A kind of high temperature and high humidity resistant halogen-free flame-retardant cable material for nuclear power cable
By cryogenically embrittlement and pulverization of the base material, polyimide, and layered silicate, combined with polyisobutylene and optimized formulation, the cracking problem of nuclear-powered ship cable material under high temperature and high humidity environment was solved, resulting in a high-performance cable material with long service life and excellent radiation resistance.
Patent Information
- Application Number
- CN202410135383.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-31
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-01-31
AI Technical Summary
Existing cable materials for nuclear-powered ships are insufficient in terms of high temperature and humidity resistance and radiation resistance. In particular, they are prone to cracking in high temperature and humidity environments, and the processing performance and cost of existing materials are relatively high.
By pre-cryogenically embrittled the base material, polyimide, and layered silicate, and then air-jet pulverizing them to form micronized particles, and mixing them with the layered silicate to form a stable interlayer structure, combined with the use of polyisobutylene, the barrier properties and mechanical properties of the material are improved. At the same time, the ratio of halogen-free flame retardant and antioxidant is optimized to achieve the material's high temperature and high humidity and radiation resistance properties.
The cable material does not crack for a long time under high temperature, high pressure and high humidity conditions, and has a thermal life of more than 84.7 years at 90℃. It has excellent radiation resistance and insulation properties, meeting the requirements of nuclear power plant cables.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to a high-temperature and high-humidity halogen-free flame-retardant cable material for nuclear power cables, belonging to the field of cable material technology. Background Technology
[0002] The thermal life requirement for cables used in third-generation nuclear power plants is 90℃ / 60 years, along with halogen-free, low-smoke, flame-retardant properties and a certain level of radiation resistance. The complete technical requirements for cables used in fourth-generation nuclear power plants are not yet fully finalized. In practice, the thermal life requirement has increased from 90℃ / 60 years for third-generation nuclear power to 90℃ / 80 years, while the radiation resistance requirement is higher under normal operating conditions (withstanding...). 60 Co-γ ray cumulative dose 412.5 kGy / room temperature) and under accident conditions (DBA and AG, resistant) 60 The Co-γ ray cumulative dose is 2064 kGy / room temperature, yet it still maintains a certain degree of insulation.
[0003] As a crucial component of nuclear-powered ships, cables have higher requirements than conventional cables. They must be resistant to high temperatures and humidity, and their installation involves numerous bends and turns due to the limited space on board. Furthermore, because nuclear-powered ships use atomic energy for power generation, cables used for power transmission connections need to withstand long-term radiation from beta and gamma rays.
[0004] In light of the specific requirements for cables used in nuclear-powered ships, and building upon the basic electrical, physical, mechanical, and radiation resistance properties of nuclear power plant cables, a key issue that needs to be addressed is ensuring the cable sheath maintains good performance under high temperature and humidity conditions. While current nuclear power plant cable materials exhibit excellent performance in terms of radiation resistance and thermal life, their ability to withstand high temperatures and humidity remains significantly insufficient when applied to nuclear-powered ships.
[0005] To improve the performance of the aforementioned cable materials, some methods employ modified polyimide materials. However, due to the high melting point of polyimide, processing temperatures are generally required to be above 300°C, which hinders its blending with other materials and limits its application range, making it unsuitable for many formulation systems. To overcome the limitations of polyimide in cable material applications, existing methods, such as the thermoplastic polyimide cable material for nuclear power and aviation disclosed in Chinese patent application (publication number CN111040448A), utilize polyetherimide-siloxane copolymers. The presence of siloxane improves the material's processing performance. However, the plasticizing blending temperature for this type of material must still be above 250°C. If blended with cable materials containing hydroxide flame retardants, such high processing temperatures can cause partial or complete decomposition and inactivation of the hydroxide flame retardants. Therefore, while this type of material is suitable for polyimide-based cable material systems, it is unsuitable for conventional halogen-free, low-smoke flame-retardant cable material systems, and the cost of using siloxane graft modification is relatively high. For example, the high flame-retardant, low-smoke, halogen-free sheathing material composition for nuclear-powered ship cables disclosed in Chinese patent application (publication number: CN109705449A) includes ethylene-acrylate copolymer, polyester elastomer, nylon elastomer, polyethylene, compatibilizer, flame retardant, flame retardant synergist, radiation resistant additives, etc. Its thermal life can only reach more than 40 years, and it cannot meet the specific requirements in terms of radiation resistance and high temperature and humidity resistance. Moreover, the amount of flame retardant in this cable material is extremely high, and it is very easy to absorb moisture in high humidity environment, which will lead to a reduction or even failure of its flame retardancy. Summary of the Invention
[0006] To address the problems existing in the prior art, this invention provides a high-temperature and high-humidity halogen-free flame-retardant cable material for nuclear power cables, solving the problem of how to improve the high-temperature and high-humidity resistance of the cable material while also providing radiation resistance.
[0007] The objective of this invention is achieved through the following technical solution: a high-temperature, high-humidity, halogen-free, low-smoke, flame-retardant cable material for nuclear power cables, characterized in that the cable material comprises the following components in parts by weight:
[0008] Base material: 100; polyimide: 50-100; layered silicate: 8.0-15; halogen-free flame retardant: 30-80; antioxidant: 4.0-12; radiation resistant agent: 1.0-12; the base material, polyimide and layered silicate are pre-formed into a masterbatch by cryogenic embrittlement followed by airflow pulverization; the base material includes at least two of ethylene-methyl methacrylate copolymer, ethylene-ethyl acrylate copolymer and polyisobutylene, and the base material contains polyisobutylene.
[0009] By first embrittled and then pulverized the base material, polyimide, and layered silicate, micronized particles are formed. This effectively avoids the processing difficulties caused by the high processing temperature and hardness of polyimide, eliminating the need for grafting modification of polyimide with siloxanes and increasing the proportion of polyimide added. Since polyimide has high flame retardancy, a higher polyimide content also reduces the amount of inorganic flame retardant needed, which helps maintain the physical and mechanical properties of the cable material. Simultaneously, mixing the base material, polyimide, and layered silicate to form micronized particles allows these particles to stably exist within the silicate's interlayer structure. This relatively stable interlayer structure greatly restricts the diffusion pathways of small gas and liquid molecules within the material, preventing rapid diffusion on a three-dimensional scale and forcing them to migrate slowly along the interlayer gaps. This results in a superior overall barrier against external corrosive substances. Meanwhile, the interlayer structure can improve the mechanical properties, thermal stability, aging resistance, electrical properties, and processability of the composite material. The layered silicate and the subsequently added halogen-free flame retardant also have a synergistic effect, resulting in excellent overall combustion crust formation and a significant smoke suppression effect. Through the above-mentioned reasonable formulation design, the light transmittance in the combustion smoke of the material can reach over 75%, and the radiation resistance of the material is also improved. On the other hand, by ensuring that the base material contains at least polyisobutylene, a material with excellent barrier and airtight properties, it can form a synergistic effect with nano-layered silicate, achieving even better barrier performance. This allows it to maintain excellent high-temperature and high-humidity resistance in high-humidity environments such as ships. The overall thermal life of the cable material of this invention reaches over 90℃ / 84.7 years under normal operating conditions (resistance... 60 The cumulative dose of Co-γ rays reaches 412 kGy / day above room temperature and under accident conditions (DBA and AG, resistant to 60 The cumulative dose of Co-γ rays reaches over 2060 kGy / room temperature, and the insulation performance meets the requirements of nuclear power plant cables. More importantly, the cable does not crack under high temperature, high pressure, high humidity and long duration (peak temperature 209℃, 2MPa saturated vapor pressure, time 2 hours, 4 hours, 15 days), indicating that the material has excellent resistance to high temperature and high humidity, thus ensuring its application in nuclear-powered ships.
[0010] In the aforementioned high-temperature, high-humidity, halogen-free, low-smoke, flame-retardant cable material for nuclear power cables, preferably, the embrittlement and subsequent pulverization and mixing treatment specifically involves: pre-cryogenically cooling the base material, polyimide, and layered silicate at -100℃ to -150℃, followed by airflow impact at low temperature to form fine particles and achieve uniform mixing. Because these fine particles have relatively high surface energy, they can form stable aggregates that are difficult to form at room temperature. More preferably, the particle size of the intercalation mixing masterbatch is between 0.5μm and 5μm. As a more preferred embodiment, the polyimide can be first cryogenically pulverized at -100℃ to -150℃ using airflow, and then mixed with the base material and layered silicate, followed by cryogenically pulverized and mixed at -100℃ to -150℃. This allows the polyimide to more easily penetrate the interlayer structure of the layered silicate during the pulverization and mixing process, improving the overall performance.
[0011] In the aforementioned high-temperature, high-humidity, halogen-free, low-smoke, flame-retardant cable material for nuclear power cables, preferably, the polyimide is formed by reacting diphenyl ether tetracarboxylic anhydride with aromatic diamine.
[0012] In the above-mentioned high-temperature and high-humidity halogen-free low-smoke flame-retardant cable material for nuclear power cables, preferably, the base material is a mixture of ethylene-methyl methacrylate copolymer, ethylene-ethyl acrylate copolymer and polyisobutylene, and the mass ratio of ethylene-methyl methacrylate copolymer: ethylene-ethyl acrylate copolymer: polyisobutylene is 1:0.5~0.8:3.0~3.5.
[0013] In the aforementioned high-temperature, high-humidity, halogen-free, low-smoke, flame-retardant cable material for nuclear power cables, preferably, the layered silicate is nanoscale, and the nano-layered silicate is selected from organically modified montmorillonite, i.e., prepared by organically treating sodium-based montmorillonite with a long-chain quaternary ammonium salt cationic surfactant. Organically modified montmorillonite, the base material, and polyimide may undergo a solid-phase chemical reaction during cryogenic pulverization and mixing, forming a more stable intercalated composite structure.
[0014] In the above-mentioned high-temperature and high-humidity halogen-free low-smoke flame-retardant cable material for nuclear power cables, preferably, the radiation-resistant agent is selected from one or more of ferrocene, 2-amino-5-(p-methoxyphenyl)-1,3,4-thiadiazole lanthanum complex, and 6-benzylaminopurine copper complex, which can make the material as a whole have better aging resistance and radiation resistance.
[0015] In the aforementioned high-temperature, high-humidity, halogen-free, low-smoke flame-retardant cable material for nuclear power cables, preferably, the halogen-free flame retardant is selected from one or more of aluminum hydroxide, aluminum diethylphosphinate, and melamine cyanurate. Because this invention increases the amount of polyimide added through micronization, and polyimide itself also has flame-retardant properties, the amount of halogen-free flame retardant added can be reduced. This reduces the problems of hygroscopicity and decreased physical and mechanical properties of the cable material caused by the presence of inorganic flame retardants. As a further preferred embodiment, the weight percentage of the halogen-free flame retardant is 35–70. Preferably, the halogen-free flame retardant is a mixture of aluminum hydroxide and aluminum diethylphosphinate, with a mass ratio of 1:0.3–0.6.
[0016] In the aforementioned high-temperature, high-humidity, halogen-free, low-smoke flame-retardant cable material for nuclear power cables, the antioxidant can be an asymmetric hindered phenolic calixarene high molecular weight primary antioxidant, a phosphite antioxidant, a hindered phenolic antioxidant, etc. Preferably, the antioxidant is selected from a combination of an asymmetric hindered phenolic calixarene high molecular weight primary antioxidant and a phosphite high molecular weight secondary antioxidant. The aforementioned asymmetric hindered phenolic calixarene is selected from asymmetric hindered phenolic calixarene[4]arene and / or asymmetric hindered phenolic calixarene[6]arene, and the phosphite high molecular weight secondary antioxidant, such as antioxidant 168, antioxidant 3010, etc., preferably has a mass ratio of 1:0.5 to 0.7.
[0017] In summary, compared with the prior art, the present invention has the following advantages:
[0018] 1. By first cryogenically embrittled the base material, polyimide, and layered silicate, and then air-jet pulverizing them, micronized particles are formed. These particles are then mixed with the layered silicate to form an interlayer structure, which plays a significant barrier role, giving the material excellent high temperature and high humidity resistance.
[0019] 2. By including at least polyisobutylene in the base material, the aim is to achieve a synergistic effect with layered silicates, thereby giving the material as a whole better barrier properties.
[0020] 3. The cable material of the present invention can still maintain the cable without cracking under high temperature, high pressure and high humidity environment for a long time (the peak temperature is 209°C, the saturated vapor pressure is 2MPa, and the time is 2 hours, 4 hours and 15 days), and has the performance of high temperature and high humidity resistance.
[0021] 4. The overall thermal life of the cable material of this invention reaches over 84.7 years at 90℃, under normal operating conditions (resistant to...). 60 The cumulative dose of Co-γ rays reaches 412 kGy / day above room temperature and under accident conditions (DBA and AG, resistant to 60The cumulative dose of Co-γ rays reaches 2060 kGy / room temperature or higher, and the insulation performance meets the requirements of nuclear power plant cables. It also has good resistance to bending cracks, radiation resistance, insulation performance, halogen-free flame retardant performance and smoke suppression performance. Detailed Implementation
[0022] The technical solution of the present invention will be further described in detail below through specific embodiments, but the present invention is not limited to these embodiments.
[0023] Example 1
[0024] This high-temperature, high-humidity, halogen-free, low-smoke, flame-retardant cable material for nuclear power cables comprises the following components by weight:
[0025] Base material: 100; Polyimide: 50; Layered silicate: 8; Halogen-free flame retardant: 70; Antioxidant: 10; Radiation resistant agent: 5; The base material, polyimide, and layered silicate are pre-emulsified and then pulverized and mixed to form an intercalation masterbatch; The base material includes ethylene-methyl methacrylate copolymer and polyisobutylene, and the mass ratio of polyisobutylene to ethylene-methyl methacrylate copolymer in the base material is 3:1. Specifically, the above-mentioned emulsification and pulverization and mixing treatment is as follows: According to the above-mentioned proportions of raw materials, the base material, polyimide, and layered silicate are pre-treated by low-temperature cryogenic airflow pulverization and mixing at -100℃ to -150℃ to form micronized particles. The above-mentioned layered silicate is nano-sized modified montmorillonite (obtained by organic treatment of sodium-based montmorillonite with long-chain quaternary ammonium salt cationic surfactant), and the polyimide is formed by reacting diphenyl ether tetracarboxylic anhydride with aromatic diamine. The antioxidant is a combination of asymmetric hindered phenolic calixarene high molecular weight primary antioxidant and phosphite high molecular weight secondary antioxidant, such as asymmetric hindered phenolic calixarene[4] and antioxidant 168 mixed, and the mass ratio of the two is 1:0.5. The halogen-free flame retardant is aluminum hydroxide, and the radiation retardant is 2-amino-5-(p-methoxyphenyl)-1,3,4-thiadiazole lanthanum complex.
[0026] The aforementioned high-temperature, high-humidity, halogen-free, low-smoke, flame-retardant cable material for nuclear power cables can be manufactured using the following methods:
[0027] According to the above proportions of raw materials, the mixture of polyimide, substrate, and nano-layered silicate is first subjected to cryogenic airflow pulverization, using cryogenic liquid nitrogen as the cooling medium, and the temperature is controlled at -100℃ to -150℃ to form mixed micro powder of 0.5μm to 5μm. Through the above cryogenic treatment, the raw materials can be embrittled at ultra-low temperatures, which makes it easy to pulverize during the pulverization process, effectively replacing the more complex or expensive processing methods such as high-temperature processing and siloxane grafting modification.
[0028] The above-obtained mixed micro powder raw materials, halogen-free flame retardant, antioxidant, and radiation retardant are mixed evenly in a twin-screw extruder according to the above proportions. The extrusion temperature is controlled at 160℃~200℃ and the twin-screw speed is 300 rpm. The mixture is then extruded and granulated to obtain a high-temperature and high-humidity halogen-free low-smoke flame-retardant cable material for cable sheathing.
[0029] Manufacturing of wires and cables
[0030] The high-temperature and high-humidity halogen-free smoke-repellent flame-retardant cable material obtained above is added to an extruder at an extrusion temperature of 150℃~200℃. After being extruded into wires and cables, the materials are irradiated by an electron accelerator. Through electron beam excitation, the polymer composite material is cross-linked by irradiation at an irradiation dose of 80kGy~200kGy to obtain the corresponding wire and cable products.
[0031] The obtained cable material was subjected to corresponding performance tests. It was tested for a long time under high temperature, high pressure and high humidity conditions (the peak temperature was 209℃, the saturated vapor pressure was 2MPa, and the time was 2 hours, 4 hours and 15 days respectively). No cable cracking was observed, indicating that it has the performance of high temperature and high humidity resistance.
[0032] Example 2
[0033] This high-temperature, high-humidity, halogen-free, low-smoke, flame-retardant cable material for nuclear power cables comprises the following components by weight:
[0034] Base material: 100; Polyimide: 100; Layered silicate: 15; Halogen-free flame retardant: 40; Antioxidant: 4.0; Radiation resistant agent: 5.0; The base material, polyimide, and layered silicate are pre-emulsified and then pulverized and mixed to form an intercalation masterbatch; The base material includes ethylene-methyl methacrylate copolymer and polyisobutylene, and the mass ratio of polyisobutylene to ethylene-methyl methacrylate copolymer in the base material is 3.5:1. Specifically, the above-mentioned emulsification and pulverization and mixing treatment is as follows: According to the above-mentioned proportions of raw materials, the base material, polyimide, and layered silicate are pre-treated by low-temperature cryogenic airflow pulverization and mixing at -100℃ to -150℃ to form micronized particles. The above-mentioned layered silicate is nano-sized modified montmorillonite (obtained by organic treatment of sodium-based montmorillonite with long-chain quaternary ammonium salt cationic surfactant), and the polyimide is mainly formed by the reaction of diphenyl ether tetracarboxylic anhydride and aromatic diamine. The antioxidant is a combination of asymmetric hindered phenolic calixarene high molecular weight primary antioxidant and phosphite high molecular weight secondary antioxidant. Asymmetric hindered phenolic calixarene[4] and antioxidant 168 are mixed, and the mass ratio of the two is 1:0.7. The halogen-free flame retardant is a mixture of aluminum hydroxide and aluminum diethylphosphinate, and the dosage ratio of the two is 1:0.6. The radiation retardant is 6-benzylaminopurine copper complex.
[0035] The specific preparation method of the high-temperature and high-humidity halogen-free low-smoke flame-retardant cable material for nuclear power cables in this embodiment is the same as that in Embodiment 1, and will not be repeated here.
[0036] The obtained cable material was subjected to corresponding performance tests. It was tested for a long time under high temperature, high pressure and high humidity conditions (the peak temperature was 209℃, the saturated vapor pressure was 2MPa, and the time was 2 hours, 4 hours and 15 days respectively). The results showed that no cable cracking occurred, indicating that it has the performance of high temperature and high humidity resistance.
[0037] Example 3
[0038] This high-temperature, high-humidity, halogen-free, low-smoke, flame-retardant cable material for nuclear power cables comprises the following components by weight:
[0039] Base material: 100; polyimide: 70; layered silicate: 11; halogen-free flame retardant: 50; antioxidant: 7.0; radiation retardant: 6.0; wherein, the base material, polyimide and layered silicate are pre-embrittled and then crushed and mixed to form an intercalation mixing masterbatch; the base material includes ethylene-methyl methacrylate copolymer, ethylene-ethyl acrylate copolymer and polyisobutylene, and the mass ratio of polyisobutylene: ethylene-methyl methacrylate copolymer: ethylene-ethyl acrylate copolymer in the base material is 3:1:0.5. Specifically, the above-mentioned embrittlement and subsequent crushing and mixing treatment is as follows: according to the above-mentioned proportions of raw materials, the base material, polyimide and layered silicate are subjected to low-temperature deep cryogenic airflow crushing and mixing treatment at -100℃ to -150℃ to form micronized particles. The above-mentioned layered silicate is made of nano-sized modified montmorillonite (made by organic treatment of sodium-based montmorillonite with long-chain quaternary ammonium salt cationic surfactant). The polyimide is mainly formed by the reaction of diphenyl ether tetracarboxylic anhydride and aromatic diamine. The antioxidant is a combination of asymmetric hindered phenolic calixarene high molecular weight main antioxidant and phosphite high molecular weight auxiliary antioxidant. Asymmetric hindered phenolic calixarene [6] is mixed with antioxidant 3010, and the mass ratio of the two is 1:0.6. The halogen-free flame retardant is aluminum hydroxide, and the radiation retardant is 2-amino-5-(p-methoxyphenyl)-1,3,4-thiadiazole lanthanum complex.
[0040] The specific preparation method of the high-temperature and high-humidity halogen-free low-smoke flame-retardant cable material for nuclear power cables in this embodiment is the same as that in Embodiment 1, and will not be repeated here.
[0041] The obtained cable material was subjected to corresponding performance tests. It was tested for a long time under high temperature, high pressure and high humidity conditions (the peak temperature was 209℃, the saturated vapor pressure was 2MPa, and the time was 2 hours, 4 hours and 15 days respectively). The results showed that no cable cracking occurred, indicating that it has the property of not cracking and also has the property of high temperature and high humidity resistance.
[0042] Example 4
[0043] This high-temperature, high-humidity, halogen-free, low-smoke, flame-retardant cable material for nuclear power cables comprises the following components by weight:
[0044] Base material: 100; polyimide: 90; layered silicate: 14; halogen-free flame retardant: 45; antioxidant: 8.0; radiation retardant: 8.0; wherein, the base material, polyimide and layered silicate are pre-emulsified and then crushed and mixed to form an intercalation mixing masterbatch; the base material includes ethylene-methyl methacrylate copolymer, ethylene-ethyl acrylate copolymer and polyisobutylene, and the mass ratio of polyisobutylene: ethylene-methyl methacrylate copolymer: ethylene-ethyl acrylate copolymer in the base material is 3:1:0.8. Specifically, the above-mentioned embrittlement and subsequent pulverization and mixing process is as follows: according to the above-mentioned proportions of raw materials, the base material, polyimide, and layered silicate are subjected to low-temperature cryogenic airflow pulverization and mixing treatment at -100℃ to -150℃ to form micronized particles. The above-mentioned layered silicate is made of nano-sized modified montmorillonite (obtained by organic treatment of sodium-based montmorillonite with long-chain quaternary ammonium salt cationic surfactant). The polyimide is mainly formed by the reaction of diphenyl ether tetracarboxylic anhydride and aromatic diamine. The antioxidant is a combination of asymmetric hindered phenolic calixarene high molecular weight primary antioxidant and phosphite high molecular weight secondary antioxidant. The asymmetric hindered phenolic calixarene[4] is mixed with antioxidant 168, and the mass ratio of the two is 1:0.5. The halogen-free flame retardant is aluminum hydroxide. The radiation retardant is a mixture of ferrocene and 2-amino-5-(p-methoxyphenyl)-1,3,4-thiadiazole lanthanum complex, and the mass ratio of the two is 1:0.5.
[0045] The specific preparation method of the high-temperature and high-humidity halogen-free low-smoke flame-retardant cable material for nuclear power cables in this embodiment is the same as that in Embodiment 1, and will not be repeated here.
[0046] The obtained cable material was subjected to corresponding performance tests. It was tested for a long time under high temperature, high pressure and high humidity conditions (the peak temperature was 209℃, the saturated vapor pressure was 2MPa, and the time was 2 hours, 4 hours and 15 days respectively). The results showed that no cable cracking occurred, indicating that it has the property of not cracking and also has the property of high temperature and high humidity resistance.
[0047] Comparative Example 1
[0048] To better illustrate the importance of the composition of the cable material of the present invention, this comparative example was carried out by not adding polyisobutylene to the material (based on the material formulation in Example 1, without adding polyisobutylene) and the performance was tested.
[0049] This halogen-free, low-smoke, flame-retardant cable material for nuclear power cables comprises the following components by weight:
[0050] Base material: 100; Polyimide: 50; Layered silicate: 8; Halogen-free flame retardant: 70; Antioxidant: 12; Radiation resistant agent: 5; The base material, polyimide, and layered silicate are pre-emulsified and then pulverized and mixed to form an intercalation masterbatch; the base material is entirely ethylene-methyl methacrylate copolymer. Specifically, the above-mentioned emulsification and pulverization and mixing treatment is as follows: according to the above-mentioned proportions of raw materials, the base material, polyimide, and layered silicate are pre-treated by low-temperature cryogenic airflow pulverization and mixing at -100℃ to -150℃ to form micronized particles. The above-mentioned layered silicate is nano-scale modified montmorillonite (obtained by organic treatment of sodium-based montmorillonite with long-chain quaternary ammonium salt cationic surfactant), and the polyimide is mainly formed by the reaction of diphenyl ether tetracarboxylic anhydride and aromatic diamine. The antioxidant is a combination of asymmetric hindered phenolic calixarene high molecular weight primary antioxidant and phosphite high molecular weight secondary antioxidant, such as asymmetric hindered phenolic calixarene[4] and antioxidant 168 mixed, and the mass ratio of the two is 1:0.5. The halogen-free flame retardant is aluminum hydroxide, and the radiation retardant is 2-amino-5-(p-methoxyphenyl)-1,3,4-thiadiazole lanthanum complex.
[0051] The specific manufacturing method is the same as in Example 1, and will not be repeated here.
[0052] The obtained cable material was subjected to corresponding performance tests. It was tested for a long time under high temperature, high pressure and high humidity conditions (the peak temperature was 209℃, the saturated vapor pressure was 2MPa, and the time was 2 hours, 4 hours and 15 days respectively). The results showed that the cable cracked during the 15-day test.
[0053] Comparative Example 2
[0054] This comparative example was implemented and its performance tested by not adding layered silicates to the material (based on the material formulation in Example 1).
[0055] This high-temperature, high-humidity, halogen-free, low-smoke, flame-retardant cable material for nuclear power cables comprises the following components by weight:
[0056] Base material: 100; Polyimide: 50; Halogen-free flame retardant: 70; Antioxidant: 12; Radiation resistant agent: 5; The base material and polyimide are pre-emulsified and then pulverized and mixed to form a mixed masterbatch; The base material includes ethylene-methyl methacrylate copolymer and polyisobutylene, and the mass ratio of polyisobutylene to ethylene-methyl methacrylate copolymer in the base material is 3:1. Specifically, the above-mentioned emulsification and pulverization and mixing treatment is as follows: According to the above-mentioned proportions of raw materials, the base material and polyimide are pre-treated by low-temperature cryogenic airflow pulverization and mixing at -100℃ to -150℃ to form micronized particles. The polyimide is mainly formed by the reaction of diphenyl ether tetracarboxylic anhydride and aromatic diamine. The antioxidant is a combination of asymmetric hindered phenolic calixarene high molecular weight primary antioxidant and phosphite high molecular weight secondary antioxidant, such as asymmetric hindered phenolic calixarene[4] and antioxidant 168 mixed, and the mass ratio of the two is 1:0.5. The halogen-free flame retardant is aluminum hydroxide, and the radiation retardant is 2-amino-5-(p-methoxyphenyl)-1,3,4-thiadiazole lanthanum complex.
[0057] The obtained cable material was subjected to corresponding performance tests. It was tested for a long time under high temperature, high pressure and high humidity conditions (the peak temperature was 209℃, the saturated vapor pressure was 2MPa, and the time was 2 hours, 4 hours and 15 days respectively). The results showed that the cable cracked during the 15-day test.
[0058] The specific manufacturing method is the same as in Example 1, and will not be repeated here.
[0059] The test results of Examples 1-4 and Comparative Examples 1 and 2 show that the simultaneous presence of polyisobutylene and layered silicate is crucial for ensuring that the cable material has qualified high temperature and high humidity resistance. Neither can be omitted. Under the action of low temperature cryogenic pulverization process, the two superimposed produce a certain synergistic barrier effect, which has not been found in previous technical literature.
[0060] To better illustrate other properties of the cable material of the present invention, cable materials obtained in the corresponding embodiments above were randomly selected for relevant performance tests. The specific test methods and results are as follows:
[0061] Physical and mechanical property testing
[0062] The physical and mechanical properties were tested in accordance with the GB / T 2951 method.
[0063] Electrical performance testing
[0064] Electrical performance was tested according to GB / T 3048.
[0065] Combustion performance test
[0066] Combustion performance was tested according to GB / T 19666 method.
[0067] Thermal life test
[0068] Thermal life was tested according to the method of GB / T 11026.
[0069] Radiation resistance test
[0070] Radiation resistance was tested according to IEC 61244 method.
[0071] Other performance tests are detailed in Tables 1, 2, 3, and 4:
[0072] Table 1:
[0073]
[0074]
[0075]
[0076] Table 2:
[0077]
[0078]
[0079]
[0080] Table 3:
[0081]
[0082]
[0083]
[0084] Table 4:
[0085]
[0086]
[0087]
[0088] As can be seen from the test results in Tables 1-4 above, the cable material of the present invention achieves high temperature and high humidity resistance. Combined with the corresponding performance tests in Examples 1-4, it is shown that under high temperature, high pressure, and high humidity conditions for extended periods (test conditions: peak temperature 209℃, saturated vapor pressure 2MPa) for 2 hours, 4 hours, and 15 days respectively, no cable cracking occurred, demonstrating its non-cracking performance and high temperature and high humidity resistance. Simultaneously, the cable material retains its other properties, exhibiting excellent performance in terms of thermal life, flame retardancy, and radiation resistance. The overall thermal life reaches over 90℃ / 84.7 years. Under normal operating conditions (resistance... 60 (cumulative dose of Co-γ rays) and under accident conditions (DBA and AG, resistance) 60 The cumulative dose of Co-γ rays reached a high level, and the insulation performance met the requirements of nuclear power plant cables.
[0089] Tables 5 and 6 below show the corresponding performance test results of the cable materials in Comparative Example 1 and Comparative Example 2.
[0090] Table 5:
[0091]
[0092]
[0093]
[0094] Table 6
[0095]
[0096]
[0097]
[0098] The specific embodiments described in this invention are merely illustrative of the spirit of the invention. Those skilled in the art to which this invention pertains can make various modifications or additions to the described specific embodiments or use similar methods to replace them, without departing from the spirit of the invention or exceeding the scope defined by the appended claims.
[0099] Although the present invention has been described in detail and specific embodiments have been cited, it will be apparent to those skilled in the art that various changes or modifications can be made without departing from the spirit and scope of the invention.
Claims
1. A high-temperature and high-humidity halogen-free flame-retardant cable material for nuclear power cables, characterized in that, The cable material comprises the following components in parts by weight: Base material: 100; Polyimide: 50-100; Layered silicate: 8.0-15; Halogen-free flame retardant: 30-80; Antioxidant: 4.0-12; Radiation resistant agent: 1.0-12; The base material, polyimide and layered silicate are pre-embrittled and then pulverized and mixed to form an intercalation masterbatch; The base material includes at least two of ethylene-methyl methacrylate copolymer, ethylene-ethyl acrylate copolymer and polyisobutylene, and the base material contains polyisobutylene.
2. The high-temperature and high-humidity halogen-free flame-retardant cable material for nuclear power cables according to claim 1, characterized in that, The embrittlement and subsequent crushing and mixing process specifically involves subjecting the base material, polyimide, and layered silicate to a low-temperature cryogenic airflow crushing and mixing process at -100°C to -150°C.
3. The high-temperature and high-humidity halogen-free flame-retardant cable material for nuclear power cables according to claim 2, characterized in that, The particle size of the intercalated masterbatch is between 0.5 μm and 5 μm.
4. The high-temperature and high-humidity halogen-free flame-retardant cable material for nuclear power cables according to claim 1, characterized in that, The polyimide is mainly formed by reacting diphenyl ether tetracarboxylic anhydride with aromatic diamine.
5. The high-temperature and high-humidity halogen-free flame-retardant cable material for nuclear power cables according to any one of claims 1-4, characterized in that, The base material is a mixture of ethylene-methyl methacrylate copolymer, ethylene-ethyl acrylate copolymer and polyisobutylene, and the mass ratio of ethylene-methyl methacrylate copolymer: ethylene-ethyl acrylate copolymer: polyisobutylene is 1:0.5-0.8:3.0-3.
5.
6. The high-temperature and high-humidity halogen-free flame-retardant cable material for nuclear power cables according to any one of claims 1-4, characterized in that, The layered silicate is nanoscale, and the nanolayered silicate is selected from modified montmorillonite.
7. The high-temperature and high-humidity halogen-free flame-retardant cable material for nuclear power cables according to any one of claims 1-4, characterized in that, The radiation-resistant agent is selected from one or more of ferrocene, 2-amino-5-(p-methoxyphenyl)-1,3,4-thiadiazole lanthanum complex and 6-benzylaminopurine copper complex.
8. The high-temperature and high-humidity halogen-free flame-retardant cable material for nuclear power cables according to any one of claims 1-4, characterized in that, The halogen-free flame retardant is selected from one or more of aluminum hydroxide, aluminum diethylphosphonate, and melamine cyanurate.
9. The high-temperature and high-humidity halogen-free flame-retardant cable material for nuclear power cables according to any one of claims 1-4, characterized in that, The antioxidant is selected from a combination of asymmetric hindered phenolic calixarene high molecular weight primary antioxidant and phosphite high molecular weight secondary antioxidant.
10. The high-temperature and high-humidity halogen-free flame-retardant cable material for nuclear power cables according to claim 9, characterized in that, The asymmetric hindered phenolic calixarene high molecular weight primary antioxidant is selected from asymmetric hindered phenolic calixarene[4]arene and / or asymmetric hindered phenolic calixarene[6]arene, and the phosphite high molecular weight secondary antioxidant is selected from antioxidant 168 and / or antioxidant 3010.
Citation Information
Patent Citations
Nuclear-powered ship cable high-flame-resistance low-smoke halogen-free sheath material, and preparation method thereof
CN109705449A
Thermoplastic polyimide cable material for nuclear power aviation
CN111040448A
Halogen-free low-smoke flame-retardant polyolefin insulating material for nuclear-grade cable
CN115353744A