Preparation method of titanium@network magnesium titanate magnesium electric positive electrode material, product and application

A two-step chemical solution method was used to prepare titanium@network magnesium titanate cathode material, which solved the problem of insufficient electrochemical performance of magnesium titanate and enabled the application of magnesium batteries with high specific capacity and stable cycle.

CN117832433BActive Publication Date: 2026-11-24SHANGHAI NAT ENG RES CENT FORNANOTECH +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311795888.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2026-11-24
Estimated Expiration
2043-12-25

AI Technical Summary

Technical Problem

The existing magnesium titanate has insufficient electrochemical performance, which limits its application in magnesium batteries.

Method used

A titanium@network magnesium titanate cathode material was prepared by a two-step chemical solution method, and the electrochemical performance of the material was improved by coating and network structure.

Benefits of technology

This improved the electrochemical performance of the material, enabling it to exhibit higher specific capacity and cycle stability in magnesium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117832433B_ABST
    Figure CN117832433B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a titanium@network magnesium titanate cathode material. The method involves adding titanium salt and a strong alkali to deionized water and stirring until homogeneous. The mixture is then transferred to a three-necked flask, stirred, and purged with argon gas. Ethanol is added to the mixture, and a reducing agent dissolved in deionized water is rapidly added to the solution. The mixture is centrifuged and washed to obtain a network Ti@TiO. Magnesium salt is added to oleylamine, stirred, and purged with Ar gas. The solution is gradually heated to 120–150 °C to dissolve the magnesium salt. Alcohol is injected into the solution, and the mixture is stirred, heated, and allowed to cool naturally to room temperature. The Ti@TiO and the cooled liquid are stirred thoroughly, heated to dryness, and calcined to obtain the final product. The titanium@network magnesium titanate exhibits an initial discharge specific capacity of approximately 198 mAh / g at a charge / discharge rate of 0.5 C, and after 50 cycles, the discharge specific capacity is approximately 184 mAh / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to magnesium battery cathode materials, their preparation and application, specifically a method for preparing a titanium@networked magnesium titanate cathode material, as well as its products and applications. Background Technology

[0002] With the development of human society, the contradiction between the global shortage of energy resources and the ever-increasing demand for energy is becoming increasingly acute. Developing battery systems with high energy density has become a major goal of current power systems. Although lithium-ion batteries, with their high energy density and environmental friendliness, are widely used in portable mobile devices such as mobile phones and laptops, as well as in electric bicycles and electric vehicles, their safety remains a significant concern, and much work remains to be done in their application as power batteries. Magnesium, one of the most abundant light metal elements on Earth, is widely used in many fields due to its excellent physicochemical properties. Current research on rechargeable magnesium batteries is largely based on rechargeable lithium-ion batteries. Because magnesium and lithium are located diagonally opposite each other in the periodic table, besides having similar atomic radii and chemical properties, magnesium has a much higher melting point (648.8 ℃) than lithium (180.5 ℃) and is less reactive, making rechargeable magnesium batteries safer. Although its specific capacity is not as high as that of lithium (3862 mAh g⁻¹), it is still quite considerable (2205 mAh g⁻¹). Moreover, my country has extremely abundant magnesium resources, and the price of magnesium is much lower than that of lithium. Furthermore, magnesium is environmentally friendly, so rechargeable magnesium batteries are attracting increasing attention.

[0003] Magnesium sulfide is a perovskite-structured compound that, due to its high dielectric constant, can also be used as a cathode material for magnesium-ion batteries. It is considered a promising magnesium-ion cathode material.

[0004] This invention provides a method for preparing titanium@networked magnesium titanate cathode material. The method employs a two-step chemical solution process to prepare the titanium@networked magnesium titanate. The electrochemical performance of the material is improved through coating and the network structure. This preparation process is relatively simple and easy to operate. Summary of the Invention

[0005] To overcome the shortcomings of existing magnesium titanate electrochemical performance, the present invention aims to provide a method for preparing titanium@networked magnesium titanate cathode material.

[0006] Another object of the present invention is to provide a titanium@network magnesium titanate cathode material product obtained by the above method.

[0007] Another object of the present invention is to provide an application of the above-mentioned product.

[0008] The objective of this invention is achieved through the following scheme: a method for preparing titanium@networked magnesium titanate cathode material, characterized by preparing titanium@networked magnesium titanate through a two-step chemical solution method, the specific steps of which are as follows: (1) Add 3-5 g of soluble titanium and 1.2-2.0 g of strong base to deionized water and stir for 1-2 h until uniform. Then transfer the mixture to a three-necked flask and continue stirring for 20-30 min. Then introduce inert gas argon for 20-30 min. (2) Add 100-150 μL of ethanol to the above mixture, dissolve 10-15g of reducing agent in deionized water, and add the reducing agent solution to the above solution quickly while stirring. After 30-60 min, centrifuge and wash with deionized water and anhydrous ethanol 3-5 times to obtain network Ti@TiO. (3) Add 0.02 to 0.04 mmol of magnesium salt to 10 to 15 mL of oleylamine, stir magnetically to form a mixed solution, then introduce inert gas Ar into it for 20 to 30 min, and gradually heat the mixed solution to 120 to 150 °C to dissolve all the magnesium salt into a solution. (4) Inject alcohol into the above solution, wherein the molar ratio of magnesium salt to alcohol is 1:8. Stir magnetically for 30 to 60 min at this temperature, then heat to 160 to 180 °C. Keep the reaction mixture at this temperature for 20 to 30 min, and then cool naturally to room temperature. (5) Mix Ti@TiO from step (2) with step (4), stir evenly, heat to evaporate the solvent, and calcine in a muffle furnace at 500-700 ℃ for 3-5 h to obtain titanium@network magnesium titanate cathode material.

[0009] Preferably, the titanium salt is one or a combination of tetrabutyl titanate or tetraisopropyl titanate.

[0010] Preferably, the strong base is one or a combination of sodium hydroxide or potassium hydroxide.

[0011] Preferably, the reducing agent is one or a combination of hydrazine hydrate or sodium borohydride.

[0012] Preferably, the magnesium salt is one or a combination of magnesium acetate, magnesium nitrate, or magnesium chloride.

[0013] Preferably, the alcohol is one or a combination of ethylene glycol or glycerol.

[0014] This invention provides a titanium@networked magnesium titanate cathode material, prepared according to any of the methods described above.

[0015] This invention provides an application of titanium@networked magnesium titanate cathode material in magnesium battery cathode materials.

[0016] Beneficial effects: This invention provides a method for preparing titanium@networked magnesium titanate cathode material. The method employs a two-step chemical solution process to prepare the titanium@networked magnesium titanate. The electrochemical performance of the material is improved through coating and the network structure. This preparation process is relatively simple and easy to operate. Attached Figure Description

[0017] Figure 1 This is a lifetime diagram of the titanium@networked magnesium titanate cathode material in Example 1.

[0018] from Figure 1 Titanium@networked magnesium titanate has an initial discharge specific capacity of approximately 198 mAh / g at a charge-discharge rate of 0.5 C, and after 50 cycles, the discharge specific capacity is approximately 184 mAh / g. Detailed Implementation

[0019] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0020] Example 1 A titanium@networked magnesium titanate cathode material is prepared by a two-step chemical solution method, according to the following steps: (1) Add 3 g of soluble titanium salt tetrabutyl titanate and 1.2 g of sodium hydroxide to deionized water and stir for 1 h until uniform. Then transfer the mixture to a three-necked flask and continue stirring for 30 min. Then introduce inert gas argon for 30 min. (2) Add 100 μL of ethanol to the above mixture, dissolve 10 g of sodium borohydride reducing agent in deionized water, and add the sodium borohydride solution to the above ethanol solution quickly while stirring. After 60 min, centrifuge and wash 5 times with deionized water and anhydrous ethanol to obtain network Ti@TiO. (3) Add 0.02 mmol magnesium acetate to 10 mL oleylamine, stir magnetically to form a mixed solution, then introduce inert gas Ar into it for 30 min, and gradually heat the mixed solution to 150 °C to dissolve all the magnesium acetate into a solution. (4) Inject ethylene glycol into the above solution, wherein the molar ratio of magnesium salt to ethylene glycol is 1:8. Stir magnetically for 60 min at this temperature, then heat to 160°C, keep the reaction mixture at this temperature for 30 min, and then cool naturally to room temperature. (5) Mix Ti@TiO from step (2) and the product from step (4), stir evenly, heat to evaporate the solvent, and calcine in a muffle furnace at 500°C for 5 h to obtain titanium@network magnesium titanate cathode material.

[0021] Figure 1 This is a lifetime diagram of the titanium@network magnesium titanate cathode material. At a charge / discharge rate of 0.5 C, the initial discharge specific capacity of the titanium@network magnesium titanate is approximately 198 mAh / g, and after 50 cycles, the discharge specific capacity is approximately 184 mAh / g.

[0022] Example 2 A titanium@networked magnesium titanate cathode material is prepared by a two-step chemical solution method, according to the following steps: (1) Add 4 g of soluble titanium salt tetraisopropyl titanate and 1.6 g of strong base sodium hydroxide to deionized water and stir for 1 hour until uniform. Then transfer the mixture to a three-necked flask, continue stirring for 20 minutes, and then introduce inert gas argon for 20 minutes to obtain the mixture. (2) Add 120 μL of ethanol to the above mixture, dissolve 10 g of reducing agent hydrazine hydrate in deionized water, and add the reducing agent solution to the above solution quickly while stirring. After 30 min, centrifuge and wash 5 times with deionized water and anhydrous ethanol to obtain network Ti@TiO. (3) Add 0.02 mmol magnesium nitrate to 10 mL oleylamine, stir magnetically to form a mixed solution, then introduce inert gas Ar into it for 30 min, and gradually heat the mixed solution to 140 °C to dissolve all the magnesium salt into a solution. (4) Inject glycerol into the solution obtained in step (3), wherein the molar ratio of magnesium nitrate to glycerol is 1:8. Stir magnetically for 60 min at this temperature, then heat to 180°C and hold for 20 min, and then cool naturally to room temperature. (5) Mix Ti@TiO from step (2) with step (4), stir evenly, heat to evaporate the solvent, and calcine in a muffle furnace at 600℃ for 5 h to obtain titanium@network magnesium titanate cathode material.

[0023] Example 3 A titanium@networked magnesium titanate cathode material is prepared by a two-step chemical solution method, according to the following steps: (1) Add 5 g of soluble tetrabutyl titanate and 2.0 g of potassium hydroxide to deionized water and stir for 2 h until uniform. Then transfer the mixture to a three-necked flask and continue stirring for 30 min. Then introduce inert argon gas for 30 min. (2) Add 150 μL of ethanol to the above mixture, dissolve 15 g of sodium borohydride in deionized water, and add the sodium borohydride solution to the above solution quickly while stirring. After 60 min, centrifuge and wash 5 times with deionized water and anhydrous ethanol to obtain network Ti@TiO. (3) Add 0.04 mmol magnesium chloride to 15 mL oleylamine, stir magnetically to form a mixed solution, then introduce inert gas Ar into it for 30 min, and gradually heat the mixed solution to 120 °C to dissolve all the magnesium salts into a solution. (4) Inject ethylene glycol into the above solution, wherein the molar ratio of magnesium chloride to ethylene glycol is 1:8. Stir magnetically for 60 min at this temperature, then heat to 180 °C, keep the reaction mixture at this temperature for 20 min, and then cool naturally to room temperature. (5) Mix Ti@TiO from step (2) with step (4), stir evenly, heat to evaporate the solvent, and calcine in a muffle furnace at 700 ℃ for 3 h to obtain titanium@network magnesium titanate cathode material.

Claims

1. A preparation method of a titanium@network-like magnesium titanate magnesium electric positive electrode material, characterized in that, Titanium@networked magnesium titanate cathode material was prepared by a two-step chemical solution method, including the following steps: (1) Add 3-5 g of soluble titanium salt and 1.2-2.0 g of strong base to deionized water and stir for 1-2 h until uniform. Then transfer the mixture to a three-necked flask and continue stirring for 20-30 min. Then introduce inert gas argon for 20-30 min. (2) Add 100-150 μL of ethanol to the above mixture, dissolve 10-15 g of reducing agent in deionized water, and add the reducing agent solution to the above solution quickly while stirring. After 30-60 min, centrifuge and wash with deionized water and anhydrous ethanol 3-5 times to obtain network Ti@TiO. (3) Add 0.02 to 0.04 mmol of magnesium salt to 10 to 15 mL of oleylamine, stir magnetically to form a mixed solution, then introduce inert gas Ar into it for 20 to 30 min, and gradually heat the mixed solution to 120 to 150 °C to dissolve all the magnesium salt into a solution. (4) Inject alcohol into the above solution, wherein the molar ratio of magnesium salt to alcohol is 1:8, stir magnetically for 30 to 60 min at this temperature, then heat to 160 to 180°C, keep the reaction mixture at this temperature for 20 to 30 min, and then cool naturally to room temperature; (5) Mix Ti@TiO from step (2) with step (4), stir evenly, heat to evaporate the solvent, and calcine in a muffle furnace at 500-700℃ for 3-5 h to obtain titanium@network magnesium titanate cathode material.

2. The method for preparing a titanium@networked magnesium titanate cathode material according to claim 1, characterized in that, In step (1), the titanium salt is one or a combination of tetrabutyl titanate or tetraisopropyl titanate; the strong base is one or a combination of sodium hydroxide or potassium hydroxide.

3. The method for preparing a titanium@networked magnesium titanate cathode material according to claim 1, characterized in that, In step (2), the reducing agent is one or a combination of hydrazine hydrate or sodium borohydride.

4. The method for preparing a titanium@networked magnesium titanate cathode material according to claim 1, characterized in that, In step (3), the magnesium salt is one or a combination of magnesium acetate, magnesium nitrate, or magnesium chloride.

5. The method for preparing a titanium@networked magnesium titanate cathode material according to claim 1, characterized in that, In step (4), the alcohol is one of ethylene glycol or glycerol or a combination thereof.

6. The method for preparing a titanium@networked magnesium titanate cathode material according to any one of claims 1 to 5, characterized in that, Prepare according to the following steps: (1) Add 3 g of soluble titanium salt tetrabutyl titanate and 1.2 g of sodium hydroxide to deionized water and stir for 1 h until uniform. Then transfer the mixture to a three-necked flask and continue stirring for 30 min. Then introduce inert gas argon for 30 min. (2) Add 100 μL of ethanol to the above mixture, dissolve 10 g of sodium borohydride reducing agent in deionized water, and add the sodium borohydride solution to the above ethanol solution quickly while stirring. After 60 min, centrifuge and wash 5 times with deionized water and anhydrous ethanol to obtain network Ti@TiO. (3) Add 0.02 mmol magnesium acetate to 10 mL oleylamine, stir magnetically to form a mixed solution, then introduce inert gas Ar into it for 30 min, and gradually heat the mixed solution to 150 °C to dissolve all the magnesium acetate into a solution. (4) Inject ethylene glycol into the above solution, wherein the molar ratio of magnesium salt to ethylene glycol is 1:

8. Stir magnetically for 60 min at this temperature, then heat to 160°C, keep the reaction mixture at this temperature for 30 min, and then cool naturally to room temperature. (5) Mix Ti@TiO from step (2) and the product from step (4), stir evenly, heat to evaporate the solvent, and calcine in a muffle furnace at 500°C for 5 h to obtain titanium@network magnesium titanate cathode material.

7. The method for preparing a titanium@networked magnesium titanate cathode material according to any one of claims 1 to 5, characterized in that, Prepare according to the following steps: (1) Add 4 g of soluble titanium salt tetraisopropyl titanate and 1.6 g of strong base sodium hydroxide to deionized water and stir for 1 hour until uniform. Then transfer the mixture to a three-necked flask, continue stirring for 20 minutes, and then introduce inert gas argon for 20 minutes to obtain the mixture. (2) Add 120 μL of ethanol to the above mixture, dissolve 10 g of reducing agent hydrazine hydrate in deionized water, and add the reducing agent solution to the above solution quickly while stirring. After 30 min, centrifuge and wash 5 times with deionized water and anhydrous ethanol to obtain network Ti@TiO. (3) Add 0.02 mmol magnesium nitrate salt to 10 mL oleylamine, stir magnetically to form a mixed solution, then introduce inert gas Ar into it for 30 min, and gradually heat the mixed solution to 140 °C to dissolve all the magnesium salt into a solution. (4) Inject glycerol into the solution obtained in step (3), wherein the molar ratio of magnesium nitrate to glycerol is 1:

8. Stir magnetically for 60 min at this temperature, then heat to 180℃ and hold for 20 min, and then cool naturally to room temperature. (5) Mix Ti@TiO from step (2) with step (4), stir evenly, heat to evaporate the solvent, and calcine in a muffle furnace at 600℃ for 5 h to obtain titanium@network magnesium titanate cathode material.

8. The method for preparing a titanium@networked magnesium titanate cathode material according to any one of claims 1 to 5, characterized in that, Prepare according to the following steps: (1) Add 5 g of soluble tetrabutyl titanate and 2.0 g of potassium hydroxide to deionized water and stir for 2 h until uniform. Then transfer the mixture to a three-necked flask and continue stirring for 30 min. Then introduce inert gas argon for 30 min. (2) Add 150 μL of ethanol to the above mixture, dissolve 15 g of sodium borohydride in deionized water, and add the sodium borohydride solution to the above solution quickly while stirring. After 60 min, centrifuge and wash 5 times with deionized water and anhydrous ethanol to obtain network Ti@TiO. (3) Add 0.04 mmol magnesium chloride to 15 mL oleylamine, stir magnetically to form a mixed solution, then introduce inert gas Ar into it for 30 min, and gradually heat the mixed solution to 120 °C to dissolve all the magnesium salts into a solution. (4) Inject ethylene glycol into the above solution, wherein the molar ratio of magnesium chloride to ethylene glycol is 1:

8. Stir magnetically for 60 min at this temperature, then heat to 180 °C, keep the reaction mixture at this temperature for 20 min, and then cool naturally to room temperature. (5) Mix Ti@TiO from step (2) and step (4), stir evenly, heat to evaporate the solvent, and calcine in a muffle furnace at 700 ℃ for 3 h to obtain titanium@network magnesium titanate cathode material.

9. A titanium@networked magnesium titanate cathode material, prepared according to the method described in any one of claims 1-8.

10. The application of the titanium@network magnesium titanate cathode material according to claim 9 in magnesium battery cathode materials.

Citation Information

Patent Citations

  • Preparation method and application of titanate-based hollow material

    CN113880134A

  • Preparation method of magnesium titanate and superoxide magnesium titanate battery material as well as product and application of magnesium titanate and superoxide magnesium titanate battery material

    CN115367789A