Preparation method of low-melting polyester chip resistant to phenolic yellowing

By adjusting the polyester molecular chain structure and adding stabilizers, low-melting-point polyester chips resistant to phenolic yellowing were prepared, solving the problem of phenolic yellowing of low-melting-point fibers in textiles, achieving yellowing resistance at high temperatures, and broadening the application range of low-melting-point polyesters.

CN117843941BActive Publication Date: 2026-11-24四川东材新材料有限责任公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410061648.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-16
Publication Date
2026-11-24
Estimated Expiration
2044-01-16

AI Technical Summary

Technical Problem

Existing low-melting-point fibers are prone to phenolic yellowing in textiles, leading to a decline in appearance and performance. Current technologies cannot effectively solve this problem, especially since low-melting-point polyester chips are more prone to yellowing when bonded at high temperatures, making it difficult to meet market demands.

Method used

By adjusting the polyester molecular chain structure, using raw materials such as isophthalic acid, sodium ethylene glycol isophthalate-5-sulfonate, and diethylene glycol, combined with hydrolysis-resistant aluminum-based catalysts and phosphoric acid stabilizers, esterification and vacuum polycondensation reactions are carried out to prepare phenol-resistant low-melting-point polyester chips. This process disrupts the regularity of the polyester, increases the number of terminal carboxyl groups, and reduces oxidative degradation, thereby achieving phenol-resistant yellowing.

Benefits of technology

The prepared phenol-resistant low-melting-point polyester chips exhibit good performance in the temperature range of 90–150℃, effectively preventing yellowing of textiles and broadening the application range of low-melting-point polyesters. They are suitable for low-melting-point fibers used in shoe material bonding, ensuring bonding performance while overcoming yellowing problems.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a method for preparing phenol-resistant, low-melting-point polyester chips. The method comprises the following steps: ethylene glycol and sodium isophthalic acid-5-sulfonate are added to a reaction vessel for esterification to obtain ethylene glycol isophthalate-5-sulfonate; terephthalic acid, isophthalic acid, ethylene glycol, and diethylene glycol are added to the reaction vessel for esterification; after esterification, sodium isophthalate-5-sulfonate, a catalyst, and a stabilizer are added; a vacuum polycondensation reaction is carried out at a higher temperature; after the reaction, the reacted material is cooled and sliced ​​to obtain phenol-resistant, low-melting-point polyester chips. Using this invention, the melting point of the phenol-resistant, low-melting-point polyester chips is 90–150°C. After being prepared into fibers, the phenol-resistant, low-melting-point polyester chips achieve a phenol-resistant yellowing grade ≥3, solving the problem of poor phenol-resistant yellowing in textile products made from ordinary low-melting-point polyester chips. This method is particularly suitable for use as a low-melting-point fiber for shoe bonding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention pertains to the preparation of organic polymer compounds, specifically a method for preparing low-melting-point polyester chips resistant to phenolic yellowing. The phenolic yellowing-resistant low-melting-point polyester chips prepared by this invention are particularly suitable for use as low-melting-point fibers in shoe material bonding. Background Technology

[0002] Yellowing of textiles severely affects their appearance and performance. Before a textile product is sold, it undergoes a complex and time-consuming process involving dyeing and finishing, storage, transportation, and sample display. Even during use, improper wearing, washing, or storage can cause color changes. As people's living standards improve, the demand for stable textile quality also increases, leading to frequent claims due to color variations. In recent years, textile producers, sellers, and third-party testing organizations have paid close attention to abnormal color changes in textiles, conducting effective analyses and proposing measures to reduce and improve yellowing.

[0003] In existing technologies, low-melting-point fibers are produced by composite spinning of general polyester and modified low-melting-point polyester. These low-melting-point fibers melt at a lower temperature than general polyester, creating a bonded core or parallel structure fibers that melt and bond with other fibers. They are an important raw material for producing nonwoven fabrics and adhesive materials using thermal bonding processes. In special fields, it is necessary to evaluate the material's resistance to phenolic yellowing. Usually, finishing methods are used to make ordinary textiles meet the standards. However, due to their lower melting point, low-melting-point fibers are not suitable for direct finishing, and some application sectors do not support finishing of finished products. Because low-melting-point polyester is modified, its molecular chain structure is looser than that of general polyester, making it more prone to phenolic yellowing. Therefore, solving the problem of phenolic yellowing resistance of materials from the raw material end has become a difficult but challenging issue.

[0004] Currently, most phenol-resistant textiles on the market are post-treatment additives, and the technology for phenol-resistant textiles made from polyester chips with a melting point of 90-150℃ is not yet mature and cannot meet market demand. Chinese patent application publication number CN109021509A discloses "a phenol-resistant functional masterbatch, its preparation method, uses, and phenol-resistant polyester," with the technical solution involving mixed extrusion to form the masterbatch. The drawback is that this physical modification results in unevenness, and the product is a conventional melting point polyester, not a low-melting-point polyester. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing phenol-resistant low-melting-point polyester chips. This provides a method for preparing phenol-resistant low-melting-point polyester chips that solves the problem of poor phenol-resistant yellowing in textile products made from ordinary low-melting-point polyester chips.

[0006] The present invention relates to a method for preparing low-melting-point polyester chips resistant to phenolic yellowing, characterized by the following steps: a. Preparation of ethylene glycol 5-sulfonate sodium isophthalate: ethylene glycol and ethylene glycol 5-sulfonate sodium are added to a reactor equipped with a process tower (existing technology equipment) at a molar ratio of ethylene glycol to ethylene glycol 5-sulfonate sodium of 1.5-2:1. After esterification reaction under normal pressure, ethylene glycol 5-sulfonate sodium isophthalate sodium isophthalate is obtained. The water produced by the esterification reaction is heated by the reaction itself, evaporates and rises to the process tower of the reactor. After being condensed in the process tower, it is separated from the reaction system. The weight of the separated water is recorded. When the water separated from the reaction system reaches 90-95% of the theoretical output water, the reaction is stopped. The theoretical output water is the amount of water theoretically produced after the reaction of sodium isophthalic acid-5-sulfonate with excess ethylene glycol. b. Take 15-25 parts by weight of terephthalic acid, 5-15 parts by weight of isophthalic acid, 7-17 parts by weight of ethylene glycol and 2-7 parts by weight of diethylene glycol, and put them into a reactor with a process tower. The esterification reaction is carried out under normal pressure. The water generated by the esterification reaction is heated by the reaction itself, evaporated and rises to the process tower of the reactor. After being condensed by the process tower, it is separated from the reaction system. The weight of the separated water is recorded. c. When the reaction in step b is separated along with the water in the reaction system, and the weight record reaches 80-95% of the theoretical water output, the esterification reaction is considered to be over. Then add 1-3 parts by weight of ethylene glycol 5-sulfonate sodium isophthalate, 4-15 parts by weight of catalyst and 2-4 parts by weight of stabilizer. The theoretical output water volume is the amount of water theoretically generated after terephthalic acid and isophthalic acid react with excess ethylene glycol and diethylene glycol; d. Heat the material to carry out a vacuum polycondensation reaction. After the reaction, shut off the reactor and connect it to the vacuum system, and introduce nitrogen gas to bring the reactor to positive pressure. Cool the reacted material and slice (granulate) it to obtain phenol-resistant, low-melting-point polyester chips.

[0007] The method for preparing phenol-resistant, low-melting-point polyester chips described in this invention is characterized by the following steps: a. Preparation of ethylene glycol 5-sulfonate sodium isophthalate: ethylene glycol and ethylene glycol 5-sulfonate sodium isophthalate are added to a reactor with a process tower according to the molar ratio of ethylene glycol to ethylene glycol 5-sulfonate sodium is 1.5-2:1. After esterification reaction under normal pressure, ethylene glycol 5-sulfonate sodium isophthalate sodium isophthalate is obtained. The water produced by the esterification reaction is heated by the reaction itself, evaporates and rises to the process tower of the reactor. After being condensed in the process tower, it is separated from the reaction system. The weight of the separated water is recorded. When the water separated from the reaction system reaches 90-95% of the theoretical output water, the reaction is stopped. The theoretical output water is the amount of water theoretically produced after the reaction of sodium isophthalic acid-5-sulfonate with excess ethylene glycol. The reaction temperature is 130–160°C, and the reaction time is 3–4 hours. b. Take 15-25 parts by weight of terephthalic acid, 5-15 parts by weight of isophthalic acid, 7-17 parts by weight of ethylene glycol and 2-7 parts by weight of diethylene glycol, and put them into a reactor with a process tower. The esterification reaction is carried out under normal pressure. The water generated by the esterification reaction is heated by the reaction itself, evaporated and rises to the process tower of the reactor. After being condensed by the process tower, it is separated from the reaction system. The weight of the separated water is recorded. The reaction temperature is 220–280°C; c. When the reaction in step b is separated along with the water in the reaction system, and the weight record reaches 80-95% of the theoretical water output, the esterification reaction is considered to be over. Then add 1-3 parts by weight of ethylene glycol 5-sulfonate sodium isophthalate, 4-15 parts by weight of catalyst and 2-4 parts by weight of stabilizer. The theoretical output water volume is the amount of water theoretically generated after terephthalic acid and isophthalic acid react with excess ethylene glycol and diethylene glycol; d. Heat to 260-290℃ and carry out vacuum polycondensation reaction at a pressure of 10-100Pa. After the reaction time is 2.5-3h, shut off the reactor and connect it to the vacuum system, and introduce nitrogen gas to the reactor to positive pressure. Cool the reacted material and slice (granulate) it to obtain phenol-resistant low-melting-point polyester chips.

[0008] In this invention: the melting point of the phenol-resistant low-melting-point polyester chips obtained in step d is 90-150°C, and the phenol-resistant low-melting-point polyester chips, after being prepared into fibers, have a phenol-resistant yellowing grade ≥3.

[0009] In this invention, the stabilizer is a phosphate-based polyester stabilizer.

[0010] In this invention, the phosphoric acid-based polyester stabilizer is trimethyl phosphate.

[0011] In this invention, the catalyst is either an aluminum-based catalyst resistant to hydrolysis or an aluminum-based catalyst not resistant to hydrolysis. The aluminum-based catalyst resistant to hydrolysis is an ethylene glycol solution of tetrabutyl titanate-ethanol complex (the product manufacturer and product model are: Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences, Al-Ⅰ), and the aluminum-based catalyst not resistant to hydrolysis is an ethylene glycol solution of tetrabutyl titanate (the product manufacturer and product model are: Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences, Al-Ⅱ).

[0012] Compared with the prior art, the present invention has the following features and beneficial effects: (1) The reason for the yellowing of polyester is that the phenolic substances in the packaging material react with the nitrogen oxides in the air and are transferred to the fabric, resulting in the yellowing of the fabric. The principle of preparing phenol-resistant yellowing low melting point polyester in this invention is as follows: the melting point is the thermodynamic equilibrium between the crystalline phase and the amorphous phase, that is, the change in free energy ΔG=0→ΔG=ΔH-TΔS=0, where ΔH (heat of fusion) marks the energy required for molecules or chain segments to leave the crystal lattice, which is related to the strength of the intermolecular interaction force. The benzene rings of the polyester macromolecular chain are in the same plane, which makes adjacent serrated macromolecules interlocked with each other, resulting in high crystallinity of polyester and a high ΔH. ΔS (entropy of fusion) marks the change in the degree of molecular disorder before and after melting, which is related to the flexibility of the molecular chain. There are a large number of benzene ring structures in the PET molecular chain, and the ester group in the repeating unit forms a conjugated system with the benzene ring, which results in high rotational resistance of the molecular chain and strong rigidity, which can only move as a whole, thus having a small ΔS. The high melting point of PET is due to its large ΔH and small ΔS. This invention addresses this by adding isophthalic acid, sodium ethylene glycol isophthalate-5-sulfonate, and diethylene glycol to disrupt the regularity of the polyester and improve the rigidity of the polyester molecular chain, thereby producing low-melting-point polyester chips. Because the regularity of the polyester molecular chain is disrupted, the number of terminal carboxyl groups in the polyester is increased, making the polyester acidic. Furthermore, by adding stabilizers, the oxidative degradation of the polyester is reduced, and the transfer of phenolic substances into the polyester is prevented. Textiles made from the prepared polyester chips can achieve a phenolic yellowing resistance level of ≥3. The catalyst used in this invention is a highly efficient, green, and non-toxic aluminum-based catalyst, replacing toxic, heavy metal antimony-based catalysts. Existing technologies have not yet solved the problem of phenolic yellowing resistance in low-melting-point polyesters. Solving this problem will help broaden the application range of low-melting-point polyesters. The characteristics of yellowing resistance, low melting point, and safety and environmental protection endow polyester with high quality. (2) Using the present invention, terephthalic acid, isophthalic acid, sodium ethylene glycol 5-sulfonate, ethylene glycol, diethylene glycol, catalyst and stabilizer are combined to achieve the effect of low melting point and resistance to phenolic yellowing by adjusting the structure of molecular chain and the ratio between each substance. A phenolic yellowing resistant low melting point polyester chip is prepared with a melting point in the range of 90 to 150°C. Phenolic yellowing resistant low melting point polyester chips in this melting point range can be customized according to customer requirements and have good performance. (3) The preparation process of this invention is simple and can solve the problem of poor phenol yellowing resistance of textile products made of ordinary low melting point polyester chips. It fills the market demand gap and can broaden the high-end applications of low melting point polyester chips. The phenol yellowing resistant low melting point polyester chips made can be used as low melting point fibers for shoe material bonding, which can not only ensure the bonding effect but also overcome the pain point of yellowing. It is highly practical. Detailed Implementation

[0013] The embodiments given below are intended to clearly and completely describe the technical solutions of the present invention, so that those skilled in the art can better understand the advantages and features of the present invention, thereby making a clearer definition of the scope of protection of the present invention; the embodiments described in the present invention are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0014] Example 1: A method for preparing phenol-resistant, low-melting-point polyester chips, comprising the following steps: a. Preparation of ethylene glycol 5-sulfonate sodium isophthalate: Ethylene glycol and ethylene glycol 5-sulfonate sodium isophthalate are added to a reactor equipped with a process tower (existing technology, hereinafter the same) at a molar ratio of 2:1. The esterification reaction is carried out under normal pressure at a temperature of 150°C. The water produced by the esterification reaction is heated by the reaction itself, evaporates and rises to the process tower of the reactor. After condensation in the process tower, it is separated from the reaction system. The weight of the separated water is recorded. When the water separated from the reaction system reaches 90% of the theoretical output, the reaction is stopped, and ethylene glycol 5-sulfonate sodium isophthalate is obtained. The reaction time is 3 hours. The theoretical output is the amount of water theoretically produced after the reaction of ethylene glycol 5-sulfonate sodium with excess ethylene glycol. b. Take 15 parts by weight of terephthalic acid, 15 parts by weight of isophthalic acid, 7 parts by weight of ethylene glycol and 7 parts by weight of diethylene glycol, and put them into a reactor with a process tower. The esterification reaction is carried out under normal pressure at a temperature of 240°C. The water generated by the esterification reaction is heated by the reaction itself, evaporates and rises to the process tower of the reactor. After being condensed by the process tower, it is separated from the reaction system. The weight of the separated water is recorded. c. When the reaction in step b is separated out along with the water in the reaction system, and the weight record reaches 95% of the theoretical water output, the esterification reaction is considered to be over. Then add 3 parts by weight of ethylene glycol 5-sulfonate sodium isophthalate, 15 parts by weight of catalyst and 4 parts by weight of stabilizer trimethyl phosphate. The catalyst is an aluminum-based catalyst resistant to hydrolysis, specifically an ethylene glycol solution of tetrabutyl titanate-ethanol complex (the product manufacturer and product model are: Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences, Al-I). The theoretical output water volume is the amount of water theoretically generated after terephthalic acid and isophthalic acid react with excess ethylene glycol and diethylene glycol; d. Heat to 260℃ and carry out vacuum polycondensation reaction at a pressure of 20Pa. After the reaction time is 3 hours, close the reactor and connect it to the vacuum system, and introduce nitrogen gas to the reactor to positive pressure. Cool the reacted material and slice (granulate) it to obtain phenol-resistant low-melting-point polyester chips.

[0015] Testing revealed that the phenol-resistant low-melting-point polyester chips prepared in this embodiment had a melting point of 90°C and an intrinsic viscosity of 0.67 dl / g. After spinning into short fibers, the phenol-resistant yellowing resistance was tested to level 3. The testing method was based on GB / T 29778-2013 "Textiles - Color Fastness Tests: Evaluation of Potential Phenolic Yellowing".

[0016] Example 2: A method for preparing phenol-resistant, low-melting-point polyester chips, comprising the following steps: a. Preparation of ethylene glycol 5-sulfonate sodium isophthalate: Ethylene glycol and ethylene glycol 5-sulfonate sodium isophthalate were added to a reactor equipped with a process tower at a molar ratio of 1.5:1. Esterification was carried out at atmospheric pressure and a reaction temperature of 130℃. The water produced by the esterification reaction was heated by the reaction itself, evaporated, and rose to the process tower of the reactor. After condensation in the process tower, the water was separated from the reaction system. The weight of the separated water was recorded. When the water separated from the reaction system reached 95% of the theoretical output, the reaction was stopped, thus obtaining ethylene glycol 5-sulfonate sodium isophthalate. The reaction time was 4 hours. The theoretical output is the amount of water theoretically produced after the reaction of ethylene glycol 5-sulfonate sodium with excess ethylene glycol. b. Take 25 parts by weight of terephthalic acid, 15 parts by weight of isophthalic acid, 17 parts by weight of ethylene glycol and 2 parts by weight of diethylene glycol, and put them into a reactor with a process tower. The esterification reaction is carried out under normal pressure at a temperature of 250°C. The water generated by the esterification reaction is heated by the reaction itself, evaporates and rises to the process tower of the reactor. After being condensed by the process tower, it is separated from the reaction system. The weight of the separated water is recorded. c. When the reaction in step b is separated out along with the water in the reaction system, and the weight record reaches 95% of the theoretical water output, the esterification reaction is considered to be over. Then add 1 part by weight of ethylene glycol 5-sulfonate sodium isophthalate, 4 parts by weight of catalyst and 2 parts by weight of stabilizer trimethyl phosphate. The catalyst is an aluminum-based catalyst that is resistant to hydrolysis, specifically an ethylene glycol solution of tetrabutyl titanate (the product manufacturer and product model is: Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences, Al-II). The theoretical output water volume is the amount of water theoretically generated after terephthalic acid and isophthalic acid react with excess ethylene glycol and diethylene glycol; d. Heat to 270℃ and carry out vacuum polycondensation reaction at a pressure of 100Pa. After the reaction time is 2.5h, shut off the reactor and connect it to the vacuum system, and introduce nitrogen gas to the reactor to positive pressure. Cool the reacted material and slice (granulate) it to obtain phenol-resistant low-melting-point polyester chips.

[0017] Testing revealed that the phenol-resistant low-melting-point polyester chips prepared in this embodiment had a melting point of 150°C and an intrinsic viscosity of 0.69 dl / g. After spinning into short fibers, the phenol-resistant yellowing resistance was tested to level 4. The testing method was based on GB / T 29778-2013 "Textiles - Color Fastness Tests: Evaluation of Potential Phenolic Yellowing".

[0018] Example 3: A method for preparing phenol-resistant, low-melting-point polyester chips, comprising the following steps: a. Preparation of ethylene glycol 5-sulfonate sodium isophthalate: Ethylene glycol and ethylene glycol 5-sulfonate sodium isophthalate were added to a reactor equipped with a process tower at a molar ratio of 1.7:1. Esterification was carried out at atmospheric pressure and a reaction temperature of 160℃. The water produced by the esterification reaction was heated by the reaction itself, evaporated, and rose to the process tower of the reactor. After condensation in the process tower, the water was separated from the reaction system. The weight of the separated water was recorded. When the water separated from the reaction system reached 92% of the theoretical output, the reaction was stopped, thus obtaining ethylene glycol 5-sulfonate sodium isophthalate. The reaction time was 3.5 hours. The theoretical output is the amount of water theoretically produced after the reaction of ethylene glycol 5-sulfonate sodium with excess ethylene glycol. b. Take 25 parts by weight of terephthalic acid, 15 parts by weight of isophthalic acid, 15 parts by weight of ethylene glycol and 5 parts by weight of diethylene glycol, and put them into a reactor with a process tower. The esterification reaction is carried out under normal pressure at a temperature of 250°C. The water generated by the esterification reaction is heated by the reaction itself, evaporates and rises to the process tower of the reactor. After being condensed by the process tower, it is separated from the reaction system. The weight of the separated water is recorded. c. When the reaction in step b is separated out along with the water in the reaction system, and the weight record reaches 85% of the theoretical water output, the esterification reaction is considered to be over. Then add 2 parts by weight of ethylene glycol 5-sulfonate sodium isophthalate, 10 parts by weight of catalyst and 3 parts by weight of stabilizer trimethyl phosphate. The catalyst is an aluminum-based catalyst resistant to hydrolysis, specifically an ethylene glycol solution of tetrabutyl titanate-ethanol complex (the product manufacturer and product model are: Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences, Al-I). The theoretical output water volume is the amount of water theoretically generated after terephthalic acid and isophthalic acid react with excess ethylene glycol and diethylene glycol; d. Heat to 290℃ and carry out vacuum polycondensation reaction at a pressure of 50Pa. After the reaction time is 2.8h, shut off the reactor and connect it to the vacuum system, and introduce nitrogen gas to the reactor to positive pressure. Cool the reacted material and cut it into chips (granules) to obtain phenol-resistant low-melting-point polyester chips.

[0019] Testing revealed that the phenol-resistant low-melting-point polyester chips prepared in this embodiment had a melting point of 120°C and an intrinsic viscosity of 0.69 dl / g. After spinning into short fibers, the phenol-resistant yellowing resistance was tested to be grade 3.5. The testing method was based on GB / T 29778-2013 "Textiles - Color Fastness Tests: Evaluation of Potential Phenolic Yellowing".

[0020] Example 4: A method for preparing phenol-resistant, low-melting-point polyester chips, comprising the following steps: a. Preparation of ethylene glycol 5-sulfonate sodium isophthalate: ethylene glycol and ethylene glycol 5-sulfonate sodium isophthalate were added to a reactor with a process tower at a molar ratio of 1.5:1 and esterified under normal pressure to obtain ethylene glycol 5-sulfonate sodium isophthalate. The water produced by the esterification reaction is heated by the reaction itself, evaporates and rises to the process tower of the reactor. After being condensed in the process tower, it is separated from the reaction system. The weight of the separated water is recorded. When the water separated from the reaction system reaches 90% of the theoretical output water, the reaction is stopped. The theoretical output water is the amount of water theoretically produced after the reaction of sodium isophthalic acid-5-sulfonate with excess ethylene glycol. The reaction temperature is 130°C; b. Take 15 parts by weight of terephthalic acid, 5 parts by weight of isophthalic acid, 7 parts by weight of ethylene glycol and 2 parts by weight of diethylene glycol, put them into the reactor, and carry out the esterification reaction under normal pressure. The water generated by the esterification reaction is heated by the reaction itself, evaporated and rises to the process tower of the reactor. After being condensed by the process tower, it is separated from the reaction system. The weight of the separated water is recorded. The reaction temperature is 220°C; c. When the reaction in step b is separated out along with the water in the reaction system, and the weight record reaches 80% of the theoretical water output, the esterification reaction is considered to be over. Then add 1 part by weight of ethylene glycol 5-sulfonate sodium isophthalate, 4 parts by weight of catalyst and 2 parts by weight of stabilizer. The theoretical output water volume is the amount of water theoretically generated after terephthalic acid and isophthalic acid react with excess ethylene glycol and diethylene glycol; d. Heat to 260℃ and carry out vacuum polycondensation reaction at a pressure of 10Pa. After the reaction time is 2.5h, shut off the reactor and connect it to the vacuum system, and introduce nitrogen gas to the reactor to positive pressure. Cool the reacted material and slice (granulate) it to obtain phenol-resistant low-melting-point polyester chips.

[0021] Example 5: A method for preparing phenol-resistant, low-melting-point polyester chips, comprising the following steps: a. Preparation of ethylene glycol 5-sulfonate sodium isophthalate: ethylene glycol and ethylene glycol 5-sulfonate sodium isophthalate were added to a reactor with a process tower at a molar ratio of 2:1 and esterified under normal pressure to obtain ethylene glycol 5-sulfonate sodium isophthalate. The water produced by the esterification reaction is heated by the reaction itself, evaporates and rises to the process tower of the reactor. After being condensed in the process tower, it is separated from the reaction system. The weight of the separated water is recorded. When the water separated from the reaction system reaches 95% of the theoretical output water, the reaction is stopped. The theoretical output water is the amount of water theoretically produced after the reaction of sodium isophthalic acid-5-sulfonate with excess ethylene glycol. The reaction temperature is 160°C; b. Take 25 parts by weight of terephthalic acid, 15 parts by weight of isophthalic acid, 17 parts by weight of ethylene glycol and 7 parts by weight of diethylene glycol, put them into the reactor, and carry out the esterification reaction under normal pressure. The water generated by the esterification reaction is heated by the reaction itself, evaporated and rises to the process tower of the reactor. After being condensed by the process tower, it is separated from the reaction system, and the weight of the separated water is recorded. The reaction temperature is 280°C; c. When the reaction in step b is separated from the water in the reaction system and the weight record reaches 95% of the theoretical water output, the esterification reaction is considered to be over. Then add 3 parts by weight of ethylene glycol 5-sulfonate sodium isophthalate, 15 parts by weight of catalyst and 4 parts by weight of stabilizer. The theoretical output water volume is the amount of water theoretically generated after terephthalic acid and isophthalic acid react with excess ethylene glycol and diethylene glycol; d. Heat to 290℃ and carry out vacuum polycondensation reaction at a pressure of 100Pa. After the reaction time is 3 hours, close the reactor and connect it to the vacuum system, and introduce nitrogen gas to the reactor to positive pressure. Cool the reacted material and cut it into chips (granules) to obtain phenol-resistant low-melting-point polyester chips.

[0022] In the above embodiments 4-5: The melting point of the phenol-resistant low-melting-point polyester chips obtained in step d is in the range of 90 to 150°C, and the phenol-resistant low-melting-point polyester chips, after being prepared into fibers, have a phenol-resistant yellowing grade of ≥3. The stabilizer mentioned is a phosphate-based polyester stabilizer; specifically, trimethyl phosphate. The catalyst is either an aluminum-resistant catalyst or a non-aluminum-resistant catalyst. The aluminum-resistant catalyst is an ethylene glycol solution of tetrabutyl titanate-ethanol complex (the product manufacturer and product model are: Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences, Al-Ⅰ). The non-aluminum-resistant catalyst is an ethylene glycol solution of tetrabutyl titanate (the product manufacturer and product model are: Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences, Al-Ⅱ).

[0023] In the above embodiments: unless otherwise specified, the percentage examples used are mass (weight) percentage examples or percentage examples known to those skilled in the art; unless otherwise specified, the proportions used are mass (weight) proportions; the weight parts can all be grams or kilograms.

[0024] In the above embodiments, the process parameters (temperature, time, pressure, etc.) and the values ​​of each component dosage in each step are ranges, and any point can be applied.

[0025] The technical contents of this invention and the above embodiments that are not specifically described are the same as those of the prior art, and the raw materials are all commercially available products.

[0026] The present invention is not limited to the above embodiments; all embodiments described herein can be implemented and have the aforementioned good effects.

Claims

1. A method for preparing phenol-resistant, low-melting-point polyester chips, characterized by the following steps: a. Preparation of ethylene glycol 5-sulfonate sodium isophthalate: ethylene glycol and ethylene glycol 5-sulfonate sodium isophthalate are added to a reactor with a process tower according to the molar ratio of ethylene glycol to ethylene glycol 5-sulfonate sodium is 1.5-2:

1. After esterification reaction under normal pressure, ethylene glycol 5-sulfonate sodium isophthalate sodium isophthalate is obtained. b. Take 15-25 parts by weight of terephthalic acid, 5-15 parts by weight of isophthalic acid, 7-17 parts by weight of ethylene glycol and 2-7 parts by weight of diethylene glycol, and put them into a reactor with a process tower. The esterification reaction is carried out under normal pressure. The water generated by the esterification reaction is separated from the reaction system, and the weight of the separated water is recorded. c. When the reaction in step b is separated from the water in the reaction system and the weight record reaches 80-95% of the theoretical water output, the esterification reaction ends. Then, add 1-3 parts by weight of sodium ethylene glycol isophthalate-5-sulfonate, 4-15 parts by weight of catalyst and 2-4 parts by weight of stabilizer; the stabilizer is a phosphate-based polyester stabilizer. d. Heat the material to carry out a vacuum polycondensation reaction. After the reaction, cool the material and slice it to obtain phenol-resistant, low-melting-point polyester chips.

2. The method for preparing phenol-resistant, low-melting-point polyester chips according to claim 1, characterized in that the steps are as follows: a. Preparation of ethylene glycol 5-sulfonate sodium isophthalate: ethylene glycol and ethylene glycol 5-sulfonate sodium isophthalate are added to a reactor with a process tower according to the molar ratio of ethylene glycol to ethylene glycol 5-sulfonate sodium is 1.5-2:

1. After esterification reaction under normal pressure, ethylene glycol 5-sulfonate sodium isophthalate sodium isophthalate is obtained. The reaction temperature is 130–160°C, and the reaction time is 3–4 hours. b. Take 15-25 parts by weight of terephthalic acid, 5-15 parts by weight of isophthalic acid, 7-17 parts by weight of ethylene glycol and 2-7 parts by weight of diethylene glycol, and put them into a reactor with a process tower. The esterification reaction is carried out under normal pressure. The water generated by the esterification reaction is separated from the reaction system, and the weight of the separated water is recorded. The reaction temperature is 220–280°C; c. When the reaction in step b is separated out along with the water in the reaction system, and the weight record reaches 80-95% of the theoretical water output, the esterification reaction ends. Then add 1-3 parts by weight of ethylene glycol 5-sulfonate sodium isophthalate, 4-15 parts by weight of catalyst and 2-4 parts by weight of stabilizer. d. Heat to 260-290℃ and carry out vacuum polycondensation reaction at a pressure of 10-100Pa for 2.5-3 hours. After the reaction, cool the material and slice it to obtain phenol-resistant, low-melting-point polyester chips.

3. The method for preparing phenol-resistant, low-melting-point polyester chips according to claim 2, characterized in that: The melting point of the phenol-resistant low-melting-point polyester chips obtained in step d is 90-150℃, and the phenol-resistant low-melting-point polyester chips, after being prepared into fibers, have a phenol-resistant yellowing grade of ≥3.

4. The method for preparing phenol-resistant, low-melting-point polyester chips according to claim 1, characterized in that: The phosphoric acid-based polyester stabilizer is trimethyl phosphate.

5. The method for preparing phenol-resistant, low-melting-point polyester chips according to claim 1, characterized in that: The catalyst is an ethylene glycol solution of tetrabutyl titanate-ethanol complex or an ethylene glycol solution of tetrabutyl titanate.

Citation Information

Patent Citations

  • Phenolic yellowing-resistant functional master batch, preparation method thereof, use thereof and phenolic yellowing-resistant polyester

    CN109021509A

  • Manufacturing method of low-melting-point polyester granules

    CN102585185A

  • Preparation method for non-crystalline low-melting point polyester hot melt adhesive

    CN102732202A