High-hardness high-wear-resistance light-weight high-entropy alloy, preparation method and application thereof
A high-hardness, high-wear-resistant, lightweight, high-entropy alloy was prepared by using the chemical composition AlxV(0.6-x)Ti(0.4-y)Zry and a vacuum arc melting process. This solved the problem of insufficient hardness and wear resistance in existing high-entropy alloys, achieving a combination of low density, high hardness, and high wear resistance, and improving the overall performance of the alloy.
Patent Information
- Application Number
- CN202311720377.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-14
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-14
AI Technical Summary
Existing high-entropy alloys struggle to balance low density, high hardness, and high wear resistance, resulting in insufficient performance under friction and wear conditions and limiting their application range.
A high-hardness, high-wear-resistant, lightweight, high-entropy alloy was prepared using the chemical composition of AlxV(0.6-x)Ti(0.4-y)Zry through vacuum arc melting. AlZr and TiV master alloys were used as raw materials, and argon protection and multiple melting processes were combined to ensure the purity and performance of the alloy.
The prepared high-hardness, high-wear-resistant, lightweight, high-entropy alloy has a low density and significantly improved hardness and wear resistance, which can effectively reduce wear and improve the safe service life and economic benefits of mechanical equipment.
Smart Images

Figure CN117821824B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of alloy preparation technology, specifically to a high-hardness, high-wear-resistant, lightweight, high-entropy alloy, its preparation method, and its applications. Background Technology
[0002] Titanium alloys and titanium-based composites are lightweight, have high specific strength, and possess excellent comprehensive properties such as corrosion resistance and high-temperature resistance. Titanium alloys for aircraft structures are mainly used in aircraft frames, doors, hydraulic lines and joints, landing gear, skin, rivets, and wing spars. Titanium alloys for aero engines are mainly used in compressor blades, discs, and casings. Titanium alloys have been widely used due to their numerous excellent properties; however, like any material, they have their advantages and disadvantages. ① The disadvantages of titanium alloys are low surface hardness and poor wear resistance. The hardness of titanium alloys typically does not exceed 350 HV, which is insufficient for many practical production applications. For example, when used as sliding parts, they easily adhere to the mating material, causing adhesive wear, which severely limits their application range. The low tribological properties of titanium alloys can be attributed to two main factors: low plastic shear resistance and work hardening rate; and low protective effect of surface oxides. Many failures of titanium alloy machine parts are caused by friction and wear, resulting in significant economic losses annually.
[0003] With the development of science and technology in aviation, aerospace, electronics, and communications, and the increasing demands on the performance of various materials, existing alloy systems are gradually becoming insufficient to meet these needs. Therefore, efforts are being made to develop new alloys to satisfy societal requirements. However, existing alloy systems are approaching saturation, and traditional design approaches are no longer sufficient to achieve significant breakthroughs. Thus, new alloy design concepts have become crucial for overcoming the bottlenecks in the field of alloy design.
[0004] In 1995, Ye Junwei broke through the traditional concept of materials design and proposed a new alloy design concept based on amorphous alloys, which he called High Entropy Alloys (HEAs). HEAs possess thermodynamic high entropy effects, structural lattice distortion effects, kinetic hysteresis diffusion effects, and performance cocktail effects. These characteristics make it easy to obtain thermally stable solid solution phases, nanostructures, and even amorphous structures. HEAs exhibit superior properties such as high strength, high hardness, high wear resistance, high oxidation resistance, and high corrosion resistance, which are not simultaneously possessed by traditional alloys. They have become one of the three most promising research areas in recent years and have high academic research value.
[0005] Utilizing the "high entropy" effect to prepare lightweight, high-strength, and high-wear-resistant high-entropy alloys can reduce wear and reduce weight, not only improving the safe service life of mechanical equipment and parts but also creating significant socio-economic benefits. However, existing high-entropy alloys struggle to simultaneously achieve low density, high hardness, and high wear resistance. Summary of the Invention
[0006] In order to overcome at least one of the technical problems existing in the prior art, the present invention provides a high-hardness, high-wear-resistant, lightweight, high-entropy alloy, its preparation method, and its application.
[0007] The above-mentioned technical problem to be solved by the present invention is achieved through the following technical solution:
[0008] The present invention first provides a high-hardness, high-wear-resistant, lightweight, high-entropy alloy. The chemical composition of the high-hardness, high-wear-resistant, lightweight, high-entropy alloy is AlxV(0.6-x)Ti(0.4-y)Zry, wherein 0.2≤x≤0.35 and 0.02≤y≤0.2.
[0009] Preferably, the chemical composition of the high-hardness, high-wear-resistant, lightweight, high-entropy alloy is AlxV(0.6-x)Ti(0.4-y)Zry, where 0.25≤x≤0.35 and 0.05≤y≤0.1.
[0010] Most preferably, the chemical composition of the high-hardness, high-wear-resistant, lightweight, high-entropy alloy is AlxV(0.6-x)Ti(0.4-y)Zry, where x = 0.3 and y = 0.08.
[0011] The present invention also provides a method for preparing the above-mentioned high-hardness, high-wear-resistant, lightweight, high-entropy alloy, which includes the following steps:
[0012] Raw material weighing steps: Accurately weigh AlZr and TiV master alloys according to atomic percentage as raw materials, and make up the missing mass with Ti, Zr, Al and V to obtain metal raw materials;
[0013] Melting steps: Place the metal raw material into the melting equipment, adjust the current intensity to 250A-300A, melt for 0.1-4 minutes, then melt for another 0.1-4 minutes under stirring, and obtain the alloy ingot after cooling; take the alloy ingot to obtain the high hardness, high wear resistance, lightweight, high entropy alloy.
[0014] Preferably, in the melting step, the current intensity is adjusted to 250A-300A, and after melting for 0.5-2 minutes, it is melted again under stirring for 0.5-2 minutes.
[0015] Preferably, the smelting process is carried out under a protective gas atmosphere.
[0016] Preferably, the smelting step is repeated 2 to 10 times.
[0017] Preferably, before the smelting step, the process further includes a gas washing step for the metal raw materials, a deoxygenation step for the smelting environment, and / or a cleaning step for the alloy casting after smelting.
[0018] Preferably, the gas washing step specifically involves: placing the metal raw material on a water-cooled copper crucible, placing the titanium ball on the copper crucible in the middle of the vacuum arc melting furnace, then closing the furnace door and evacuating the furnace, followed by gas washing with high-purity argon, and finally evacuating until the vacuum level inside the furnace is below 4 × 10⁻⁶. -3 Pa.
[0019] Preferably, the deoxygenation step in the smelting environment specifically involves: placing the electrode head close to the copper crucible, igniting an arc on the copper crucible, and first smelting the titanium balls under a protective gas to remove residual oxygen in the furnace.
[0020] The cleaning steps for the alloy ingot after smelting are as follows: the alloy ingot after smelting is wiped with anhydrous ethanol.
[0021] The present invention also provides an application of the above-mentioned high-hardness, high-wear-resistant, lightweight, high-entropy alloy in the preparation of products with high hardness.
[0022] Preferably, the chemical composition of the high-hardness, high-wear-resistant, lightweight, high-entropy alloy used to prepare products with high hardness is Al. 0.3 V 0.3 Ti 0.32 Zr 0.08 .
[0023] The present invention also provides an application of the above-mentioned high-hardness, high-wear-resistant, lightweight, high-entropy alloy in the preparation of products with high wear resistance.
[0024] Preferably, the chemical composition of the high-hardness, high-wear-resistant, lightweight, high-entropy alloy used to prepare products with high wear resistance is Al. 0.3 V 0.3 Ti 0.32 Zr 0.08 .
[0025] Beneficial Effects: This invention provides a novel high-hardness, high-wear-resistant, lightweight high-entropy alloy and its preparation method. The invention uses AlZr and TiV master alloys as raw materials, and the missing mass is supplemented with Ti, Zr, Al, and V of the same purity. AlxV(0.6-x)Ti(0.4-y)Zry is prepared by vacuum arc melting. This preparation method is advanced and has accurate and detailed technical parameters. Furthermore, the high-entropy alloy of this invention not only has a low density but also high strength and hardness, effectively improving the hardness and wear resistance of the lightweight high-entropy alloy. In addition, this lightweight high-entropy alloy can save energy, improve economic efficiency, and has potential applications in the engineering field. Attached Figure Description
[0026] Figure 1 Al obtained in Example 3 of the present invention 0.25 V 0.35 Ti 0.35 Zr 0.05 Scanning electron microscope image of the surface of a lightweight high-entropy alloy;
[0027] Figure 2 Al obtained in Example 3 of the present invention 0.25 V 0.35 Ti 0.35 Zr 0.05 XRD pattern of a lightweight high-entropy alloy.
[0028] Figure 3 Al obtained in Example 3 of the present invention 0.25 V 0.35 Ti 0.35 Zr 0.05 The static compressive stress-strain curve of a lightweight high-entropy alloy. Detailed Implementation
[0029] The present invention will be further explained below with reference to specific embodiments, but the embodiments do not limit the present invention in any way.
[0030] The technical solutions in the embodiments of the present invention will be fully described below with reference to examples of the present invention. The following are only a part of the examples of the present invention, not all of them. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit the present invention or its application or use. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0031] Unless otherwise specifically stated, the numerical values set forth in these embodiments do not limit the scope of the invention. Techniques and methods known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques and methods should be considered part of the specification. In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may have different values.
[0032] In this invention, Al represents aluminum, V represents vanadium, Ti represents titanium, and Zr represents zirconium; the protective gases are nitrogen and rare gases.
[0033] Hardness testing method: The alloy ingot is cut into small pieces by wire cutting, and then sanded with sandpaper in the order of 180, 800, 1000, 1500, 2000, 2500 and 5000 grit. After sanding, diamond polishing paste is used to polish until the surface is free of scratches. After polishing, the surface is cleaned with anhydrous ethanol using ultrasonic cleaning to remove surface stains, and then the hardness is tested. The hardness test uses a Vickers hardness tester and a digital microhardness tester (Shanghai Taiming Optical Instrument Co., Ltd.), with a pressure of 200gf and a holding time of 15s.
[0034] Example 1
[0035] A high-hardness, high-wear-resistant, lightweight, high-entropy alloy, measured atomically, comprises 25% Al, 35% V, 30% Ti, and 10% Zr, expressed as Al... 0.25 V 0.35 Ti 0.3 Zr 0.1 The preparation method of the high-entropy alloy in this example is as follows:
[0036] Step 1: Use AlZr and TiV master alloys with a purity higher than 99.9% as raw materials. Make up any missing mass with Ti, Zr, Al, and V of the same purity. Weigh them precisely according to the above proportions to prepare 30g of raw material. Place the prepared metal raw material on a copper crucible. Place titanium balls on the copper crucible in the center of the vacuum arc melting furnace. Then close the furnace door and evacuate the furnace. Next, purge with high-purity argon (≥99.999%) until the pressure gauge reads -0.02MPa. Finally, use a mechanical pump and a molecular pump to evacuate the furnace until the vacuum level is below 4×10⁻⁶. -3 Pa, repeat the gas washing twice;
[0037] Step 2: After purging, fill with high-argon protective gas until the pressure gauge reads -0.05MPa;
[0038] Step 3: Place the electrode head slightly close to the copper crucible and ignite an arc on the copper crucible. Melt the titanium ball for 2 minutes under the protection of argon atmosphere to remove residual oxygen in the furnace.
[0039] Step 4: Start melting the metal raw material from Step 1. Rotate the arc gun lifting device to keep the electrode head at an appropriate distance from the raw material. Adjust the current intensity to 280A. After melting for 1 minute, turn on the magnetic stirring to melt for another minute. Then turn off the magnetic stirring and melt the alloy into a round cake shape. After melting and cooling, use a flipping metal spoon to flip the alloy ingot.
[0040] Step 5: Following the steps in Step 4, repeatedly turn and melt the alloy ingot. After melting, allow the alloy ingot to cool naturally in the furnace to room temperature. Then, remove the ingot and clean it to obtain the high-hardness, high-wear-resistant, lightweight, high-entropy alloy. The alloy ingot is ultrasonically cleaned with anhydrous ethanol to ensure a clean surface. Multiple melting processes are performed, with a total of 5 repetitions. After each melting process, the alloy ingot needs to be turned using a metal ladle.
[0041] The total mass after melting, measured using an electronic balance, was 29.90 g, with a burn loss rate of less than 0.5%. The Al content was measured using a digital microhardness tester. 0.25 V 0.35 Ti 0.3 Zr 0.1 The lightweight high-entropy alloy has an average hardness of 595.5 HV and a density of 4.80 g / cm³. 3 Its hardness value is much higher than that of TC4 titanium alloy.
[0042] Example 2
[0043] A high-hardness, high-wear-resistant, lightweight, high-entropy alloy, measured atomically, comprises 30% Al, 30% V, 32% Ti, and 8% Zr, expressed as Al... 0.3 V 0.3 Ti 0.32 Zr 0.08 The preparation method of the high-entropy alloy in this example is as follows:
[0044] Step 1: Use AlZr and TiV master alloys with a purity higher than 99.9% as raw materials. Make up any missing mass with Ti, Zr, Al, and V of the same purity. Weigh them precisely according to the above proportions to prepare 30g of raw material. Place the prepared metal raw material on a copper crucible. Place titanium balls on the copper crucible in the center of the vacuum arc melting furnace. Then close the furnace door and evacuate the furnace. Next, purge with high-purity argon (≥99.999%) until the pressure gauge reads -0.02MPa. Finally, use a mechanical pump and a molecular pump to evacuate the furnace until the vacuum level is below 4×10⁻⁶. -3Pa, repeat the gas washing twice;
[0045] Step 2: After purging, fill with high-argon protective gas until the pressure gauge reads -0.05MPa;
[0046] Step 3: Place the electrode head slightly close to the copper crucible and ignite an arc on the copper crucible. Melt the titanium ball for 2 minutes under the protection of argon atmosphere to remove residual oxygen in the furnace.
[0047] Step 4: Start melting the metal raw material from Step 1. Rotate the arc gun lifting device to keep the electrode head at an appropriate distance from the raw material. Adjust the current intensity to 250A. After melting for 1 minute, turn on the magnetic stirring to melt for another minute. Then turn off the magnetic stirring and melt the alloy into a round cake shape. After melting and cooling, use a flipping metal spoon to flip the alloy ingot.
[0048] Step 5: Following the steps in Step 4, repeatedly turn and melt the alloy ingot. After melting, allow the alloy ingot to cool naturally in the furnace to room temperature. Then, remove the ingot and clean it to obtain the high-hardness, high-wear-resistant, lightweight, high-entropy alloy. The alloy ingot is ultrasonically cleaned with anhydrous ethanol to ensure a clean surface. Multiple melting processes are performed, with a total of 5 repetitions. After each melting process, the alloy ingot needs to be turned using a metal ladle.
[0049] The total mass after melting was measured to be 29.88g using an electronic balance, with a burn loss rate of less than 0.5%. The Al content was measured using a digital microhardness tester. 0.3 V 0.3 Ti 0.32 Zr 0.08 The lightweight high-entropy alloy has an average hardness of 608.3 HV and a density of 4.59 g / cm³. 3 Its hardness value is much higher than that of TC4 titanium alloy.
[0050] Example 3
[0051] A high-hardness, high-wear-resistant, lightweight, high-entropy alloy, measured by atomic percentage, comprises 25% Al, 35% V, 35% Ti, and 5% Zr, and its formula is: Al 0.25 V 0.35 Ti 0.35 Zr 0.05 The preparation method of the high-entropy alloy in this example is as follows:
[0052] Step 1: Use AlZr and TiV master alloys with a purity higher than 99.9% as raw materials. Make up any missing mass with Ti, Zr, Al, and V of the same purity. Weigh them precisely according to the above proportions to prepare 30g of raw material. Place the prepared metal raw material on a copper crucible. Place titanium balls on the copper crucible in the center of the vacuum arc melting furnace. Then close the furnace door and evacuate the furnace. Next, purge with high-purity argon (≥99.999%) until the pressure gauge reads -0.02MPa. Finally, use a mechanical pump and a molecular pump to evacuate the furnace until the vacuum level is below 4×10⁻⁶. -3 Pa, repeat the gas washing twice;
[0053] Step 2: After purging, fill with high-argon protective gas until the pressure gauge reads -0.05MPa;
[0054] Step 3: Place the electrode head slightly close to the copper crucible and ignite an arc on the copper crucible. Melt the titanium ball for 2 minutes under the protection of argon atmosphere to remove residual oxygen in the furnace.
[0055] Step 4: Start melting the metal raw material from Step 1. Rotate the arc gun lifting device to keep the electrode head at an appropriate distance from the raw material. Adjust the current intensity to 300A. After melting for 1 minute, turn on the magnetic stirring to melt for another minute. Then turn off the magnetic stirring and melt the alloy into a round cake shape. After melting and cooling, use a flipping metal spoon to flip the alloy ingot.
[0056] Step 5: Following the steps in Step 4, repeatedly turn and melt the alloy ingot. After melting, allow the alloy ingot to cool naturally in the furnace to room temperature. Then, remove the ingot and clean it to obtain the high-hardness, high-wear-resistant, lightweight, high-entropy alloy. The alloy ingot is ultrasonically cleaned with anhydrous ethanol to ensure a clean surface. Multiple melting processes are performed, with a total of 5 repetitions. After each melting process, the alloy ingot needs to be turned using a metal ladle.
[0057] The total mass after melting, measured using an electronic balance, was 29.93 g, with a burn loss rate of less than 0.5%. The Al content was measured using a digital microhardness tester. 0.25 V 0.35 Ti 0.35 Zr 0.05 The lightweight high-entropy alloy has an average hardness of 570.5 HV and a density of 4.66 g / cm³. 3 Its hardness value is much higher than that of TC4 titanium alloy.
[0058] Example 4
[0059] A high-hardness, high-wear-resistant, lightweight, high-entropy alloy, measured by atomic percentage, comprises 8% Al, 32% V, 35% Ti, and 25% Zr, and its formula is: Al0.08 V 0.32 Ti 0.35 Zr 0.25 The preparation method of the high-entropy alloy in this example is as follows:
[0060] Step 1: Use AlZr and TiV master alloys with a purity higher than 99.9% as raw materials. Make up any missing mass with Ti, Zr, Al, and V of the same purity. Weigh them precisely according to the above proportions to prepare 30g of raw material. Place the prepared metal raw material on a copper crucible. Place titanium balls on the copper crucible in the center of the vacuum arc melting furnace. Then close the furnace door and evacuate the furnace. Next, purge with high-purity argon (≥99.999%) until the pressure gauge reads -0.02MPa. Finally, use a mechanical pump and a molecular pump to evacuate the furnace until the vacuum level is below 4×10⁻⁶. -3 Pa, repeat the gas washing twice;
[0061] Step 2: After purging, fill with high-argon protective gas until the pressure gauge reads -0.05MPa;
[0062] Step 3: Place the electrode head slightly close to the copper crucible and ignite an arc on the copper crucible. Melt the titanium ball for 2 minutes under the protection of argon atmosphere to remove residual oxygen in the furnace.
[0063] Step 4: Start melting the metal raw material from Step 1. Rotate the arc gun lifting device to keep the electrode head at an appropriate distance from the raw material. Adjust the current intensity to 260A. After melting for 1 minute, turn on the magnetic stirring to melt for another minute. Then turn off the magnetic stirring and melt the alloy into a round cake shape. After melting and cooling, use a flipping metal spoon to flip the alloy ingot.
[0064] Step 5: Following the steps in Step 4, repeatedly turn and melt the alloy ingot. After melting, allow the alloy ingot to cool naturally in the furnace to room temperature. Then, remove the ingot and clean it to obtain the high-hardness, high-wear-resistant, lightweight, high-entropy alloy. The alloy ingot is ultrasonically cleaned with anhydrous ethanol to ensure a clean surface. Multiple melting processes are performed, with a total of 5 repetitions. After each melting process, the alloy ingot needs to be turned using a metal ladle.
[0065] The total mass after melting, measured using an electronic balance, was 29.91 g, with a burn loss rate of less than 0.5%. The Al content was measured using a digital microhardness tester. 0.08 V 0.32 Ti 0.35 Zr 0.25 The lightweight high-entropy alloy has an average hardness of 503.6 HV and a density of 5.43 g / cm³. 3 However, this formula has a higher density and a relatively lower hardness value.
[0066] Example 5
[0067] A high-hardness, high-wear-resistant, lightweight, high-entropy alloy, measured by atomic percentage, comprises 5% Al, 35% V, 25% Ti, and 35% Zr, and its formula is: Al 0.05 V 0.35 Ti 0.25 Zr 0.35 The preparation method of the high-entropy alloy in this example is as follows:
[0068] Step 1: Use AlZr and TiV master alloys with a purity higher than 99.9% as raw materials. Make up any missing mass with Ti, Zr, Al, and V of the same purity. Weigh them precisely according to the above proportions to prepare 30g of raw material. Place the prepared metal raw material on a copper crucible. Place titanium balls on the copper crucible in the center of the vacuum arc melting furnace. Then close the furnace door and evacuate the furnace. Next, purge with high-purity argon (≥99.999%) until the pressure gauge reads -0.02MPa. Finally, use a mechanical pump and a molecular pump to evacuate the furnace until the vacuum level is below 4×10⁻⁶. -3 Pa, repeat the gas washing twice;
[0069] Step 2: After purging, fill with high-argon protective gas until the pressure gauge reads -0.05MPa;
[0070] Step 3: Place the electrode head slightly close to the copper crucible and ignite an arc on the copper crucible. Melt the titanium ball for 2 minutes under the protection of argon atmosphere to remove residual oxygen in the furnace.
[0071] Step 4: Start melting the metal raw material from Step 1. Rotate the arc gun lifting device to keep the electrode head at an appropriate distance from the raw material. Adjust the current intensity to 270A. After melting for 1 minute, turn on the magnetic stirring to melt for another minute. Then turn off the magnetic stirring and melt the alloy into a round cake shape. After melting and cooling, use a flipping metal spoon to flip the alloy ingot.
[0072] Step 5: Following the steps in Step 5, repeatedly turn and melt the alloy ingot. After melting, allow the alloy ingot to cool naturally in the furnace to room temperature. Then, remove the alloy ingot and clean it to obtain the high-hardness, high-wear-resistant, lightweight, high-entropy alloy. The alloy ingot is ultrasonically cleaned with anhydrous ethanol to ensure a clean surface. Multiple melting processes are performed, with a total of 5 repetitions. After each melting process, the alloy ingot needs to be turned using a metal ladle.
[0073] The total mass after melting was measured to be 29.92g using an electronic balance, with a burn loss rate of less than 0.5%. The Al content was measured using a digital microhardness tester. 0.08 V 0.32 Ti 0.35 Zr0.25 The lightweight high-entropy alloy has an average hardness of 516.3 HV and a density of 5.75 g / cm³. 3 However, this formula has a higher density and a relatively lower hardness value.
[0074] Experimental Sample Performance Testing
[0075] The tribological properties of the lightweight high-entropy alloys prepared in Examples 1-5 of this invention were characterized using a RETC multi-functional tribological testing machine. The characterization conditions were as follows: mode: ball-and-disc type, paired balls were 6mm diameter GCR15 steel balls, speed was 5Hz, friction time was 30 minutes, room temperature, air humidity was 65±10%, and load was 10N. Tribological properties were compared using a TC4 tester under the same conditions. The hardness and wear volume of the high-hardness, high-wear-resistant lightweight high-entropy alloys prepared in Examples 1-5 are shown in Table 1.
[0076] In addition, the prepared Al was tested using an electronic universal testing machine (MTS E45.305). 0.25 V 0.35 Ti 0.35 Zr 0.05 Compression performance tests were conducted on a high-hardness, high-wear-resistant, lightweight, high-entropy alloy; test results are shown below. Figure 3 .
[0077] Table 1. Performance test results of the high-hardness, high-wear-resistant, lightweight, high-entropy alloy of the present invention.
[0078] High-hardness, high-wear-resistant, lightweight, high-entropy alloy types hardness Wear volume <![CDATA[Al 0.25 V 0.35 You 0.3 Zr 0.1 ]]> 595.5HV <![CDATA[33.6×10 -3 mm 3 ]]> <![CDATA[Al 0.3 V 0.3 You 0.32 Zr 0.08 ]]> 608.3HV <![CDATA[29.5×10 -3 mm 3 ]]> <![CDATA[Al 0.25 V 0.35 You 0.35 Zr 0.05 ]]> 570.5HV <![CDATA[42.2×10 -3 mm 3 ]]> <![CDATA[Al 0.08 V 0.32 You 0.35 Zr 0.25 ]]> 503.6HV <![CDATA[66.7×10 -3 mm 3 ]]> <![CDATA[Al 0.05 V 0.35 You 0.25 Zr 0.35 ]]> 516.3HV <![CDATA[61.8×10 -3 mm 3 ]]> TC4 alloy 343.1HV <![CDATA[98.6×10 -3 mm 3 ]]>
[0079] As can be seen from the experimental results in Table 1, the high-hardness, high-wear-resistant, lightweight, high-entropy alloy described in this invention has a hardness of over 500 HV, which is significantly higher than that of the TC4 alloy. This indicates that the high-hardness, high-wear-resistant, lightweight, high-entropy alloy with the chemical composition AlxV(0.6-x)Ti(0.4-y)Zry of this invention has very high hardness; its hardness is significantly higher than that of the TC4 alloy.
[0080] Furthermore, as can be seen from the experimental results in Table 1, in the high-hardness, high-wear-resistant, lightweight, high-entropy alloy with the chemical composition AlxV(0.6-x)Ti(0.4-y)Zry of this invention, the hardness of the resulting high-hardness, high-wear-resistant, lightweight, high-entropy alloy varies considerably depending on the values of x and y. The above experimental results indicate that the chemical composition Al... 0.3 V 0.3 Ti 0.32 Zr 0.08 The high-hardness, high-wear-resistant, lightweight, high-entropy alloy has the highest hardness, significantly higher than that of Al alloys. 0.25 V 0.35 Ti 0.35 Zr 0.05A high-hardness, high-wear-resistant, lightweight, high-entropy alloy, while significantly higher than that with an Al chemical composition. 0.08 V 0.32 Ti 0.35 Zr 0.25 And the chemical composition is Al 0.05 V 0.35 Ti 0.25 Zr 0.35 High-hardness, high-wear-resistant, lightweight, high-entropy alloy.
[0081] As can be seen from the experimental results in Table 1, the wear volume of the high-hardness, high-wear-resistant, lightweight, high-entropy alloy described in this invention is significantly, even substantially, lower than that of the TC4 alloy. This indicates that the high-hardness, high-wear-resistant, lightweight, high-entropy alloy with the chemical composition AlxV(0.6-x)Ti(0.4-y)Zry of this invention has very good wear resistance; its wear resistance is significantly, even substantially, higher than that of the TC4 alloy.
[0082] Furthermore, as can be seen from the experimental results in Table 1, in the high-hardness, high-wear-resistant, lightweight, high-entropy alloy with the chemical composition AlxV(0.6-x)Ti(0.4-y)Zry of this invention, the wear volume of the high-hardness, high-wear-resistant, lightweight, high-entropy alloy varies significantly depending on the values of x and y; the chemical composition Al 0.3 V 0.3 Ti 0.32 Zr 0.08 The wear volume of high-hardness, high-wear-resistant, lightweight, high-entropy alloys is the smallest, and its wear volume is significantly lower than that of Al alloys. 0.25 V 0.35 Ti 0.3 Zr 0.1 And the chemical composition is Al 0.25 V 0.35 Ti 0.35 Zr 0.05 A high-hardness, high-wear-resistant, lightweight, high-entropy alloy, while significantly lower in hardness than Al. 0.08 V 0.32 Ti 0.35 Zr 0.25 And the chemical composition is Al 0.05 V 0.35 Ti 0.25 Zr 0.35 A high-hardness, high-wear-resistant, lightweight, high-entropy alloy; this indicates that the chemical composition is Al. 0.3 V 0.3 Ti 0.32 Zr 0.08 High-hardness, high-wear-resistant, lightweight, high-entropy alloys possess excellent wear resistance, significantly higher than those with an Al chemical composition. 0.25 V 0.35 Ti 0.3 Zr0.1 And the chemical composition is Al 0.25 V 0.35 Ti 0.35 Zr 0.05 A high-hardness, high-wear-resistant, lightweight, high-entropy alloy, while significantly higher than that with an Al chemical composition. 0.08 V 0.32 Ti 0.35 Zr 0.25 And the chemical composition is Al 0.05 V 0.35 Ti 0.25 Zr 0.35 High-hardness, high-wear-resistant, lightweight, high-entropy alloy.
Claims
1. A high-hardness, high-wear-resistant, lightweight, high-entropy alloy, characterized in that, The high hardness, high wear resistance and lightweight The chemical composition of the high-entropy alloy is AlxV(0.6-x)Ti(0.4-y)Zry, where x=0.3 and y=0.
08.
2. The method for preparing the high-hardness, high-wear-resistant, lightweight, high-entropy alloy according to claim 1, characterized in that, It includes the following steps: Raw material weighing steps: Accurately weigh AlZr and TiV master alloys according to atomic percentage as raw materials, and make up the missing mass with Ti, Zr, Al and V to obtain metal raw materials; Melting steps: Place the metal raw material into the melting equipment, adjust the current intensity to 250A-300A, melt for 0.1~4min, then melt for another 0.1~4min under stirring, and obtain the alloy ingot after cooling; take the alloy ingot to obtain the high hardness, high wear resistance, lightweight high entropy alloy.
3. The method for preparing the high-hardness, high-wear-resistant, lightweight, high-entropy alloy according to claim 2, characterized in that, During the melting process, the current intensity is adjusted to 250A-300A, and after melting for 0.5-2 minutes, it is melted again under stirring for 0.5-2 minutes.
4. The method for preparing the high-hardness, high-wear-resistant, lightweight, high-entropy alloy according to claim 2, characterized in that, The smelting process is carried out under a protective gas atmosphere.
5. The method for preparing the high-hardness, high-wear-resistant, lightweight, high-entropy alloy according to claim 2, characterized in that, The smelting step is repeated 2 to 10 times.
6. The method for preparing a high-hardness, high-wear-resistant, lightweight, high-entropy alloy according to claim 2, characterized in that, Before the smelting step, the process also includes a gas washing step for the metal raw materials, a deoxygenation step for the smelting environment, and / or a cleaning step for the alloy ingots after smelting.
7. The application of the high-hardness, high-wear-resistant, lightweight, high-entropy alloy of claim 1 in the preparation of products with high hardness.
8. The application of the high-hardness, high-wear-resistant, lightweight, high-entropy alloy according to claim 1 in the preparation of products with high wear resistance.