Humidity-responsive pc / abs composite material and preparation method and application thereof
By introducing covalent organic framework materials into PC/ABS composites, the problems of insufficient humidity response and aging resistance of the materials were solved, achieving accurate humidity response and stable mechanical properties.
Patent Information
- Application Number
- CN202311856182.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-29
AI Technical Summary
Existing PC/ABS composite materials lack humidity response capabilities, making it difficult to achieve intelligent response to environmental humidity and stable aging resistance in specific application scenarios.
By introducing covalent organic framework materials (S-COFs) and utilizing their structural transformation under different humidity conditions, a humidity-responsive PC/ABS composite material was prepared. Combined with a porous framework structure to embed polycarbonate degradation end groups, the material's humidity response and aging resistance properties were achieved.
It achieves accurate response of PC/ABS composite materials to humidity changes and maintains good mechanical properties and stability under high humidity and heat conditions.
Smart Images

Figure BDA0004642277610000061 
Figure BDA0004642277610000062
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer composition technology, and more specifically, to a humidity-responsive PC / ABS composite material, its preparation method, and its application. Background Technology
[0002] PC / ABS composite material is a thermoplastic made from a blend of polycarbonate (PC) and acrylonitrile-butadiene-styrene (ABS). It possesses not only the mechanical strength and high heat distortion temperature of polycarbonate but also the excellent processing and molding properties of ABS, making it widely used in automotive interiors and home appliances. Furthermore, with the diversification of applications, PC / ABS composite materials are required not only to have excellent mechanical properties but also higher demands on their appearance. For example, when using PC / ABS composite materials to manufacture storage boxes or transfer devices for humidity-sensitive items, they need not only excellent and stable impact resistance to adequately protect the contents during transportation or transfer but also the ability to promptly and dynamically reflect the humidity of the internal environment to take quick action and prevent damage to humidity-sensitive items.
[0003] In existing technologies, the modification of PC / ABS mainly focuses on improving aging resistance, flame retardancy, and mechanical properties, lacking improvements in intelligent response. For example, an existing technology discloses a flame-retardant PC / ABS material, which includes PC, ABS, toughening agent, intumescent flame retardant, synergistic flame retardant, organic-inorganic hybrid helical silica fiber, and anti-aging agent. By introducing synergistic flame retardant and organic-inorganic hybrid helical silica fiber into the intumescent flame-retardant system, not only is the flame retardant performance significantly improved, but the mechanical properties are also improved to some extent. However, this material does not possess intelligent response functionality and cannot meet the needs of specific application scenarios. Summary of the Invention
[0004] The purpose of this invention is to overcome the shortcomings and deficiencies of existing PC / ABS composite materials, which are difficult to combine aging resistance and humidity response, and to provide a humidity-responsive PC / ABS composite material.
[0005] Another object of the present invention is to provide a method for preparing a humidity-responsive PC / ABS composite material.
[0006] Another object of the present invention is to provide an application of the above-mentioned humidity-responsive PC / ABS composite material in humidity-responsive enclosure materials.
[0007] The above-mentioned objective of this invention is achieved through the following technical solution:
[0008] This invention protects a humidity-responsive PC / ABS composite material, comprising the following components by weight:
[0009] 30-85 parts polycarbonate, 13-57 parts ABS resin, 1-8 parts toughening agent, and 0.5-3 parts covalent organic framework material;
[0010] The covalent organic framework material is obtained by Schiff base reaction of 2,6-dialdehyde-1,5-dihydroxynaphthalene and 4-(4-aminophenyl)-2,6-bis(4-aminophenyl)pyridine; the polycarbonate has a viscosity-average molecular weight ≥20,000.
[0011] It should be noted that: the mass fraction of polycarbonate in the above-mentioned humidity-responsive PC / ABS composite material is ≥30%; the above-mentioned covalent organic framework material (S-COFs) is a known material, which can be obtained by referring to Huang, Wei, et al. "Solvothermal Synthesis of Microporous, Crystalline Covalent Organic Framework Nanofibers and Their Colorimetric Nanohybrid Structures." Acs Appl Mater Interfaces 5.18(2013):8845-8849. The preparation method is as follows:
[0012] 2,6-Diaaldehyde-1,5-dihydroxynaphthalene, 4-(4-aminophenyl)-2,6-bis(4-aminophenyl)pyridine and an organic solvent were mixed evenly and then reacted at 115-125℃ for 45-50 h. After purification, a covalent organic framework material was obtained. The molar ratio of 2,6-diaaldehyde-1,5-dihydroxynaphthalene to 4-(4-aminophenyl)-2,6-bis(4-aminophenyl)pyridine was (2-4):(1-3).
[0013] Specifically, the process includes the following steps: 2,6-dialdehyde-1,5-dihydroxynaphthalene and 4-(4-aminophenyl)-2,6-bis(4-aminophenyl)pyridine are mixed in ethanol solvent at a molar ratio of 3:2, and the mixture is ultrasonically or stirred at room temperature (25°C) until homogeneous. Then, the mixture is transferred to a high-pressure reactor and reacted at a temperature above 120°C for 48 hours. After filtering and collecting the precipitate, it is thoroughly washed with ethanol, 1,4-dioxane or acetone, and then dried under vacuum to obtain the covalent organic framework material.
[0014] This invention utilizes the fact that the enol structure of a covalent organic framework material can be converted into a ketone structure under different humidity conditions. This interconversion of structures causes the color of the PC / ABS composite material to change with ambient humidity, thus achieving an accurate responsiveness to humidity. More importantly, research has found that when the covalent organic framework material is used as a filler, its stable porous framework structure can encapsulate the end groups generated by the degradation of polycarbonate. This allows the PC / ABS composite material to exhibit humidity responsiveness while also possessing good aging resistance under high humidity and heat conditions, thereby achieving stable mechanical properties.
[0015] It should also be noted that the humidity-responsive PC / ABS composite material of the present invention was placed in a constant temperature and humidity chamber at 25°C. After 2 hours at RH=20%, the L, a, and b values were measured using a colorimeter, representing the primary RH=20% color. Then, it was placed back in the chamber at RH=100% for 2 hours, and the L, a, and b values were measured again, representing the secondary RH=20% color. Finally, it was placed back in the chamber at RH=20% for 2 hours, and the L, a, and b values were measured again, representing the secondary RH=20% color. The results showed that the color difference ΔE between the secondary RH=20% color and the primary RH=20% color was ≤1.5, which fully demonstrates that the humidity-responsive PC / ABS composite material of the present invention has stable humidity responsiveness.
[0016] Preferably, the humidity-responsive PC / ABS composite material comprises: 45-70 parts of polycarbonate, 25-47 parts of ABS resin, 3-6 parts of toughening agent, and 1-1.8 parts of covalent organic framework material.
[0017] Specifically, the viscosity-average molecular weight of the polycarbonate is 25,000–30,000, which can be determined by gel permeation chromatography (GPC), according to GB / T 21863-2008. Using tetrahydrofuran as the eluent, 1–5 mg of sample is mixed with 1 mL of tetrahydrofuran solvent, heated until the sample is completely dissolved, and then injected for testing to obtain the viscosity-average molecular weight of the polycarbonate. Alternatively, the viscosity-average molecular weight of the polycarbonate can be 26,000, 27,000, 28,000, or 29,000.
[0018] The covalent organic framework material (S-COFs) of the present invention is a nanoparticle. When the viscosity-average molecular weight of polycarbonate is 25,000 to 30,000, the covalent organic framework material can be more uniformly dispersed in the resin matrix while maintaining the excellent mechanical properties of the composite material, thereby making the PC / ABS composite material more sensitive to different humidity levels.
[0019] Specifically, the ABS resin is an acrylonitrile-butadiene-styrene terpolymer. Optionally, the mass percentage of butadiene in the acrylonitrile-butadiene-styrene terpolymer is 10% to 20%, and the particle size of butadiene in the acrylonitrile-butadiene-styrene terpolymer is 0.3 to 1.2 μm.
[0020] Specifically, the toughening agent is at least one of the following: an organosilicon core-shell copolymer, a styrene-butadiene-methyl methacrylate terpolymer, and ABS high-resin powder.
[0021] Optionally, the humidity-responsive PC / ABS composite material further includes 0.1 to 1 part by weight of antioxidant and 0.2 to 1 part by weight of lubricant; the antioxidant is at least one of hindered phenolic antioxidant, phosphite antioxidant and thioester antioxidant; the lubricant is pentaerythritol stearate and / or silicone masterbatch.
[0022] In addition, the aforementioned humidity-responsive PC / ABS composite material may also include conventional additives that do not affect its humidity responsiveness, such as one or more of colorants, UV stabilizers, heat stabilizers or flame retardants.
[0023] This invention also protects a method for preparing a humidity-responsive PC / ABS composite material, comprising the following steps:
[0024] A moisture-responsive PC / ABS composite material is obtained by mixing polycarbonate, covalent organic framework material, ABS, toughening agent, lubricant and antioxidant, melting and extruding the mixture.
[0025] Preferably, polycarbonate is premixed with covalent organic framework material for 2-5 minutes, then ABS, toughening agent, lubricant and antioxidant are added and mixed, and then melt-extruded to obtain humidity-responsive PC / ABS composite material.
[0026] The covalent organic framework material (S-COFs) of the present invention is a nanoparticle containing a large number of hydroxyl structures. Compared with mixing multiple components directly together, mixing the covalent organic framework material with polycarbonate first can make the S-COFs more uniformly dispersed in the polycarbonate resin. When mixed with other components, it can be more uniformly dispersed in the entire PC / ABS composite material.
[0027] Specifically, in the above preparation method, a twin-screw extruder can be used for melt extrusion, and the melt extrusion temperature is 150–250°C. Optionally, the specific process parameters of the twin-screw extruder are as follows: metering section temperature 150–190°C, compression section temperature 220–230°C, conveying section temperature 230–250°C, and screw speed 450–550 r / min.
[0028] The application of the above-mentioned humidity-responsive PC / ABS composite material in humidity-responsive enclosure materials is also within the scope of protection of this invention.
[0029] Compared with the prior art, the beneficial effects of the present invention are:
[0030] The humidity-responsive PC / ABS composite material of the present invention utilizes the fact that the enol structure of the covalent organic framework material can interconvert with the ketone structure under different humidity conditions to achieve accurate responsiveness to changes in environmental humidity; and uses the covalent organic framework material as a filler, utilizing its stable porous skeleton structure to embed the end groups generated by the degradation of polycarbonate, so that the PC / ABS composite material has humidity responsiveness and good aging resistance under high humidity and heat conditions, thereby possessing stable mechanical properties. Detailed Implementation
[0031] The present invention will be further described below with reference to specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise stated, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0032] 1. Raw materials and reagents
[0033] Polycarbonate:
[0034] PC-1, with a viscosity-average molecular weight of 26,000, is branded as PC 2100 and manufactured by Wanhua Chemical.
[0035] PC-2, with a viscosity-average molecular weight of 30,000, is branded as PC 2030 and manufactured by Wanhua Chemical.
[0036] PC-3, with a viscosity-average molecular weight of 16,000, brand name LC1500, and manufacturer: Idemitsu.
[0037] ABS resin (acrylonitrile-butadiene-styrene terpolymer):
[0038] The ABS grade is ABS 8434, and the manufacturer is Gaoqiao Petrochemical.
[0039] The toughening agent is MBS (styrene-butadiene-methyl methacrylate copolymer), brand name M-521, manufactured by Kaneka Corporation of Japan;
[0040] Antioxidant 1 is a hindered phenolic antioxidant, brand name SONOX 1076, manufactured by Mitutoyo Chemical.
[0041] Antioxidant 2 is a phosphite antioxidant, brand name SONOX 168, manufactured by Sanfeng Chemical.
[0042] The lubricant is a pentaerythritol stearate lubricant, brand name PETS-AP, manufactured by Faji;
[0043] Covalent organic framework materials (S-COFs) are prepared by the following methods:
[0044] 2,6-dialdehyde-1,5-dihydroxynaphthalene and 4-(4-aminophenyl)-2,6-bis(4-aminophenyl)pyridine were mixed in ethanol solvent at a molar ratio of 3:2 and ultrasonically or by stirring at room temperature (25°C) until homogeneous. The mixture was then transferred to a high-pressure reactor and reacted at a temperature above 120°C for 48 hours. The precipitate was collected by filtration and thoroughly washed with ethanol, 1,4-dioxane or acetone. After vacuum drying, the covalent organic framework material was obtained.
[0045] 2. The humidity-responsive PC / ABS composite materials of the various embodiments and comparative examples of the present invention were prepared by the following method:
[0046] Premix polycarbonate with covalent organic framework material for 2-5 minutes, then add ABS, toughening agent, lubricant and antioxidant, mix and feed into a twin-screw extruder, melt extrude at 150-250℃ to obtain humidity-responsive PC / ABS composite material;
[0047] The specific process parameters of the twin-screw extruder are as follows: metering section temperature is 150~190℃, compression section temperature is 220~230℃, conveying section temperature is 230~250℃, and screw speed is 450~550r / min.
[0048] 3. Performance Testing
[0049] (1) Cantilever beam notched impact test: The PC / ABS composite materials prepared in each example and comparative example were randomly divided into two groups, A and B. Group A was directly tested on a Zwick electronic universal testing machine according to ASTM D256-10 (2018) standard to obtain the notched impact strength X; Group B was first subjected to a damp heat aging test (temperature 85℃, humidity 85%, time 1000h), and then tested on a Zwick electronic universal testing machine according to ASTM D256-10 (2018) standard to obtain the notched impact strength Y.
[0050] Notched impact strength retention rate (%) = X / Y * 100%.
[0051] (2) Humidity response test: The PC / ABS composite materials prepared in each example and comparative example were placed in a constant temperature and humidity chamber at a temperature of 25°C. After being placed under RH=20% for 2 hours, the L, a, and b values were measured using a colorimeter, which is the color at RH=20%. Then, the composite materials were placed back in the constant temperature and humidity chamber and placed under RH=100% for 2 hours. After being placed back in the chamber, the L, a, and b values were measured using a colorimeter, which is the color at RH=100%.
[0052] Examples 1-7 and Comparative Examples 1-3
[0053] The weight parts of each component in the humidity-responsive PC / ABS composite materials of Examples 1-7 and Comparative Examples 1-3 are shown in Table 1.
[0054] Table 1 shows the weight parts of each component in the humidity-responsive PC / ABS composite materials of Examples 1-7 and Comparative Examples 1-3.
[0055]
[0056] The performance test results of the humidity-responsive PC / ABS composite materials in each embodiment and comparative example according to the methods mentioned above are shown in Table 2.
[0057] Table 2 Test results for each embodiment and comparative example
[0058]
[0059] According to the data in Table 2, by comparing the L, a, and b values, it can be seen that the color of the humidity-responsive PC / ABS composite materials in Examples 1-7 at RH=100% has a significant color difference compared to their color at RH=20% (i.e., good humidity responsiveness). Furthermore, it can be observed that the notched impact strength retention rate of the humidity-responsive PC / ABS composite materials in Examples 1-7 after undergoing a double 85% damp heat aging test (temperature 85℃, humidity 85%, time 1000h) reaches over 77% (i.e., excellent resistance to damp heat aging). This fully demonstrates that the humidity-responsive PC / ABS composite material of the present invention not only possesses good humidity responsiveness, with its color changing significantly with changes in ambient humidity, but also exhibits excellent resistance to damp heat aging.
[0060] Examples 3 and 4 show that when polycarbonate comprises 30-85 parts, ABS resin 13-57 parts, toughening agent 1-8 parts, and covalent organic framework material 0.5-3 parts, the PC / ABS composite material exhibits a relatively obvious color response to humidity and possesses a high retention rate of damp heat impact strength. Examples 5 and 6 show that when polycarbonate comprises 45-70 parts, ABS resin 25-47 parts, toughening agent 3-6 parts, and covalent organic framework material 1-1.8 parts, the PC / ABS composite material not only exhibits a more sensitive response to humidity but also achieves a notched impact strength retention rate of over 90%, indicating superior aging resistance.
[0061] As shown in Comparative Example 1, when the amount of covalent organic framework material added is too high, although the notched impact strength of the PC / ABS composite material can be maintained at 95.33%, its L value at RH=20% is 35.29 and at RH=100% is 30.63, which is significantly lower than the L value under the corresponding humidity conditions in the example. The lower L value will result in a darker color of the PC / ABS composite material, thereby reducing the sensitivity of visual observation and making it difficult for the naked eye to distinguish the color change of the PC / ABS composite material under different humidity conditions, thus losing the significance of humidity responsiveness. As shown in Comparative Example 2, when the amount of covalent organic framework material added is too low, although the color change under different humidity is also more obvious, the notched impact strength retention rate is relatively low, indicating that long-term humidity environment will significantly reduce the impact performance of PC / ABS composite material, fully demonstrating the effect of covalent organic framework material on improving the aging resistance of PC / ABS composite material.
[0062] As can be seen from Examples 1 and 2 and Comparative Example 3, when the molecular weight of polycarbonate is too low, the notched impact strength retention rate of PC / ABS composite material after damp heat aging will be too low; when the molecular weight is too high, the viscosity of the system will be too high and the dispersion uniformity of the covalent organic framework material will decrease. Therefore, the molecular weight of polycarbonate is preferably 25,000 to 30,000.
[0063] The above embodiments of the present invention are merely examples for clearly illustrating the present invention and are not intended to limit the implementation of the present invention. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively describe all possible implementations here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the claims of the present invention.
Claims
1. A humidity-responsive PC / ABS composite material, characterized in that, By weight, it includes the following components: 30-85 parts polycarbonate, 13-57 parts ABS resin, 1-8 parts toughening agent, and 0.5-3 parts covalent organic framework material; The covalent organic framework material is obtained by Schiff base reaction of 2,6-dialdehyde-1,5-dihydroxynaphthalene and 4-(4-aminophenyl)-2,6-bis(4-aminophenyl)pyridine; the polycarbonate has a viscosity-average molecular weight of 20,000 to 30,000.
2. The humidity-responsive PC / ABS composite material according to claim 1, characterized in that, The composition includes 45-70 parts of polycarbonate, 25-47 parts of ABS resin, 3.5-6 parts of toughening agent, and 1-1.8 parts of covalent organic framework material.
3. The humidity-responsive PC / ABS composite material according to claim 1, characterized in that, The polycarbonate has a viscosity-average molecular weight of 25,000 to 30,000.
4. The humidity-responsive PC / ABS composite material according to claim 1, characterized in that, The butadiene content in the ABS resin is 10% to 20% by mass.
5. The humidity-responsive PC / ABS composite material according to claim 1, characterized in that, The butadiene in the ABS resin has a particle size of 0.3–1.2 μm.
6. The humidity-responsive PC / ABS composite material according to any one of claims 1 to 5, characterized in that, The toughening agent is at least one of the following: organosilicon core-shell copolymer, styrene-butadiene-methyl methacrylate terpolymer, and ABS high-resin powder.
7. The humidity-responsive PC / ABS composite material according to any one of claims 1 to 5, characterized in that, It also includes antioxidants and lubricants; the antioxidant is at least one of hindered phenolic antioxidants, phosphite antioxidants and thioester antioxidants; the lubricant is pentaerythritol stearate and / or silicone masterbatch.
8. A method for preparing a humidity-responsive PC / ABS composite material according to any one of claims 1 to 7, characterized in that, Includes the following steps: By mixing polycarbonate, covalent organic framework material, ABS resin, toughening agent, optional lubricant and optional antioxidant, the mixture is melted and extruded to obtain a moisture-responsive PC / ABS composite material.
9. The use of the humidity-responsive PC / ABS composite material according to any one of claims 1 to 7 in humidity-responsive enclosure materials.
Citation Information
Patent Citations
PC / ABS material composition for relieving yellow discoloration
CN101759979A