A preparation method of a net structure low-damage graphene and silicon carbide hybrid reinforced aluminum matrix composite material

A network-structured graphene-silicon carbide hybrid reinforced aluminum matrix composite material was prepared by pre-ball milling and multi-stage mixing processes. This solved the problems of weak interfacial bonding, damage to the reinforcing phase, and uneven distribution, and improved the strength and wear resistance of the material, making it suitable for aerospace and other fields.

CN117821795BActive Publication Date: 2026-11-20XIAN RARE METAL MATERIALS RES INST CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410028638.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-09
Publication Date
2026-11-20
Estimated Expiration
2044-01-09

AI Technical Summary

Technical Problem

In the existing technology, the preparation of aluminum matrix composites reinforced by hybrid micron-sized silicon carbide particles and nano-graphene has problems such as interface problems, damage to the reinforcing phase, and uneven distribution of the reinforcing phase, which makes it difficult to meet the service conditions requirements under complex conditions such as aerospace.

Method used

By pre-ball-milling aluminum powder into flakes and then mixing it with graphene nanosheets, combined with multi-stage mixing and powder metallurgy processes, damage to graphene and silicon carbide is reduced, and uniform distribution is achieved to form a network structure, thereby improving the interfacial bonding strength.

Benefits of technology

It effectively reduces damage to graphene and silicon carbide, improves interfacial bonding strength and the uniformity of reinforcing phase distribution, and significantly enhances the mechanical properties and wear resistance of aluminum-based composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117821795B_ABST
    Figure CN117821795B_ABST
Patent Text Reader

Abstract

The application discloses a preparation method of a net structure low-damage graphene and silicon carbide hybrid reinforced aluminum matrix composite material, and the method comprises the following steps: firstly, aluminum powder is pre-milled and then added into graphene nanosheets for milling to obtain graphene / aluminum composite powder; secondly, the graphene / aluminum composite powder is mixed with part of silicon carbide powder to obtain a first mixed powder; thirdly, the first mixed powder is mixed with the remaining silicon carbide powder to obtain a second mixed powder; fourthly, the second mixed powder is cold-pressed and vacuum hot-pressed and sintered to obtain a composite material blank; and finally, the composite material blank is hot-rolled and processed. According to the method, the aluminum powder is pre-milled and the silicon carbide is mixed in multiple stages, so that the damage to the graphene nanosheets is reduced, the interface bonding strength between the graphene nanosheets and the aluminum powder is improved, the damage to the silicon carbide reinforcing phase is reduced, the silicon carbide reinforcing phase is uniformly distributed in a net structure, and the rigidity, hardness, wear resistance, self-lubricating property and other mechanical and physical properties of the aluminum matrix composite material are improved. The method has the advantages of simple process flow, high efficiency, energy saving, time saving, low preparation cost and application promotion value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of composite material preparation technology, specifically relating to a method for preparing a hybrid aluminum-based composite material with a network structure of low-damage graphene and silicon carbide. Background Technology

[0002] Aluminum-based composite materials possess excellent properties such as high specific strength, high specific stiffness, good wear resistance, and dimensional stability, making them widely used in transportation, shipbuilding, and aerospace fields. For example, they can be used as wheels for lunar rover missions, brake discs for rail trains, and deployment structural components for spacecraft. However, with the rapid development of modern industry and the continuous optimization of my country's industrial structure, the reinforcing effect of single-phase reinforced composite materials is limited, making it difficult to meet the service conditions under complex conditions in aerospace, marine, and other applications.

[0003] Graphene nanosheets (GNS) have been widely used in aluminum-based composites in recent years due to their outstanding mechanical and thermal properties and excellent interfacial bonding. Studies have shown that graphene can promote interfacial dislocation storage and hinder grain boundary sliding, significantly improving the room-temperature plasticity and high-temperature strength of the composites. However, single-graphene reinforcement suffers from drawbacks such as insufficient stiffness and low wear resistance. To address this issue, a hybrid reinforcement approach is adopted, incorporating micron-sized silicon carbide particles (SiC) into the composites. p By introducing multiphase synergistic reinforcement into graphene composites and maintaining the advantages of each reinforcing phase, composite materials with a variety of excellent properties such as high modulus, high strength, high wear resistance, and high temperature resistance can be obtained.

[0004] Currently, the preparation of aluminum matrix composites reinforced with hybrid silicon carbide particles and nano-graphene mainly faces the following technical problems: (1) Interface problem; The interface between the reinforcing phase and the matrix is ​​an important support for the reinforcing phase to play its load transfer role. There are two reinforcing phases in the hybrid composite material, and its hot pressing process parameters are more difficult to control. Improper control of hot pressing parameters can easily lead to the generation of interface products and weak interface bonding. (2) Damage problem of the reinforcing phase; The structural integrity of the reinforcing phase has a huge impact on its strengthening effect. For example, once the structure of nano-reinforcing phases such as graphene is damaged, its reinforcing efficiency will be halved or even zero. Micron-sized silicon carbide is a ceramic phase. If it is broken, its wear resistance, strength, modulus, etc. will be greatly reduced. Although the traditional high-energy ball milling process can disperse graphene, it will cause great damage to graphene. In recent years, some new ball milling methods have been proposed, such as variable speed ball milling process (patent publication numbers CN112725660A, CN 114951664A, etc.). Although this process can reduce graphene damage, the short-time high-speed ball milling process can still damage micron-sized silicon carbide. (3) Distribution of reinforcing phase; According to the Hashin-Shtrikman (HS) theory, in discontinuous reinforced aluminum matrix composites, when the hard phase surrounds the soft phase, that is, when the reinforcing particles are distributed in a network, the elastic modulus of the composite material can reach the upper limit of HS, which can significantly improve the mechanical properties of the composite material. In hybrid composites, the two reinforcing phases have large size differences, making it difficult to ensure uniform distribution of the reinforcing phase and construct a network structure. Summary of the Invention

[0005] The technical problem to be solved by this invention is to address the shortcomings of the prior art by providing a method for preparing a network-structured, low-damage graphene-silicon carbide hybrid reinforced aluminum-based composite material. This method involves first ball-milling aluminum powder into flakes before ball-milling and mixing it with the reinforcing phase graphene nanosheets. This reduces damage to the graphene nanosheets and improves the interfacial bonding strength between the two. Furthermore, by introducing the silicon carbide reinforcing phase through multi-stage mixing, damage to the silicon carbide reinforcing phase is effectively reduced, resulting in a uniformly distributed network of silicon carbide reinforcing phase. This allows for a multi-phase synergistic reinforcement effect, improving the performance of the aluminum-based composite material and solving the problems of easy damage, easy interfacial reaction, weak interfacial bonding, and uneven distribution of the reinforcing phases during dispersion.

[0006] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: a method for preparing a network structure low-damage graphene and silicon carbide hybrid reinforced aluminum matrix composite material, characterized in that the method includes the following steps:

[0007] Step 1: Under argon protection, aluminum powder is pre-ball-milled, and then graphene nanosheets are added and ball-milled to obtain graphene / aluminum composite powder.

[0008] Step 2: Under argon protection, the graphene / aluminum composite powder obtained in Step 1 is mixed with a portion of silicon carbide powder to obtain a primary mixed powder.

[0009] Step 3: Under argon protection, the primary mixed powder obtained in step 2 is mixed with the remaining silicon carbide powder in a secondary mixture to obtain a secondary mixed powder.

[0010] Step 4: The secondary mixed powder obtained in Step 3 is subjected to cold pressing and vacuum hot pressing sintering in sequence to obtain composite material ingots;

[0011] Step 5: The composite material billet obtained in Step 4 is hot-rolled to obtain a graphene and silicon carbide hybrid reinforced aluminum matrix composite material.

[0012] Typically, the damage to the nano-carbon reinforcing phase is greatest during the initial ball milling stage. To address this challenge, this invention first uses a pre-ball milling method to transform aluminum powder into flakes with a larger surface area, changing it from spherical to larger flakes. Then, graphene nanosheets are added for further ball milling. The graphene nanosheets can quickly embed into the aluminum powder surface, and the softer aluminum powder protects them. During subsequent cold-welding ball milling, the graphene is encapsulated within the aluminum powder, effectively reducing damage to the graphene nanosheets and preventing damage to the nanosheets in the early stages of ball milling. Compared to existing traditional ball milling and variable-speed ball milling processes, this significantly reduces graphene damage, saves energy and time, and simultaneously yields a graphene / aluminum composite powder with strong interfacial bonding.

[0013] Next, this invention first performs a primary mixing of graphene / aluminum composite powder and a portion of silicon carbide powder to ensure uniform mixing and that some silicon carbide particles are distributed around the graphene / aluminum composite powder, forming a network structure. Then, the primary mixed powder is further mixed with the remaining silicon carbide powder in a secondary mixing process to achieve thorough homogenization. Simultaneously, this invention employs a low ball-to-particle ratio in both the primary and secondary mixing stages, reducing damage to the silicon carbide particles and improving the reinforcing efficiency of silicon carbide. Therefore, this invention utilizes a multi-stage mixing method to effectively reduce damage to the silicon carbide reinforcing phase and obtain a uniformly distributed network of silicon carbide reinforcing phase.

[0014] Finally, the present invention cold-presses the secondary mixed powder of matrix powder and reinforcing phase powder and then vacuum hot-presses and sintersects it. Through powder metallurgy, the probability of interfacial reaction is greatly reduced, and the interfacial bonding between aluminum matrix and reinforcing phase is further strengthened. Then, combined with hot rolling, the porosity in the composite material is further eliminated and the density is improved.

[0015] In summary, the method of the present invention effectively solves the problems of large damage to the reinforcing phase, weak interfacial bonding, and uneven distribution of the reinforcing phase in hybrid composite materials.

[0016] The method for preparing a low-damage graphene-silicon carbide hybrid reinforced aluminum matrix composite material with a network structure is characterized in that, in step one, the aluminum powder has a particle size of 10 μm to 100 μm, the graphene nanosheets have a diameter of 4 μm to 20 μm and a thickness of less than 10 nm, and the silicon carbide powder in steps two and three has a particle size of 4 μm to 50 μm. By limiting the size of the aluminum powder and graphene nanosheets, the graphene nanosheets are ensured to be rapidly embedded and encapsulated in the aluminum powder, reducing damage to the graphene nanosheets; by limiting the particle size of the silicon carbide powder, the uneven distribution caused by excessive size difference between the aluminum powder and silicon carbide powder is avoided.

[0017] The above-mentioned method for preparing a low-damage graphene and silicon carbide hybrid reinforced aluminum matrix composite material with a network structure is characterized in that, by volume percentage, the aluminum powder in step one is 77%–98.9%, the graphene nanosheets are 0.1%–3%, and the silicon carbide powder in steps two and three is 1%–20%. By limiting the volume percentage of aluminum powder, graphene nanosheets, and silicon carbide powder in the raw materials, the agglomeration of graphene nanosheets is avoided, which is beneficial to assisting in the formation of a network structure.

[0018] The preparation method of the above-mentioned low-damage graphene and silicon carbide hybrid reinforced aluminum matrix composite material with a mesh structure is characterized in that the pre-ball milling and ball milling in step one are both planetary ball milling, and process control agents ethanol or stearic acid are added during the process, with the added mass being 1% to 3% of the total mass of aluminum powder and graphene nanosheets.

[0019] The preparation method of the above-mentioned low-damage graphene and silicon carbide hybrid reinforced aluminum matrix composite material with a mesh structure is characterized in that the ball milling media used in the pre-ball milling and ball milling are stainless steel balls, the ball-to-material ratio is 15:1 to 25:1, the rotation speed is 300 r / min to 500 r / min, the pre-ball milling time is 2 h to 3 h, and the total time of pre-ball milling and ball milling is 4 h to 6 h.

[0020] The method for preparing a low-damage graphene-silicon carbide hybrid reinforced aluminum matrix composite material with a mesh structure, as described above, is characterized in that the primary mixing in step two and the secondary mixing in step three are performed using a roller ball mill, with stainless steel balls as the milling media, a ball-to-material ratio of 1:1 to 5:1, a rotation speed of 100 r / min to 200 r / min, and the mixing time for both primary and secondary mixing being 2 h to 3 h. The preferred rotation speed range for primary and secondary mixing in this invention is beneficial for achieving uniform distribution of silicon carbide and reducing silicon carbide damage.

[0021] The preparation method of the above-mentioned low-damage graphene and silicon carbide hybrid reinforced aluminum matrix composite material with a mesh structure is characterized in that the silicon carbide powder in step two accounts for 30% to 50% of the total mass of silicon carbide powder.

[0022] The above-mentioned method for preparing a low-damage graphene and silicon carbide hybrid reinforced aluminum matrix composite material with a mesh structure is characterized in that the specific process of vacuum hot pressing sintering in step four is as follows: at 10 -2 Under vacuum conditions of Pa, the composite preform obtained by cold pressing is heated to 580℃~640℃ by pulsed current, and hot pressing pressure of 35MPa~60MPa is applied and held for 60min~90min.

[0023] The method for preparing a low-damage graphene-silicon carbide hybrid reinforced aluminum matrix composite material with a mesh structure is characterized in that the hot rolling process in step five is as follows: the composite material billet is rolled at 450℃ to 540℃, and the total rolling deformation is 10% to 30%. By controlling the hot rolling process, cracking of the composite material is avoided.

[0024] Compared with the prior art, the present invention has the following advantages:

[0025] 1. This invention reduces damage to the graphene nanosheets and improves the interfacial bonding strength by first ball-milling aluminum powder into flakes and then ball-milling it with the reinforcing phase graphene nanosheets. The multi-stage mixing method effectively reduces damage to the silicon carbide reinforcing phase, resulting in a uniformly distributed network of silicon carbide reinforcing phase. This allows for the synergistic reinforcement effect of multiple phases, improving the strengthening efficiency of the reinforcing phase in aluminum-based composite materials. At the same time, it improves the mechanical and physical properties of aluminum-based composite materials, such as stiffness, hardness, wear resistance, and self-lubrication.

[0026] 2. In the graphene and silicon carbide hybrid reinforced aluminum matrix composite material prepared by this invention, the graphene is uniformly dispersed, the structural damage is small, the graphene-aluminum interface is firmly bonded, and no impurity compounds are generated at the interface. This effectively improves the load transfer efficiency of the reinforcing phase, avoids interface debonding during the stretching process, and improves the mechanical properties of the aluminum matrix composite material.

[0027] 3. The graphene and silicon carbide hybrid reinforced aluminum matrix composite material prepared by this invention has good silicon carbide-aluminum interface bonding, high integrity of silicon carbide particle structure, and forms a network distribution, which significantly improves the strength, plasticity and modulus of aluminum matrix composite material.

[0028] 4. This invention employs powder metallurgy and hot rolling processes, which avoids interfacial reactions, effectively eliminates defects such as pores in aluminum-based composite materials, and improves the mechanical properties of aluminum-based composite materials.

[0029] 5. The preparation method of the present invention has a simple process, reliable and efficient technology, energy saving and time saving, and low preparation cost, and has application and promotion value.

[0030] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0031] Figure 1 This is a process flow diagram of the preparation method of the present invention.

[0032] Figure 2a This is a distribution diagram of graphene nanosheets in the graphene and silicon carbide hybrid reinforced aluminum matrix composite material prepared in Example 3 of the present invention.

[0033] Figure 2b This is a graphene-aluminum interface diagram in the graphene-silicon carbide hybrid reinforced aluminum matrix composite material prepared in Example 3 of the present invention.

[0034] Figure 3 The image shows the metallographic structure of the graphene and silicon carbide hybrid reinforced aluminum matrix composite material prepared in Example 4 of this invention.

[0035] Figure 4 This is a scan image of the graphene and silicon carbide hybrid reinforced aluminum matrix composite material prepared in Example 4 of the present invention.

[0036] Figure 5 The image shows the X-ray diffraction pattern of the graphene and silicon carbide hybrid reinforced aluminum matrix composite material prepared in Example 4 of this invention. Detailed Implementation

[0037] Example 1

[0038] like Figure 1 As shown, this embodiment includes the following steps:

[0039] Step 1: Select aluminum powder with an average particle size D50 of 20 μm, graphene nanosheets with a diameter of 4 μm to 7 μm and a thickness of 5 nm, and silicon carbide with a particle size of 4 μm to 10 μm. The aluminum powder accounts for 98.9% of the total volume, the graphene nanosheets account for 0.1%, and the silicon carbide powder accounts for 1%. The total mass of the three is 100 g.

[0040] Under argon protection, aluminum powder was first placed in a planetary ball mill and 2g of stearic acid was added as a process control agent for pre-ball milling. The ball milling media used was stainless steel balls, the ball-to-material ratio was 15:1, the rotation speed was 400r / min, and the pre-ball milling time was 2h. Then, graphene nanosheets were added and ball milling was continued for 4h under the same conditions to obtain graphene / aluminum composite powder.

[0041] Step 2: Under argon protection, the graphene / aluminum composite powder obtained in Step 1 is placed in a drum ball mill, and 30% of the total mass of silicon carbide powder is added for primary mixing. The ball milling media is stainless steel balls, the ball-to-material ratio is 1:1, the rotation speed is 100 r / min, and the time is 2 h to obtain primary mixed powder.

[0042] Step 3: Under argon protection, the primary mixed powder obtained in Step 2 is mixed with the remaining silicon carbide powder under the same conditions as the primary mixing to obtain the secondary mixed powder;

[0043] Step 4: Under argon protection, the secondary mixed powder obtained in Step 3 is cold-pressed to obtain a composite preform, and then... -2 Under vacuum conditions of Pa, the composite preform was heated to 580°C by pulsed current, and then hot-pressed at 60 MPa for 60 min. After cooling, a composite preform with a diameter of 60 mm was obtained.

[0044] Step 5: The composite material billet obtained in Step 4 is hot rolled at 450℃ with a total rolling deformation of 10% to obtain a graphene and silicon carbide hybrid reinforced aluminum matrix composite material, namely graphene / silicon carbide / composite material.

[0045] Measurements showed that the average particle size of the silicon carbide particles in the graphene-silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment was 6.3 μm, which is similar to the average particle size of 7 μm for silicon carbide particles with a particle size of 4 μm to 10 μm in the raw material. Characterization showed that the graphene phase in the graphene-silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment has a high I... D / I G The value increased from 0.94 for the initial graphene nanosheets to 1.03, an increase of only 0.09, indicating that the pre-grinding and multi-stage mixing methods adopted in this invention resulted in minimal damage to both the graphene and silicon carbide reinforcing phases.

[0046] Example 2

[0047] like Figure 1 As shown, this embodiment includes the following steps:

[0048] Step 1: Select aluminum powder with an average particle size D50 of 100 μm, graphene nanosheets with a diameter of 10 μm to 20 μm and a thickness of 10 nm, and silicon carbide with a particle size of 40 μm to 50 μm. The aluminum powder accounts for 77% of the total volume, the graphene nanosheets account for 3% of the total volume, and the silicon carbide powder accounts for 20% of the total volume. The total mass of the three components is 100 g.

[0049] Under argon protection, aluminum powder was first placed in a planetary ball mill and 3g of ethanol was added as a process control agent for pre-ball milling. The ball milling media used were stainless steel balls, the ball-to-material ratio was 25:1, the rotation speed was 300r / min, and the pre-ball milling time was 2h. Then, graphene nanosheets were added and ball milling was continued for 4h under the same conditions to obtain graphene / aluminum composite powder.

[0050] Step 2: Under argon protection, the graphene / aluminum composite powder obtained in Step 1 is placed in a drum ball mill, and 50% of the total mass of silicon carbide powder is added for primary mixing. The ball milling media is stainless steel balls, the ball-to-material ratio is 5:1, the rotation speed is 200 r / min, and the time is 2 h to obtain primary mixed powder.

[0051] Step 3: Under argon protection, the primary mixed powder obtained in Step 2 is mixed with the remaining silicon carbide powder under the same conditions as the primary mixing, and the secondary mixing time is 3 hours to obtain the secondary mixed powder.

[0052] Step 4: Under argon protection, the secondary mixed powder obtained in Step 3 is cold-pressed to obtain a composite preform, and then... -2 Under vacuum conditions of Pa, the composite preform is heated to 640°C by pulsed current, hot pressing pressure of 35MPa is applied and held for 90min for hot pressing sintering, and then the composite preform is obtained after cooling treatment.

[0053] Step 5: The composite material billet obtained in Step 4 is hot rolled at 540℃ with a total rolling deformation of 30% to obtain a graphene and silicon carbide hybrid reinforced aluminum matrix composite material, namely graphene / silicon carbide / composite material.

[0054] Measurements showed that the average particle size of the silicon carbide particles in the graphene-silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment was 44 μm, which is similar to the average particle size of 45 μm of the silicon carbide particles in the raw material, which have a particle size of 40 μm to 50 μm. Characterization showed that the graphene phase in the graphene-silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment has a... D / I G The value increased from 0.94 for the initial graphene nanosheets to 1.04, an increase of only 0.1, indicating that the pre-grinding and multi-stage mixing methods employed in this invention resulted in almost no damage to the graphene and silicon carbide reinforcing phase.

[0055] Example 3

[0056] like Figure 1 As shown, this embodiment includes the following steps:

[0057] Step 1: Select aluminum powder with an average particle size D50 of 20 μm, graphene nanosheets with a diameter of 4 μm to 7 μm and a thickness of 5 nm, and silicon carbide with a particle size of 20 μm to 40 μm. The aluminum powder accounts for 89% of the total volume, the graphene nanosheets account for 10%, and the silicon carbide powder accounts for 1%. The total mass of the three is 100 g.

[0058] Under argon protection, aluminum powder was first placed in a planetary ball mill and 2g of stearic acid was added as a process control agent for pre-ball milling. The ball milling media used were stainless steel balls, the ball-to-material ratio was 15:1, the rotation speed was 500r / min, and the pre-ball milling time was 2h. Then, graphene nanosheets were added and ball milling was continued for 2h under the same conditions to obtain graphene / aluminum composite powder.

[0059] Step 2: Under argon protection, the graphene / aluminum composite powder obtained in Step 1 is placed in a drum ball mill, and 30% of the total mass of silicon carbide powder is added for primary mixing. The ball milling media is stainless steel balls, the ball-to-material ratio is 5:1, the rotation speed is 150 r / min, and the time is 2 h to obtain primary mixed powder.

[0060] Step 3: Under argon protection, the primary mixed powder obtained in Step 2 is mixed with the remaining silicon carbide powder under the same conditions as the primary mixing, and the secondary mixing time is 3 hours to obtain the secondary mixed powder.

[0061] Step 4: Under argon protection, the secondary mixed powder obtained in Step 3 is cold-pressed to obtain a composite preform, and then... -2 Under vacuum conditions of Pa, the composite preform is heated to 620°C by pulsed current, hot pressing pressure of 45MPa is applied and held for 60min for hot pressing sintering, and then the composite preform is obtained after cooling treatment.

[0062] Step 5: The composite material billet obtained in Step 4 is hot rolled at 500℃ with a total rolling deformation of 20% to obtain a graphene and silicon carbide hybrid reinforced aluminum matrix composite material, namely graphene / silicon carbide / composite material.

[0063] Figure 2a This is a distribution map of graphene nanosheets in the graphene-silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment. Figure 2a It can be seen that the graphene in the composite material is uniformly dispersed and no graphene agglomeration was found.

[0064] Figure 2b This is a graphene-aluminum interface diagram in the graphene-silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment. Figure 2b It can be seen that the graphene-aluminum interface in the composite material is clean and neat, the graphene structure is intact, and no other interface compounds were found.

[0065] Measurements showed that the average particle size of the silicon carbide particles in the graphene-silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment was 33.2 μm, which is similar to the average particle size of 30 μm for silicon carbide particles with a particle size of 20 μm to 40 μm in the raw material. Characterization showed that the graphene phase in the graphene-silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment has a high I... D / I G The value increased from 0.94 for the initial graphene nanosheets to 1.02, an increase of only 0.08, indicating that the pre-grinding and multi-stage mixing methods adopted in this invention resulted in minimal damage to both the graphene and silicon carbide reinforcing phases.

[0066] Example 4

[0067] like Figure 1 As shown, this embodiment includes the following steps:

[0068] Step 1: Select aluminum powder with an average particle size D50 of 20 μm, graphene nanosheets with a diameter of 4 μm to 7 μm and a thickness of 5 nm, and silicon carbide with a particle size of 10 μm to 20 μm. The aluminum powder accounts for 84.5% by volume, the graphene nanosheets account for 0.5%, and the silicon carbide powder accounts for 15%. The total mass of the three is 100 g.

[0069] Under argon protection, aluminum powder was first placed in a planetary ball mill and 2g of stearic acid was added as a process control agent for pre-ball milling. The ball milling media used were stainless steel balls, the ball-to-material ratio was 15:1, the rotation speed was 400r / min, and the pre-ball milling time was 1h. Then, graphene nanosheets were added and ball milling was continued for 5h under the same conditions to obtain a uniformly mixed graphene / aluminum composite powder.

[0070] Step 2: Under argon protection, the graphene / aluminum composite powder obtained in Step 1 is placed in a drum ball mill, and 30% of the total mass of silicon carbide powder is added for primary mixing. The ball milling media is stainless steel balls, the ball-to-material ratio is 5:1, the rotation speed is 150 r / min, and the time is 3 h to obtain primary mixed powder.

[0071] Step 3: Under argon protection, the primary mixed powder obtained in Step 2 is mixed with the remaining silicon carbide powder under the same conditions as the primary mixing, and the secondary mixing time is 3 hours to obtain the secondary mixed powder.

[0072] Step 4: Under argon protection, the secondary mixed powder obtained in Step 3 is cold-pressed to obtain a composite preform, and then... -2 Under vacuum conditions of Pa, the composite preform is heated to 620°C by pulsed current, hot pressing pressure of 45MPa is applied and held for 60min for hot pressing sintering, and then the composite preform is obtained after cooling treatment.

[0073] Step 5: The composite material billet obtained in Step 4 is hot rolled at 520℃ with a rolling deformation of 20% to obtain a graphene and silicon carbide hybrid reinforced aluminum matrix composite material, namely graphene / silicon carbide / composite material.

[0074] Figure 3 The image shows a metallographic image of the graphene and silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment. Figure 3 It can be seen that the silicon carbide and aluminum matrix have good interfacial bonding in the composite material, and no other compounds were found to be generated at the silicon carbide-aluminum interface.

[0075] Figure 4 This is a scan image of the graphene and silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment. Figure 4 It can be seen that the silicon carbide in the composite material is uniformly distributed, and adjacent silicon carbide particles are interconnected to form a network structure. According to the HS theory, when hard particles surround the soft phase, the reinforcing efficiency will be greatly improved. Therefore, the network structure in the composite material is beneficial to improving the strengthening effect of the reinforcing phase.

[0076] Figure 5 The X-ray diffraction pattern of the graphene and silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment is shown below. Figure 4 It can be seen that the composite material contains only Al phase, SiC phase and a very small amount of Al4C3 phase, and no other compounds were detected, indicating that there was almost no interfacial reaction between silicon carbide and graphene.

[0077] Testing showed that the graphene and silicon carbide reinforced aluminum matrix composite material of this embodiment has a tensile strength of up to 287 MPa, a Brinell hardness of 109 HB, and an elongation of 1%.

[0078] Measurements showed that the average particle size of the silicon carbide particles in the graphene-silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment was 16.7 μm, which is similar to the average particle size of 15 μm for silicon carbide particles with a particle size of 10 μm to 20 μm in the raw material. Characterization showed that the graphene phase in the graphene-silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment has a high I... D / I G The value increased from 0.94 for the initial graphene nanosheets to 1.00, an increase of only 0.06, indicating that the pre-grinding and multi-stage mixing methods adopted in this invention resulted in minimal damage to both the graphene and silicon carbide reinforcing phases.

[0079] Example 5

[0080] like Figure 1 As shown, this embodiment includes the following steps:

[0081] Step 1: Select aluminum powder with an average particle size D50 of 10 μm, graphene nanosheets with a diameter of 10 μm to 20 μm and a thickness of 5 nm, and silicon carbide with a particle size of 10 μm to 20 μm. The aluminum powder accounts for 93% of the total volume, the graphene nanosheets account for 2%, and the silicon carbide powder accounts for 5%. The total mass of the three is 100 g.

[0082] Under argon protection, aluminum powder was first placed in a planetary ball mill and 1g of stearic acid was added as a process control agent for pre-ball milling. The ball milling media used were stainless steel balls, the ball-to-material ratio was 20:1, the rotation speed was 320r / min, and the pre-ball milling time was 2h. Then, graphene nanosheets were added and ball milling was continued for 4h under the same conditions to obtain graphene / aluminum composite powder.

[0083] Step 2: Under argon protection, the graphene / aluminum composite powder obtained in Step 1 is placed in a drum ball mill, and 30% of the total mass of silicon carbide powder is added for primary mixing. The ball milling media is stainless steel balls, the ball-to-material ratio is 1:1, the rotation speed is 200 r / min, and the time is 3 h to obtain primary mixed powder.

[0084] Step 3: Under argon protection, the primary mixed powder obtained in Step 2 is mixed with the remaining silicon carbide powder under the same conditions as the primary mixing, and the secondary mixing time is 3 hours to obtain the secondary mixed powder.

[0085] Step 4: Under argon protection, the secondary mixed powder obtained in Step 3 is cold-pressed to obtain a composite preform, and then... -2 Under vacuum conditions of Pa, the composite preform is heated to 580°C by pulsed current, then hot-pressed at 50MPa for 60min, and then cooled to obtain the composite preform.

[0086] Step 5: The composite material billet obtained in Step 4 is hot rolled at 500℃ with a total rolling deformation of 30% to obtain a graphene and silicon carbide hybrid reinforced aluminum matrix composite material, namely graphene / silicon carbide / composite material.

[0087] Measurements showed that the average particle size of the silicon carbide particles in the graphene-silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment was 16.4 μm, which is similar to the average particle size of 15 μm for silicon carbide particles with a particle size of 10 μm to 20 μm in the raw material. Characterization showed that the graphene phase in the graphene-silicon carbide hybrid reinforced aluminum matrix composite material prepared in this embodiment has a... D / I G The value increased from 0.94 for the initial graphene nanosheets to 1.06, an increase of only 0.12, indicating that the damage to both graphene and silicon carbide reinforcing phases was minimal through the pre-grinding and multi-stage mixing method of the present invention.

[0088] The graphene and silicon carbide hybrid reinforced aluminum matrix composites prepared in Examples 1 to 5 of this invention were subjected to tensile tests and hardness tests: the tensile tests used plate-shaped room temperature tensile specimens with a gauge length of 15 mm, and the tensile standard was in accordance with GB / T228.1-2010 "Metallic Materials Tensile Testing Standard", with a tensile rate of 1.38 mm / min; the Brinell hardness test was conducted in accordance with GB / T231.1-2002 "Metallic Materials Brinell Hardness Test", and the test results are shown in Table 1 below.

[0089] Table 1

[0090]

[0091] In summary, the preparation method of the low-damage graphene-silicon carbide hybrid reinforced aluminum matrix composite material with a network structure of the present invention employs aluminum powder pre-ball milling and multi-stage mixing to effectively disperse graphene, reduce damage to both graphene and silicon carbide reinforcing phases, improve the reinforcing efficiency of the reinforcing phase, and obtain a strong reinforcing phase-aluminum interface bond. Simultaneously, the network distribution of silicon carbide particles is constructed, and the network structure provides excellent support, significantly improving the composite material's strength, plasticity, hardness, and elastic modulus. The preparation method of the present invention is simple to operate, has a short process flow, and has potential for industrial production.

[0092] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention in any way. Any simple modifications, alterations, and equivalent changes made to the above embodiments based on the inventive essence shall still fall within the protection scope of the present invention.

Claims

1. A method for preparing a network-structured, low-damage graphene and silicon carbide hybrid reinforced aluminum matrix composite material, characterized in that, The method includes the following steps: Step 1: Under argon protection, aluminum powder is pre-ball-milled, and then graphene nanosheets are added and ball-milled to obtain graphene / aluminum composite powder. Step 2: Under argon protection, the graphene / aluminum composite powder obtained in Step 1 is mixed with a portion of silicon carbide powder in a primary mixing process to obtain a primary mixed powder. The primary mixing and the secondary mixing in Step 3 are performed using a roller ball mill with stainless steel balls as the milling media. The ball-to-material ratio is 1:1 to 5:1, and the rotation speed is 100 r / min to 200 r / min. Both the primary and secondary mixing times are 2 to 3 hours. The silicon carbide powder constitutes 30% to 50% of the total mass of the silicon carbide powder. Step 3: Under argon protection, the primary mixed powder obtained in step 2 is mixed with the remaining silicon carbide powder in a secondary mixture to obtain a secondary mixed powder. By volume percentage, the aluminum powder in step one is 77%~98.9%, the graphene nanosheets are 0.1%~3%, and the silicon carbide powder mentioned in steps two and three is 1%~20%. Step 4: The secondary mixed powder obtained in Step 3 is subjected to cold pressing and vacuum hot pressing sintering in sequence to obtain composite material ingots; Step 5: The composite material billet obtained in Step 4 is hot-rolled to obtain a graphene and silicon carbide hybrid reinforced aluminum matrix composite material.

2. The method for preparing a mesh-structured low-damage graphene and silicon carbide hybrid reinforced aluminum matrix composite material according to claim 1, characterized in that, The aluminum powder in step one has a particle size of 10μm to 100μm, the graphene nanosheets have a diameter of 4μm to 20μm and a thickness of less than 10nm, and the silicon carbide powder in steps two and three has a particle size of 4μm to 50μm.

3. The method for preparing a mesh-structured low-damage graphene and silicon carbide hybrid reinforced aluminum matrix composite material according to claim 1, characterized in that, The pre-ball milling and ball milling described in step one are both planetary ball milling, and process control agents such as ethanol or stearic acid are added during the process, with the added mass being 1% to 3% of the total mass of aluminum powder and graphene nanosheets.

4. The method for preparing a mesh-structured low-damage graphene and silicon carbide hybrid reinforced aluminum matrix composite material according to claim 1, characterized in that, The ball milling media used in the pre-milling and ball milling are stainless steel balls, with a ball-to-material ratio of 15:1 to 25:1, a rotation speed of 300 r / min to 500 r / min, and a pre-milling time of 2 h to 3 h. The total time for pre-milling and ball milling is 4 h to 6 h.

5. The method for preparing a mesh-structured low-damage graphene and silicon carbide hybrid reinforced aluminum matrix composite material according to claim 1, characterized in that, The specific process of vacuum hot pressing sintering described in step four is as follows: at 10 -2 Under vacuum conditions of Pa, the composite preform obtained by cold pressing is heated to 580℃~640℃ by pulsed current, and hot pressing pressure of 35MPa~60MPa is applied and held for 60min~90min.

6. The method for preparing a mesh-structured low-damage graphene and silicon carbide hybrid reinforced aluminum matrix composite material according to claim 1, characterized in that, The specific process of hot rolling in step five is as follows: the composite material billet is rolled at 450℃~540℃, and the total deformation during rolling is 10%~30%.

Citation Information

Patent Citations

  • Powder metallurgy preparation method of graphene reinforced aluminum-based composite material

    CN112725660A

  • Preparation method of graphene and silicon carbide hybrid reinforced aluminum-based composite material

    CN114951664A

  • Preparation method of graphene-reinforced aluminum-based composite material

    CN108085524A

  • Preparation method of high-performance graphene reinforced aluminum-based composite material

    CN117230337A