transverse and longitudinal tensile strength = (longitudinal tensile strength - transverse tensile strength) / transverse tensile strength * 100%. The percentage difference between the two can reflect the anisotropy of the material. The larger the difference between the two directions, the stronger the anisotropy.

[0039] (4) Density: After injection molding into standard specimens, the density is measured by the immersion method according to GB / T 1033-1986.

[0040] Table 1: Weight parts of each component and test results of the liquid crystal polyester compositions in Examples 1-7 Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Liquid Crystal Polyester A 55 40 70 55 55 Liquid Crystal Polyester B 55 Liquid crystal polyester C 55 5-7mm carbon fiber 15 15 15 10 20 15 15 Screw speed, revolutions per minute 200 200 200 200 200 200 200 Carbon fiber retention length, micrometers 135 131 137 132 137 130 136 Hollow glass microspheres A 15 15 15 10 20 15 15 Polyarylate A 1.5 1.5 1.5 1 2 0.3 0.9 Liquidity mm 31 28 27 34 25 35 32 Transverse tensile strength, MPa 79 65 70 79 56 62 65 Longitudinal tensile strength, MPa 105 94 98 110 80 89.5 93 Percentage of difference between transverse and longitudinal stretching, % 32.9 44.6 40.0 39.2 42.8 44.3 43.1 Density, g / cm³ 1.14 1.14 1.16 1.15 1.13 1.16 1.15 As can be seen from Examples 1-3, when the repeating units of the preferred liquid crystal polyester are derived from p-hydroxybenzoic acid / 6-hydroxy-2-naphthoic acid, the flowability, tensile strength, percentage difference in transverse / longitudinal tensile strength, and density are the best.

[0041] As can be seen from Examples 1 / 6-10, the addition of polyarylate can significantly improve anisotropy, but it also severely reduces fluidity. Considering the comprehensive performance of processing performance, mechanical properties, and low anisotropy, the optimal amount of polyarylate added is more suitable for preparing acoustic diaphragms, while also exhibiting excellent mechanical properties.

[0042] Table 2: Weight parts of each component and test results of the liquid crystal polyester compositions in Examples 8-13 Example 8 Example 9 Example 10 Example 11 Example 12 Example 13 Liquid Crystal Polyester A 55 55 55 55 55 55 5-7mm carbon fiber 15 15 15 Carbon fiber 7-9 mm 15 3-5 mm carbon fiber 15 Carbon fiber 10-12 mm 15 Screw speed, revolutions per minute 200 200 200 250 150 300 Carbon fiber retention length, micrometers 137 133 135 142 120 148 Hollow glass microspheres A 15 15 15 15 15 15 Polyarylate A 1.8 2.4 4.5 1.5 1.5 1.5 Liquidity 30 29 25 28 34 27 Transverse tensile strength, MPa 80 83 83 83 72 85 Longitudinal tensile strength, MPa 103 100 98 112 98.5 117 Percentage of difference between transverse and longitudinal stretching, % 28.7 20.5 18.1 34.9 36.8 37.6 Density, g / cm³ 1.14 1.15 1.16 1.17 1.16 1.19 As can be seen from Examples 1 / 11-13, the density and the percentage difference between transverse and longitudinal tensile strength are lowest at the preferred carbon fiber retention length.

[0043] Table 3: Weight parts of each component and test results of the liquid crystal polyester compositions in Examples 14-18 Example 14 Example 15 Example 16 Example 17 Example 18 Liquid Crystal Polyester A 55 55 55 55 55 5-7mm carbon fiber 15 15 15 15 15 Screw speed, revolutions per minute 200 200 200 200 200 Carbon fiber retention length, micrometers 132 137 130 135 132 Hollow glass microspheres A 15 15 15 Hollow glass microspheres B 15 Hollow glass microspheres C 15 Polyarylate A 1.5 1.5 Polyarylate B 1.5 Polyarylate C 1.5 Polyarylate D 1.5 Liquidity 30 29 32 33 34 Transverse tensile strength, MPa 75 67 80 82 81 Longitudinal tensile strength, MPa 101 90.5 106 105 103 Percentage of difference between transverse and longitudinal stretching, % 34.7 35.2 32.5 28.0 27.2 Density, g / cm³ 1.13 1.15 1.14 1.14 1.14 As can be seen from Examples 1 / 14 / 15, hollow glass microspheres with the preferred particle size exhibit the best flowability and mechanical properties, and the lowest percentage difference in transverse / longitudinal tensile strength.

[0044] As can be seen from Examples 1 / 16-18, the optimal content of each polyarylate unit results in better mechanical properties, a lower percentage difference in transverse / longitudinal tensile strength, and better flowability.

[0045] Table 4: Weight parts of each component and test results of liquid crystal polyester compositions in Comparative Examples 1-6 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Liquid Crystal Polyester A 55 55 55 55 55 55 5-7mm carbon fiber 15 15 25 5 15 Carbon fiber 10-12 mm 15 Screw speed, revolutions per minute 200 200 200 200 250 200 Carbon fiber retention length, micrometers 131 136 133 139 112 163 Hollow glass microspheres A 15 15 5 25 15 15 Polyarylate A 0 6 1.5 1.5 1.5 1.5 Liquidity 35 19 20 28 30 21 Transverse tensile strength, MPa 63 80 85 52 64 89 Longitudinal tensile strength, MPa 96 94 131 84 95 129 Percentage of difference between transverse and longitudinal stretching, % 52.3 17.5 54.1 61.5 48.4 44.9 Density, g / cm³ 1.14 1.17 1.34 0.99 1.18 1.20 As can be seen from Comparative Example 1 / 2 and Examples 1 / 6-10, when the content of polyarylate is too low, the mechanical properties are poor and the anisotropy is poor; when the content of polyarylate is too high, the fluidity is severely reduced, making it difficult to meet the requirements of injection molding acoustic diaphragms.

[0046] As can be seen from Comparative Example 3 / 4, the content of carbon fiber / hollow glass microspheres is not within the scope of this invention and cannot meet the requirements of injection-molded audio diaphragms.

[0047] Table 5: Weight parts of each component and test results of the liquid crystal polyester compositions of Comparative Examples 7-12 Comparative Example 7 Comparative Example 8 Comparative Example 9 Comparative Example 10 Comparative Example 11 Comparative Example 12 Liquid Crystal Polyester A 55 55 55 55 55 55 5-7mm carbon fiber 15 15 15 15 15 15 Screw speed, revolutions per minute 200 200 200 200 200 200 Carbon fiber retention length, micrometers 135 133 130 138 131 139 Hollow glass microspheres A 15 15 Hollow glass microspheres D 15 Hollow glass microspheres E 15 Hollow glass microspheres F 15 Hollow glass microspheres G 15 Polyarylate A 1.5 1.5 1.5 1.5 Polyarylate E 1.5 Polyarylate F 1.5 Liquidity 33 29 32 28 29 30 Transverse tensile strength, MPa 74 68 70 56 64 69 Longitudinal tensile strength, MPa 106 95 98 82 94 101 Percentage of difference between transverse and longitudinal stretching, % 43.2 39.7 40.0 46.42 46.8 46.3 Density, g / cm³ 1.23 1.22 1.25 1.15 1.14 1.14 As can be seen from Comparative Examples 7-10 and Example 1, if the particle size of the hollow glass microspheres is not within the range of the present invention, the percentage value of the difference between transverse and longitudinal tensile strength and the density are relatively high; if the compressive strength of the hollow glass microspheres is too low, they are easily damaged during processing, resulting in an increase in density; if the compressive strength of the hollow glass microspheres is too high, the anisotropy is severe.

[0048] As can be seen from Comparative Examples 11 / 12, when the content of each unit of polyarylate is not within the scope of the present invention, the percentage difference between transverse and longitudinal tensile strength is large.

Claims

1. A liquid crystal polyester composition, characterized in that, By weight, it includes the following components: 38-70 parts of liquid crystal polyester; 10-20 parts carbon fiber; 10-20 parts of hollow glass microspheres; The average retention length of the carbon fiber is 120-150 micrometers, the diameter range of the hollow glass microspheres is D50=22-28 micrometers, D90=37-43 micrometers, the density is 0.40-0.44 g / cm³, and the compressive strength is 7000-9000 psi. It also includes polyarylate, the content of which is 1-15% of the sum of the weight parts of carbon fiber and hollow glass microspheres; The polyarylate is a bisphenol A type polyarylate, with terephthalic acid accounting for 40-60 mol of the dicarboxylic acid units and isophthalic acid accounting for 40-60 mol of the dicarboxylic acid units.

2. The liquid crystal polyester composition according to claim 1, characterized in that, The repeating units of the liquid crystal polyester are derived from p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid.

3. The liquid crystal polyester composition according to claim 1, characterized in that, The content of polyarylate is 3-8% of the sum of the weight parts of carbon fiber and hollow glass microspheres.

4. The liquid crystal polyester composition according to claim 3, characterized in that, The content of polyarylate is 5-6% of the sum of the weight parts of carbon fiber and hollow glass microspheres.

5. The liquid crystal polyester composition according to claim 1, characterized in that, In polyarylates, terephthalic acid accounts for 51-54 mol of dicarboxylic acid units, and isophthalic acid accounts for 46-49 mol of dicarboxylic acid units.

6. The liquid crystal polyester composition according to claim 1, characterized in that, The average retention length of carbon fibers is 130-140 micrometers.

7. The liquid crystal polyester composition according to claim 1, characterized in that, The diameter range of hollow glass microspheres is D50=24-26 micrometers and D90=39-41 micrometers.

8. The liquid crystal polyester composition according to claim 1, characterized in that, The product also includes 0-2 parts by weight of additives, wherein the additives are selected from at least one of antioxidants and lubricants.

9. A method for preparing the liquid crystal polyester composition according to any one of claims 1-8, characterized in that, The process includes the following steps: mixing the components evenly according to the formula, and granulating them by extrusion through a twin-screw extruder to obtain a liquid crystal polyester composition.

10. The use of the liquid crystal polyester composition according to any one of claims 1-8, characterized in that, Used for injection molding of speaker diaphragms.

Citation Information

Patent Citations

  • Sound system, voice diaphragm device and voice diaphragm device manufacturing process

    CN112351375A

  • Low-density liquid crystal polymer and preparation method thereof

    CN111087765A

  • Low-dielectric-constant liquid crystal polymer and preparation method thereof

    CN111138815A