Polypropylene fiber cloth with water super-spreading and preparation method and application thereof

By self-assembling hydrophilic polymers on the surface of polypropylene fiber cloth, the problem of poor hydrophilicity of polypropylene nonwoven fabric was solved, achieving super-spreading performance and broadening its application range.

CN117845618BActive Publication Date: 2026-11-20CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211205620.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2026-11-20
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

Existing polypropylene nonwoven fabrics have poor hydrophilicity and moisture absorption, which limits their application in fields such as high-efficiency separation and anti-biofouling, especially in terms of superhydrophilicity and superspreading properties.

Method used

By contacting polypropylene fiber cloth with a hydrophilic polymer solution, the hydrophilic polymer is self-assembled on the fiber surface by intermolecular forces to form a coating layer, thereby achieving super-spreading performance.

Benefits of technology

Polypropylene fiber cloth achieves a static contact angle of 0° with water within 1 second, broadening its application areas and enabling efficient and low-cost industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117845618B_ABST
    Figure CN117845618B_ABST
Patent Text Reader

Abstract

The application relates to the technical field of new material preparation, in particular to a polypropylene fiber cloth with water super-spreading, a preparation method and application thereof. The super-spreading polypropylene fiber cloth comprises a polypropylene fiber cloth substrate and a hydrophilic polymer, the content of the hydrophilic polymer is 0.01%-7% based on 100% of the mass of the super-spreading fiber cloth, and the static contact angle of the polypropylene fiber cloth with water can reach 0 within 1 second. The method for preparing the polypropylene fiber cloth does not need any pretreatment such as graft modification of the polypropylene fiber cloth, directly contacts the hydrophilic polymer, and the super-spreading polypropylene fiber cloth in the application can be obtained by means of external force, and the method has the characteristics of high efficiency, low consumption and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of new material preparation technology, specifically to a water-spreadable polypropylene fiber cloth, its preparation method, and its application. Background Technology

[0002] Nonwoven fabric, also known as non-woven cloth or non-woven fabric, is a type of polypropylene fiber fabric. It refers to a fiber fabric composed of oriented or randomly arranged fibers, typically characterized by breathability and lightweight. Nonwoven fabric is a type of non-woven material made by directly using polymer chips, short fibers, or filaments to form a web through airflow or mechanical means, followed by hydroentangling, needle punching, or thermal rolling for reinforcement, and finally finishing processes to create a non-woven fabric. It is a new type of fiber product with a soft, breathable, and planar structure. Its advantages include no fiber shedding, strength, durability, silky softness, and a cotton-like feel. Compared to cotton fabrics, nonwoven bags are easier to shape and cheaper to produce.

[0003] Common materials used to prepare nonwoven fabrics include polypropylene, polyethylene, polyester, and polyamide, with polypropylene nonwoven fabric being the most widely used. Currently, polypropylene nonwoven fabric is widely used in masks, protective clothing, geomembranes, and other fields. However, polypropylene nonwoven fabric has poor hydrophilicity and hygroscopicity, with a contact angle with water typically around 130°, limiting its application areas. For example, it is limited in applications such as wet wipes, face masks, medical gauze, wastewater treatment, filter cloths, and functionalized polypropylene nonwoven fabrics. Especially in areas requiring superhydrophilicity and superspreading properties, such as high-efficiency separation and resistance to biofouling, traditional polypropylene nonwoven fabrics cannot be used. Superspreading (or superdiffusion) refers to the ability of small droplets (below 2μl, excluding the influence of gravity) to quickly achieve a contact angle of 0° upon complete contact with an object surface. Materials with superspreading properties have better hydrophilicity than traditional superhydrophilic materials (contact angle less than 5°), allowing liquids to be rapidly transferred and flow within the material, resulting in high throughput. Therefore, they have significant advantages in separation, filtration and other fields.

[0004] Currently, most publicly available or reported water-based superspreading materials are naturally occurring. For example, Miao et al. discovered that the cornea of ​​rabbits possesses superspreading properties, reducing the contact angle (CA) to 0° within 1 second. Based on the structural analysis of the rabbit cornea, a nanofiber array mold was designed, and a hydrogel of the nanofiber array was obtained through molding. This hydrogel reduced the time to reduce the contact angle to 0° to 0.45 seconds. Zheng et al., in their article "2D prior spreading inspired from Chinese Xuan papers" (Adv. Funct. Mater. 2018, 28, 1800832.), used electrospinning to prepare a cellulose ultrafine fiber membrane with superspreading effects. In this material, cellulose fibers form an ultrafine fiber structure, and the cellulose surface contains hydrophilic groups and micropores with extremely small pore sizes. The combined effect of these factors creates the superspreading effect. Currently, all publicly available superspreading materials use hydrophilic polymer matrices and achieve their excellent hydrophilic properties through loaded structural design; however, the materials used in existing technologies are costly, and the preparation processes are complex, making industrialization difficult. Polyolefin materials are the world's most important synthetic resins, especially polypropylene, which is widely used in construction, medicine, and other fields. Chinese invention patent CN114133612A, "A Biomimetic Hyperspreadable Surface and Its Preparation Method," discloses a biomimetic hyperspreadable surface with a raised honeycomb structure, similar to the surface of natural plants. Combined with modification with hydrophilic materials, its water contact angle is reduced to below 60°. This technology does not reduce the water contact angle to 0°. Currently, polypropylene is an important component of synthetic resin materials, widely used in all aspects of daily life. However, polypropylene itself has poor hydrophilicity. Although its hydrophilicity can be improved by grafting polar monomers or adding surfactants, it is difficult to achieve a contact angle of 0°, let alone achieve hyperspreading.

[0005] Therefore, developing superspreadable materials based on polypropylene that are easy to produce in a continuous industrial process is of great practical significance. It can meet the needs of fields such as separation and environmental protection, and has a huge market potential. Summary of the Invention

[0006] To address the technical problems existing in the prior art, this invention provides a polypropylene fiber cloth with super-spreading properties, its preparation method, and its applications. This polypropylene fiber cloth has good hydrophilicity and can achieve a static contact angle of 0 degrees with water within 1 second, further broadening the application range of polypropylene fiber cloth. Moreover, the method for preparing this polypropylene fiber cloth does not require any pretreatment such as grafting modification of the polypropylene fiber cloth. It can be obtained directly by contacting the polypropylene fiber cloth with a hydrophilic polymer and with the aid of external force. This method is characterized by high efficiency, low consumption, and low cost.

[0007] Firstly, the purpose of this invention is to provide a super-spreadable polypropylene fiber cloth, wherein the super-spreadable polypropylene fiber cloth comprises a polypropylene fiber cloth matrix and a hydrophilic polymer, wherein, based on the mass of the super-spreadable fiber cloth as 100%, the content of the polypropylene fiber cloth matrix in the super-spreadable polypropylene fiber cloth is 93%-99.99%; the content of the hydrophilic polymer is 0.01%-7%; and the static contact angle between the polypropylene fiber cloth and water can reach 0° within a time of no more than 1 second.

[0008] According to the present invention, the superspreadable polypropylene can achieve a static contact angle of 0 degrees with water within 1 second; more preferably, it can achieve a static contact angle of 0 degrees with water within 0.005 seconds to 1 second. For example, it can be 0.005 seconds, 0.01 seconds, 0.05 seconds, 0.1 seconds, 0.5 seconds, 0.9 seconds, 1 second, or any two values ​​or any interval of any two values.

[0009] According to the present invention, the time required for the static contact angle between the polypropylene fiber cloth and water to reach 0 degrees can be tested using conventional testing methods in the art. These methods include, but are not limited to, the following: The fiber cloth sample is flatly attached to a glass slide, ensuring the sample remains horizontal during attachment. The slide is then fixed on the sample stage of a contact angle measuring instrument. A water droplet with a volume of less than 2 μL is dropped into the center of the sample. The angle between the solid-liquid interface, through the interior of the droplet, and the vapor-liquid interface at the three-phase interface is measured; this is the static contact angle (referred to as the water contact angle). The time is calculated from the moment the droplet contacts the fiber cloth surface and is lifted off the surface, until the droplet is fully spread and the contact angle reaches 0 degrees. Controlling the volume to less than 2 μL eliminates the influence of gravity, better demonstrating the excellent hydrophilicity and superspreading properties of the polypropylene fiber cloth.

[0010] According to the present invention, based on the total mass of the super-spreadable polypropylene fiber cloth as 100%, the content of the polypropylene fiber cloth matrix in the polypropylene fiber cloth is more preferably 93%-99.99%, preferably 95%-99.95%, for example, it can be 95%, 97%, 98.3%, 99%, 99.95%, and any two values ​​or any range of any two values.

[0011] According to the present invention, based on the total mass of the polypropylene fiber cloth as 100%, the content of the hydrophilic polymer is more preferably 0.01%-7%, preferably 0.05%-5%, for example 0.01%, 0.7%, 3%, 5%, and any two values ​​or any range of any two values.

[0012] Preferably, the sum of the content of the polypropylene fiber matrix and the content of the hydrophilic polymer is 100%.

[0013] According to the present invention, the mass content of the hydrophilic polymer in the polypropylene fiber cloth can be detected using conventional testing methods in the art. These methods include, but are not limited to, the following: weigh the unmodified polypropylene fiber cloth (m1), treat it using the methods listed in the examples, and then dry it to obtain the treated polypropylene fiber cloth (m2). The mass content of the hydrophilic polymer is calculated as (m2-m1) / m2 × 100%.

[0014] According to the present invention, the selectable range of hydrophilic polymer content per unit surface area of ​​the polypropylene fiber cloth is relatively wide. In a preferred embodiment of the present invention, the hydrophilic polymer content per unit surface area of ​​the polypropylene fiber cloth is 0.005 g / m². 2 -3g / m 2 Preferably, it is 0.005 g / m 2 -2g / m 2, For example, 0.005 g / m 2 1g / m 2 2g / m 2 The content of hydrophilic polymer per unit surface area of ​​the polypropylene fiber cloth, and any two values ​​or any interval between two values, can be determined using conventional detection methods in the art, including but not limited to the following methods:

[0015] First, the sample to be tested is coated with gold. Then, the coated sample is placed on an SEM stage, and a 5μm × 5μm area on the sample is scanned using SEM. Then, the mass fraction of oxygen in this area is determined using EDS energy dispersive spectroscopy, and recorded as w0 and w1 respectively. The oxygen content is then calculated using the following formula: W = (w1 - w0) / (M O / MA )×M, where M O M is the relative atomic mass of oxygen. A M is the molecular weight of a single hydrophilic polymer unit, M is the areal density of the polypropylene fiber cloth, and W is the content of hydrophilic polymer per unit area of ​​the polypropylene fiber cloth.

[0016] According to the present invention, the polypropylene fiber fabric matrix can be selected from a wide range of options, such as meltblown polypropylene nonwoven fabric, spunbond polypropylene nonwoven fabric, etc.

[0017] According to the present invention, the fiber diameter of the polypropylene fiber fabric matrix can be selected from a wide range. In a preferred embodiment of the present invention, the fiber diameter is less than 20 micrometers, preferably less than 10 micrometers, and more preferably 0.1-10 micrometers.

[0018] The range of fiber diameters in the polypropylene fiber fabric matrix described in this invention refers to the range of nominal fiber diameters or statistically obtained values ​​of commercially available polypropylene fiber fabric matrices in the art. Where the nominal fiber diameter range or statistically obtained values ​​are within the scope of this invention, and where occasionally some (or a few) fibers in the overall polypropylene fiber fabric matrix have diameters outside the range specified in this application, these are also within the protection scope of this invention. The fiber diameter detection method described above can employ conventional methods in the art, including but not limited to observing fibers under a microscope, such as an electron microscope or an optical microscope, and measuring and statistically analyzing the fiber diameter.

[0019] In a more preferred embodiment of the present invention, the hydrophilic polymer is selected from water-soluble polymers. Preferably, the hydrophilic polymer contains polar and non-polar segments. More preferably, it includes, but is not limited to, at least one of the following polymers and / or at least one of the following polymers crosslinked with a crosslinking agent to form a crosslinked polymer: polyvinyl alcohol, polyacrylamide, polyethyleneimine, sodium polyacrylate, polyacrylic acid, maleic anhydride copolymer and its derivatives, and at least one of polyethylene glycol. More preferably, it includes, at least one of sodium polyacrylate, polyvinyl alcohol, maleic anhydride copolymer and its derivatives, and polyethylene glycol.

[0020] According to the present invention, the hydrophilic polymer can undergo a crosslinking reaction as needed, and the range of selectable crosslinking agents is wide. In a preferred embodiment of the present invention, the crosslinking agent is selected from at least one of polybasic acids and polybasic aldehydes, including but not limited to at least one of glutaraldehyde and boric acid.

[0021] According to the present invention, the range of selectable hydrophilic polymers is relatively wide. In a preferred embodiment of the present invention, the hydrophilic polymer can self-assemble on the fiber surface in the polypropylene fiber matrix. The non-polar segments of the hydrophilic polymer are assembled on the polypropylene fiber surface, and the polar segments are distributed on the fiber surface after assembly, thereby improving the hydrophilicity of the polypropylene fiber fabric.

[0022] Preferably, the super-spreadable polypropylene fiber cloth contains polypropylene fibers coated with a hydrophilic polymer, and the above phenomenon can be detected by scanning electron microscopy.

[0023] In a more preferred embodiment of the present invention, the super-spreadable polypropylene fiber cloth is prepared by contacting a polypropylene fiber cloth matrix with a solution containing a hydrophilic polymer under the action of external force, wherein the content of the hydrophilic polymer in the solution containing the hydrophilic polymer is not higher than 5 wt%.

[0024] Under the aforementioned hydrophilic polymer concentration conditions and the action of external force, the contact utilizes intermolecular forces to cause the hydrophilic polymer to self-assemble on the surface of the polypropylene fiber cloth, resulting in an ultra-spreadable polypropylene fiber cloth with polypropylene fibers coated with hydrophilic polymer.

[0025] Secondly, the object of the present invention is to provide a method for preparing the polypropylene fiber cloth described in the first aspect, comprising contacting a polypropylene fiber cloth matrix with a solution containing a hydrophilic polymer under the action of an external force, wherein the content of the hydrophilic polymer in the solution is not higher than 5 wt%, thereby obtaining the super-spreadable polypropylene fiber cloth.

[0026] By using the above technical solution, the polypropylene fiber cloth matrix is ​​brought into contact with a solution containing a hydrophilic polymer, and the hydrophilic polymer is self-assembled on the surface of the polypropylene fiber cloth by utilizing intermolecular forces, thereby achieving the super-spreading performance of the polypropylene fiber cloth.

[0027] The method for preparing the polypropylene fiber cloth of the present invention does not require any pretreatment such as grafting modification of the polypropylene fiber cloth. It directly contacts the polypropylene fiber cloth with a solution of hydrophilic polymer. The method has the characteristics of high efficiency, low consumption and low cost.

[0028] According to the present invention, the content of the hydrophilic polymer in the solution containing the hydrophilic polymer can be selected within a wide range. In a preferred embodiment of the present invention, the content of the hydrophilic polymer in the solution containing the hydrophilic polymer is 0.05-4.5 wt%, preferably 0.1-4.5 wt%, for example 0.1 wt%, 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, and any two values ​​or any range of any two values, more preferably 0.3-3 wt%.

[0029] In a more preferred embodiment of the present invention, the contact is carried out in a solution containing a hydrophilic polymer, thereby resulting in a more uniform superspreading property of the obtained polypropylene fiber cloth.

[0030] According to the present invention, the contact between the fiber cloth and the hydrophilic polymer can be carried out over a wide temperature range, preferably not exceeding the melting temperature of polypropylene and the hydrophilic polymer, and more preferably not exceeding the glass transition temperature of the hydrophilic polymer.

[0031] According to the present invention, the preparation method further includes a step of drying the polypropylene fiber cloth matrix after contacting the hydrophilic polymer; specifically, the drying temperature does not exceed the melting temperature of the fiber cloth matrix and the hydrophilic polymer, and more preferably does not exceed the glass transition temperature of the hydrophilic polymer.

[0032] According to the present invention, during the self-assembly of hydrophilic polymers on the surface of polypropylene fibers, external forces can be used to help them to quickly achieve assembly. The external forces include, but are not limited to, one or more of the following methods: ultrasound, rolling, filtration, lamination, molding, etc.

[0033] According to the present invention, the conditions for the application of external force are wide-ranging, such as the processing time, the number of processing times, and the process conditions of the processing method, without specific limitations.

[0034] The ultrasonic treatment conditions in this invention can be selected over a wide range. In a preferred embodiment of this invention, the ultrasonic treatment conditions include: the ultrasonic frequency is not less than 5 kHz, preferably not less than 10 kHz; for example, 10 kHz, 20 kHz, 30 kHz, 40 kHz, 45 kHz, 50 kHz, 55 kHz, and 60 kHz. The higher the ultrasonic power, the fewer the intervals and number of treatments.

[0035] According to the present invention, the ultrasonic processing equipment can be selected from conventional ultrasonic processing equipment, including but not limited to ultrasonic cleaning tables, cell disruptors, ultrasonic probes, industrial ultrasonic devices, etc. The present invention does not particularly limit the power of the specific ultrasonic processing equipment; preferably, the power is 50-750W, more preferably 50-500W, and even more preferably 150-350W.

[0036] According to the present invention, the range of selectable ultrasonic treatment time in the preparation step is wide. The ultrasonic time is related to the solution concentration, fiber diameter, and areal density. According to the process conditions of the embodiments of the present invention, it is preferably not less than 5 minutes, more preferably 10-120 minutes, for example, 10 minutes, 20 minutes, 30 minutes, 40 minutes, 60 minutes, 100 minutes, 120 minutes, etc.

[0037] In another preferred embodiment of the present invention, the filtration conditions can be selected over a wide range, and the processing time and number of processes can be reduced as the vacuum level increases. In a preferred embodiment of the present invention, the filtration conditions include: a vacuum level of not less than 5 Pa, preferably not less than 10 Pa, and / or a filtration time of not less than 1 second, preferably not less than 5 seconds. Preferably, the hydrophilic polymer solution remains wetted in the polypropylene fiber fabric matrix until filtration is stopped.

[0038] In a more preferred embodiment of the present invention, the preparation method may include the following steps:

[0039] The polypropylene fiber fabric matrix is ​​brought into contact with a solution containing a hydrophilic polymer under external force; an aqueous solution of the hydrophilic polymer is then immersed in the polypropylene fiber fabric matrix; and the matrix is ​​dried. In a preferred embodiment of the present invention, the hydrophilic polymer is selected from water-soluble polymers, including at least one of polyvinyl alcohol, polyacrylamide, polyethyleneimine, sodium polyacrylate, polyacrylic acid, maleic anhydride copolymers and their derivatives, and polyethylene glycol, more preferably at least one of sodium polyacrylate, maleic anhydride copolymers and their derivatives, polyvinyl alcohol, and polyethylene glycol.

[0040] According to the present invention, there are no particular limitations on the molecular weight of the hydrophilic polymer; for example, the number average molecular weight can be 30,000-300,000. Taking the embodiments of the present invention below as examples, polyvinyl alcohol with a degree of polymerization of 1700 can be selected, as well as maleic anhydride copolymers and their derivatives with a number average molecular weight of 260,000-350,000; sodium polyacrylate with a number average molecular weight of 260,000-270,000 can also be selected.

[0041] According to the present invention, the polypropylene fiber fabric matrix can be selected from a wide range of materials, such as meltblown polypropylene nonwoven fabric, spunbond polypropylene nonwoven fabric, spunlace polypropylene nonwoven fabric, etc. In a preferred embodiment of the present invention, the polypropylene nonwoven fabric matrix is ​​polypropylene meltblown nonwoven fabric.

[0042] The polypropylene meltblown fiber cloth can be selected from a wide range of options. Preferably, the areal density of the polypropylene meltblown fiber cloth is 10-60 g / m². 2 Preferably 20-50g / m 2 And / or, the fiber diameter is not greater than 20 micrometers, preferably less than 10 micrometers, more preferably 0.1-10 micrometers.

[0043] The range of fiber diameters in the polypropylene fiber fabric matrix described in this invention refers to the range of nominal fiber diameters or statistically obtained values ​​of commercially available polypropylene fiber fabric matrices in the art. Where the nominal fiber diameter range or statistically obtained values ​​are within the scope of this invention, and where occasionally some (or a few) fibers in the overall polypropylene fiber fabric matrix have diameters outside the range specified in this application, these are also within the protection scope of this invention. The fiber diameter detection method described above can employ conventional methods in the art, including but not limited to observing fibers under a microscope, such as an electron microscope or an optical microscope, and measuring and statistically analyzing the fiber diameter.

[0044] The preparation method further includes an optional crosslinking step, which can be performed selectively depending on the specific application.

[0045] In the crosslinking step, the polypropylene fiber cloth obtained by contacting the polypropylene fiber cloth matrix with the hydrophilic polymer is subjected to a crosslinking reaction in a solution containing a crosslinking agent.

[0046] The cross-linked hydrophilic polymer forms a network structure, increasing its stability within the fiber fabric and thus enhancing its hydrophilic stability. However, the cross-linking structure requires the participation of polar segments in the hydrophilic polymer during the reaction, thereby reducing the number of polar segments on the polypropylene fiber surface and affecting the fiber fabric's spreading time. Therefore, cross-linked and uncross-linked products exhibit significant differences in spreading time and superspreading stability, making them unsuitable for certain applications.

[0047] The aforementioned super-spreading stability refers to the change in contact angle after the hydrophilic fiber fabric is completely immersed in deionized water and treated under ultrasonic cleaning conditions for 5 minutes, repeated 3 times. The smaller the change in contact angle, the better its hydrophilic stability.

[0048] According to the present invention, the crosslinking agent can be selected from a wide range. In a preferred embodiment of the present invention, the crosslinking agent is selected from at least one of polybasic acid and polybasic aldehyde, preferably at least one of glutaraldehyde and boric acid, and more preferably glutaraldehyde.

[0049] According to the present invention, the selectable range of crosslinking agent content in the solution containing the crosslinking agent is relatively wide. In a preferred embodiment of the present invention, the crosslinking agent content in the solution containing the crosslinking agent is 0.005-0.8 wt%, preferably 0.01-0.5 wt%; and / or, the crosslinking temperature conditions include:

[0050] According to the present invention, the crosslinking conditions can be selected over a wide range. Preferably, the crosslinking temperature does not exceed the glass transition temperature of the hydrophilic polymer, preferably 30-70°C; and / or, the pH of the solution containing the crosslinking agent is 4-7; the crosslinking reaction time is 1 min-120 min, preferably 1 min-90 min, for example, it can be 1 min, 3 min, 5 min, 10 min, 20 min, 50 min, 70 min, 90 min, and any two values ​​or any range of any two values.

[0051] The present invention does not have any particular limitations on the raw materials used to adjust the pH; any conventional acid or base raw materials in the art can be used.

[0052] According to the present invention, the cross-linked fiber cloth can be cleaned to remove residual cross-linking agents and other substances. The present invention does not particularly limit the cleaning method, including but not limited to rinsing with water. To improve cleaning efficiency, ultrasonic cleaning is preferred. The ultrasonic conditions are not particularly limited here. For example, the ultrasonic frequency is 20-80 kHz. Preferably, the ultrasonic cleaning time is 1-30 minutes per cycle, more preferably 15-25 minutes per cycle, and the number of cleaning cycles is selected from 1-5 times, preferably 2-4 times.

[0053] According to the present invention, if the superspreadable polypropylene fiber cloth needs to be dried, the drying temperature shall not exceed the glass transition temperature of the hydrophilic polymer. When the processing temperature exceeds the glass transition temperature, the hydrophilic polymer undergoes molecular chain segment movement, which will destroy its self-assembled structure and affect the superspreading performance.

[0054] The third aspect of this invention is to provide an ultra-spreadable polypropylene fiber cloth, prepared according to the preparation method described in the second aspect.

[0055] Fourthly, an object of the present invention is to provide the application of the super-spreadable polypropylene fiber cloth described in either the first or third aspect in the following fields:

[0056] Oil-water separation, brine desalination, wastewater treatment, ion concentration or extraction, suspended solids filtration, oily rainwater separation, and medical and health products.

[0057] According to the present invention, its application fields include, but are not limited to, oil-water separation, brine desalination, wastewater treatment, ion concentration or extraction, suspended solids filtration, oily rainwater separation, etc., and it can also be used in medical and health products including but not limited to diapers, diaper pads, sanitary napkins, and accessories (such as medical and health accessories).

[0058] Compared with the prior art, the present invention has the following advantages:

[0059] The polypropylene fiber cloth of this invention possesses excellent hydrophilic properties, enabling super-spreading of water and achieving a water contact angle of 0° within one second. This polypropylene fiber cloth can be used in oil-water separation, brine desalination, ion concentration or extraction, and saline wastewater treatment, thus broadening the application range of polypropylene fiber cloth and realizing its high-value utilization.

[0060] The polypropylene fiber cloth of this invention possesses the above-mentioned properties through the inventors' unexpected discovery during their research. When the fiber diameter of the polypropylene fiber cloth is less than a certain size, capillary action occurs on the surface and inside of the fiber cloth. During contact or impregnation with the hydrophilic polymer aqueous solution, the solution comes into contact with the surface of the polypropylene fiber through capillary force or with the assistance of external force. When the content of the hydrophilic polymer in the solution is not higher than 5 wt%, the hydrophilic polymer molecular chains in the aqueous solution are uniformly dispersed. The non-polar segments (segments without hydroxyl groups) exhibit good compatibility with the equally non-polar polypropylene and undergo self-assembly upon contact with the polypropylene fiber cloth matrix. In this process, the hydrophilic polymer separates the polar and non-polar segments, i.e., the non-polar segments coat the surface of the polypropylene fiber, while the polar segments are exposed on the surface of the polypropylene fiber after self-assembly, thus giving the polypropylene fiber cloth hydrophilic properties. By controlling the process conditions (e.g., external force, concentration of hydrophilic polymer, etc.), thin-layer self-assembly of the hydrophilic polymer on the surface of the polypropylene fiber can be achieved. Through the combined effects of capillary force and self-assembly, polypropylene fiber cloth contains polypropylene fibers coated with hydrophilic polymers, giving the polypropylene fiber cloth super-spreading properties. This process can occur better under external forces, such as ultrasound, where the hydrophilic polymer solution can quickly penetrate between the fibers, promoting contact between non-polar segments and the polypropylene fiber surface, thereby accelerating the speed and efficiency of self-assembly.

[0061] Moreover, the method for preparing the polypropylene fiber cloth of the present invention does not require any pretreatment such as grafting modification of the polypropylene fiber cloth, and the method is characterized by high efficiency, low consumption and low cost. Attached Figure Description

[0062] Figure 1 This is a SEM (scanning electron microscope) image of the polypropylene fiber cloth in the blank sample (comparative example 1).

[0063] Figure 2 This is a SEM image of the polypropylene nonwoven fabric in Example 1.

[0064] Figure 1 As shown in the electron micrograph of the blank sample, the surface of the polypropylene nonwoven fabric fibers is smooth, and no filaments, membranes, or other structures are observed in the interfiber spaces. Figure 2 As shown, there was no significant difference in fiber appearance and size between Example 1 and the blank sample of Comparative Example 2, indicating that the hydrophilic polymer can form a thin layer of self-assembly on the surface of polypropylene fibers without affecting the morphology such as the diameter.

[0065] The oxygen mass fraction of the unmodified and hydrophilically modified polypropylene nonwoven fabrics in this region was determined by EDS energy dispersive spectroscopy and denoted as w0 and w1, respectively. The oxygen content was then calculated using the following formula: W = (w1 - w0) / (M O / M A )×M, where M O M is the relative atomic mass of oxygen. A Let M be the molecular weight of a single hydrophilic polymer unit, M be the areal density of the polypropylene nonwoven fabric, and W be the content of hydrophilic polymer per unit area of ​​the polypropylene nonwoven fabric. EDS energy dispersive spectroscopy verification showed that the hydrophilic polymer content per unit area in Example 1 was 0.31 g / m². 2 , combined Figure 1 , 2 The comparative results further confirm that the hydrophilic polymer forms a thin self-assembled film on the surface of polypropylene fibers without affecting the diameter and other morphologies of the polypropylene fibers.

[0066] Figure 3 This is a screenshot from a video recording of the contact angle test in Example 1. Figure 3 As can be seen, by the time the video recording screenshot was taken at 0.60 seconds, the water had already spread completely on the surface of the fiber cloth. Detailed Implementation

[0067] The present invention will now be described in detail with reference to specific embodiments. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.

[0068] The experimental data in the examples were measured using the following instruments and methods:

[0069] The water contact angle and spreading time (spreading time is the time required for the water contact angle to reach 0°) obtained in the example were measured using the German EASYDROP contact angle tester: The non-woven fabric was cut into a sample of 1cm×1cm size, and then the sample was flatly attached to a glass slide. During the attachment process, care was taken to keep the sample flat in the horizontal direction. Then the glass slide was placed on the sample stage of the EASYDROP contact angle measuring instrument and fixed. The instrument was adjusted to control the volume of water droplets to drop into the center of the sample. After 10 seconds, the angle between the solid-liquid interface, through the interior of the droplet, and to the vapor-liquid interface at the three-phase interface was measured, which is the static contact angle (abbreviated as water contact angle).

[0070] Liquid content of hydrophilic polypropylene nonwoven fabric: Take a dry hydrophilic polypropylene nonwoven fabric and weigh it. Then rinse the sample with deionized water until there is no foam, and hang it at 25°C and 30% humidity. After no water droplets fall for 1 minute, weigh it again. The difference between the two weighings divided by the mass after drying is the liquid content of the sample, expressed in multiples.

[0071] The mass content of hydrophilic polymer in the polypropylene nonwoven fabric obtained in the example: Weigh the unmodified polypropylene nonwoven fabric by mass m1, process it by the method listed in the example and dry it to obtain the processed polypropylene nonwoven fabric, weigh it by mass m2, and (m2-m1) / m2×100% is the mass content of hydrophilic polymer.

[0072] The content of hydrophilic polymer per unit surface area of ​​the polypropylene nonwoven fabric was determined as follows: First, the sample to be tested was coated with a gold coating. Then, the coated sample was placed on an SEM detection stage, and a 5μm × 5μm area on the sample was scanned using SEM. Then, the mass fraction of oxygen in the unmodified and hydrophilically modified polypropylene nonwoven fabrics was determined using EDS energy dispersive spectroscopy in this area, denoted as w0 and w1 respectively. The oxygen content was calculated using the following formula: W = (w1 - w0) / (M O / M A )×M, where M O M is the relative atomic mass of oxygen. A M is the molecular weight of a single hydrophilic polymer unit, M is the areal density of the polypropylene nonwoven fabric, and W is the content of hydrophilic polymer per unit area of ​​the polypropylene nonwoven fabric.

[0073] All materials used in this invention, except for maleic anhydride copolymer, are commercially available.

[0074] In the following examples, polyvinyl alcohol, PVA-1799, with a degree of polymerization of 1700 and a degree of alcoholysis of 99%, was purchased from Aladdin; unless otherwise specified, the polypropylene meltblown nonwoven fabric (matrix) used in the examples and comparative examples was from Sinopec Yanshan Petrochemical, with an areal density of 25 g / m³. 2 The fiber diameter is 0.5-8 micrometers.

[0075] Example 1

[0076] Polypropylene meltblown nonwoven fabric was immersed in a 0.3wt% polyvinyl alcohol (from Aladdin, PVA-1799, glass transition temperature 72℃) aqueous solution at 25℃ and ultrasonically treated at 50kHz for 30 minutes under a 250W ultrasonic probe. The treated polypropylene meltblown fabric was then crosslinked in a 0.5wt% glutaraldehyde crosslinking solution (pH 6) at 60℃ for 1 hour. After crosslinking, the polypropylene meltblown fabric was cleaned three times in a 100W ultrasonic water bath at 50kHz for 20 minutes each time, and then dried (at 60℃ for 1 hour).

[0077] The obtained polypropylene nonwoven fabric was tested for water contact angle, mass content of hydrophilic polymer, fiber diameter of polypropylene nonwoven fabric and hydrophilic polymer content per unit area. The specific test data are shown in Table 1.

[0078] Example 2

[0079] Except for changing the concentration of the PVA aqueous solution to 1 wt%, the other operations were the same as in Example 1. The specific test data are shown in Table 1.

[0080] Example 3

[0081] Except for changing the ultrasonic treatment time when soaking in polyvinyl alcohol aqueous solution to 50 minutes, all other aspects were the same as in Example 1. Specific test data are shown in Table 1.

[0082] Example 4

[0083] Except for the cleaning steps performed without crosslinking and after crosslinking, all other operations were the same as in Example 1, and the specific test data are shown in Table 1.

[0084] Comparative Example 1

[0085] Polypropylene meltblown nonwoven fabric was immersed in deionized water at 25°C and ultrasonically treated for 30 minutes at 50kHz under a 250W ultrasonic probe. The treated polypropylene meltblown fabric was then placed in a 0.5wt% glutaraldehyde crosslinking solution (pH 6) and treated in a 60°C oven for 1 hour. After treatment, the polypropylene meltblown fabric was cleaned three times in a 100W ultrasonic water bath at 50kHz, 20 minutes each time, and then dried (at 60°C for 1 hour).

[0086] The obtained polypropylene nonwoven fabric was tested for water contact angle, mass content of hydrophilic polymer, fiber diameter before and after treatment, and hydrophilic polymer content per unit area. The specific test data are shown in Table 1.

[0087] Comparative Example 2

[0088] Polypropylene meltblown nonwoven fabric was immersed in a 0.1 wt% polyvinyl alcohol (PVA-1799 from Aladdin) aqueous solution at 25°C and ultrasonically treated at 50 kHz for 30 minutes under a 250 W ultrasonic probe. The treated polypropylene meltblown fabric was then crosslinked in a 0.5 wt% glutaraldehyde crosslinking solution (pH 6) at 80°C for 1 hour. After crosslinking, the polypropylene meltblown fabric was cleaned three times in a 100 W ultrasonic water bath at 50 kHz for 20 minutes each time, followed by drying (at 85°C for 1 hour). The glass transition temperature of PVA-1799 is 72°C.

[0089] The obtained polypropylene nonwoven fabric was tested for water contact angle, mass content of hydrophilic polymer, fiber diameter before and after treatment, and hydrophilic polymer content per unit area. The specific test data are shown in Table 1.

[0090] Comparative Example 3

[0091] Polypropylene nonwoven fabric was prepared according to the method in Example 1, except that polypropylene spunbond nonwoven fabric (Shandong Lingxiang New Material Co., Ltd., model YC188, with an areal density of 80 g / m²) was used. 2 Replace polypropylene meltblown nonwoven fabric (a product of Sinopec Yanshan Petrochemical, with a surface density of 25 g / m³). 2 With all other conditions remaining unchanged, the specific test data is shown in Table 1.

[0092] Example 5

[0093] Polypropylene nonwoven fabric was prepared according to the method in Example 4, except that the polyvinyl alcohol solution was replaced with an aqueous solution of sodium maleate-isobutylene alternating copolymer of equal mass concentration. Specific test data are shown in Table 1.

[0094] The preparation method for sodium maleate-isobutylene alternating copolymer is as follows: Take 10g of maleic anhydride-isobutylene alternating copolymer (Kuraray ISOBAM, molecular weight 300,000), place it in a 500ml beaker, add 100ml of deionized water, then add 1.5g of NaOH, and stir in a 75℃ water bath for 30 minutes. After complete dissolution, dry in a forced-air oven to obtain sodium maleate alternating copolymer. Its glass transition temperature was determined to be 167℃ by DSC.

[0095] Example 6

[0096] The external force was applied using a roller pressing method. Both upper and lower rollers were cylindrical with a diameter of 8 cm and a length of 20 cm (with an outer layer of soft rubber). The roller speed was 30 r / min, and the upper and lower rollers rotated at the same speed. The pressure between the rollers was 100 kPa. The rollers were positioned below the surface of the PVA solution. The nonwoven fabric underwent two roller pressing treatments. The remaining conditions were the same as in Example 1. Specific test data are shown in Table 1.

[0097] Example 7

[0098] In Example 6, a 250W ultrasonic probe was added to the aqueous solution and ultrasonicated at a frequency of 50kHz. The nonwoven fabric was subjected to a roll pressing treatment once in the ultrasonically treated aqueous solution. The other conditions were the same as in Example 6. The specific test data are shown in Table 1.

[0099] Comparative Example 4

[0100] A 0.8 wt% aqueous solution was prepared using PVA 1750 (purchased from Shandong Jiaying Chemical Technology Co., Ltd.) and deionized water at 90℃. 500 ml of the PVA solution was weighed and mixed with 600 ml of the crosslinking solution to obtain a mixed solution. The crosslinking solution contained 45 ml of glutaraldehyde aqueous solution (50 wt%), as well as acetic acid aqueous solution (10 vol%), methanol aqueous solution (10 vol%), and sulfuric acid aqueous solution (10 vol%), with a volume ratio of 3:2:1. Polypropylene meltblown nonwoven fabric (Sinopec Yanshan Petrochemical, surface density 25 g / m²) was used. 2 The sample was placed in a mixed solution and shaken at 150 rpm for 60 minutes at 50°C in a shaking incubator. It was then placed in deionized water for 1 hour to remove residual crosslinking agent and PVA, and finally dried in a 50°C oven for 1 hour. Specific test results are shown in Table 1.

[0101] Example 8

[0102] The concentration of PVA aqueous solution was changed to 0.1 wt%, the crosslinking agent was changed to boric acid with a concentration of 0.5 wt%, and the crosslinking time was 90 minutes. All other operations were the same as in Example 1. Specific test data are shown in Table 1.

[0103] Example 9

[0104] The concentration of the hydrophilic aqueous solution was changed to 4.5 wt%, and the ultrasonic treatment process was changed to ultrasonic treatment at a frequency of 40 kHz for 20 minutes. All other operations were the same as in Example 6. The specific test data are shown in Table 1.

[0105] Example 10

[0106] Take polypropylene meltblown nonwoven fabric (a product of Sinopec Yanshan Petrochemical, with a surface density of 25 g / m³). 2The polypropylene nonwoven fabric was spread evenly in a Buchner funnel. 50 ml of a 0.5 wt% PVA solution (from Aladdin, PVA-1799) was added to the funnel, followed by vacuum filtration at a vacuum level of 10 Pa. Filtration was stopped when only 10 ml of PVA solution remained in the funnel. The treated polypropylene nonwoven fabric was then immersed in a 0.3 wt% acidic glutaraldehyde solution (pH 6) and crosslinked in a 70°C oven for 120 minutes. After crosslinking, it was placed in a 100W ultrasonic water bath and cleaned once at a frequency of 50 kHz for 10 minutes each time. Finally, it was dried in a 60°C forced-air oven for 1 hour. Specific test data are shown in Table 1.

[0107] Example 11

[0108] The roller press is positioned above the liquid surface. The nonwoven fabric is pre-immersed in the aqueous solution for 20 seconds, leaving some solution on the fabric surface, and then subjected to roller pressing. The remaining conditions are the same as in Example 6, and the specific test data are shown in Table 1.

[0109] After treatment, the area near the solution on the surface exhibits superspreading properties, while the unsolvable areas are non-hydrophilic. The superspreading properties of the product are unevenly distributed. Table 1 lists the parameters for the superspreadable range. Through multiple experiments, it has been found that if a significant amount of solution can be retained on the surface after impregnation, wetting can still be achieved after applying external force, but uniformity is affected.

[0110] Comparative Example 5

[0111] Take polypropylene meltblown nonwoven fabric (Sinopec Yanshan Petrochemical, surface density 25 g / m³) 2 The polypropylene meltblown substrate was immersed in a 5 wt% aqueous solution of polyvinyl alcohol (from Aladdin, PVA-1799) and ultrasonically treated at 50 kHz for 20 minutes under a 250 W ultrasonic probe. The treated meltblown substrate was then crosslinked in a 0.5 wt% glutaraldehyde crosslinking solution (pH 6) at 60 °C for 1 hour. After crosslinking, the meltblown substrate was cleaned three times in a 100 W ultrasonic water bath at 50 kHz for 20 minutes each time, followed by drying (at 60 °C for 1 hour).

[0112] Table 1

[0113]

[0114]

[0115] As shown in Table 1, the polypropylene fiber cloth of this invention exhibits a static contact angle of 0 degrees with water, demonstrating good hydrophilicity, and a water spreading time of less than 1 second, exhibiting superspreading properties. In contrast, polypropylene fiber cloths prepared by conventional methods cannot achieve a static contact angle of 0 degrees and cannot spread with water, demonstrating significant technical advantages and substantial progress. Furthermore, the method for preparing this polypropylene fiber cloth does not require any pretreatment such as grafting modification; the superspreading polypropylene fiber cloth of this invention can be obtained directly through contact with a hydrophilic polymer and with the aid of external force. This method is characterized by high efficiency, low consumption, and low cost.

[0116] It should be noted that the embodiments described above are only for explaining the present invention and do not constitute any limitation on the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory terms, not limiting terms. Modifications can be made to the present invention within the scope of the claims, and revisions can be made to the present invention without departing from the scope and spirit of the present invention. Although the present invention described herein relates to specific methods, materials, and embodiments, it does not mean that the present invention is limited to the specific examples disclosed herein; on the contrary, the present invention can be extended to all other methods and applications with the same function.

[0117] All publications, patent applications, patents, and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings commonly understood by those skilled in the art. In case of conflict, the definitions in this specification shall prevail.

[0118] When this specification uses the prefixes “known to those skilled in the art,” “prior art,” or similar terms to derive materials, substances, methods, steps, apparatus, or components, the objects derived from such prefixes cover those commonly used in the art at the time of this application, but also include those that are not currently commonly used but will become generally recognized in the art as suitable for similar purposes.

[0119] The endpoints and any values ​​of the ranges disclosed in this application are not limited to the precise ranges or values; such ranges or values ​​should be understood to include values ​​close to them. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein. In principle, various technical solutions can be combined with each other to obtain new technical solutions, which should also be considered as specifically disclosed herein.

[0120] In the context of this specification, except where expressly stated otherwise, any matters or issues not mentioned shall apply directly to those known in the art without any modification.

[0121] Furthermore, any implementation described herein can be freely combined with one or more other implementations described herein, and the resulting technical solutions or technical ideas shall be regarded as part of the original disclosure or original record of the present invention, and should not be regarded as new content not disclosed or anticipated herein, unless those skilled in the art consider the combination to be obviously unreasonable.

Claims

1. A super-spreadable polypropylene fiber cloth, wherein the super-spreadable polypropylene fiber cloth comprises a polypropylene fiber cloth matrix and a hydrophilic polymer, wherein, based on 100% by mass of the super-spreadable polypropylene fiber cloth, the content of the polypropylene fiber cloth matrix in the super-spreadable polypropylene fiber cloth is 93%-99.99%; the content of the hydrophilic polymer is 0.01%-7%; and the static contact angle between the polypropylene fiber cloth and water can reach 0° within no more than 1 second. The super-spreadable polypropylene fiber cloth contains polypropylene fibers coated with a hydrophilic polymer. The hydrophilic polymer contains polar and non-polar segments; the fiber diameter in the super-spreadable polypropylene fiber cloth is less than 10 micrometers. The super-spreadable polypropylene fiber cloth is prepared by the following method, which includes: contacting a polypropylene fiber cloth matrix with a solution containing a hydrophilic polymer under external force, wherein the content of the hydrophilic polymer in the solution is 0.05-4.5 wt%, thereby obtaining the super-spreadable polypropylene fiber cloth; wherein the hydrophilic polymer in the solution is selected from water-soluble polymers, and the contact is carried out in an aqueous solution containing the hydrophilic polymer. The preparation method further includes an optional crosslinking step: when the crosslinking step is included, the polypropylene fiber cloth obtained by contacting the polypropylene fiber cloth matrix with the hydrophilic polymer is subjected to a crosslinking reaction in a solution containing a crosslinking agent, wherein the crosslinking temperature does not exceed the glass transition temperature of the hydrophilic polymer.

2. The super-spreadable polypropylene fiber cloth according to claim 1, characterized in that: The static contact angle between the super-spreadable polypropylene fiber cloth and water can reach 0° within 0.005 seconds to 1 second; and / or, Based on the mass of the super-spreadable polypropylene fiber cloth as 100%, the content of the polypropylene fiber cloth matrix in the super-spreadable polypropylene fiber cloth is 95%-99.95%; and the content of the hydrophilic polymer is 0.05%-5%.

3. The super-spreadable polypropylene fiber cloth according to claim 1, characterized in that: The fiber diameter in the super-spreadable polypropylene fiber cloth is 0.1-10 micrometers.

4. The super-spreadable polypropylene fiber cloth according to claim 1, characterized in that: The hydrophilic polymer is selected from water-soluble polymers.

5. The super-spreadable polypropylene fiber cloth according to claim 1, characterized in that: The hydrophilic polymer on the super-spreadable polypropylene fiber cloth is at least one of the following polymers and / or at least one of the following polymers formed with a crosslinking agent to form a crosslinked polymer: polyvinyl alcohol, polyacrylamide, polyethyleneimine, sodium polyacrylate, polyacrylic acid, maleic anhydride copolymer, and polyethylene glycol.

6. The super-spreadable polypropylene fiber cloth according to claim 1, characterized in that: The hydrophilic polymer on the super-spreadable polypropylene fiber cloth is at least one of the following polymers and / or at least one of the following polymers formed with a crosslinking agent to form a crosslinked polymer: sodium polyacrylate, polyvinyl alcohol, maleic anhydride copolymer and polyethylene glycol.

7. The super-spreadable polypropylene fiber cloth according to claim 5, characterized in that: The crosslinking agent is selected from at least one of polybasic acids and polybasic aldehydes.

8. The super-spreadable polypropylene fiber cloth according to claim 5, characterized in that: The crosslinking agent is glutaraldehyde and / or boric acid.

9. A method for preparing an ultra-spreadable polypropylene fiber cloth according to any one of claims 1-8, comprising contacting a polypropylene fiber cloth matrix with a solution containing a hydrophilic polymer under the action of an external force, wherein the content of the hydrophilic polymer in the solution is 0.05-4.5 wt%, thereby obtaining the ultra-spreadable polypropylene fiber cloth; wherein the ultra-spreadable polypropylene fiber cloth contains polypropylene fibers coated with the hydrophilic polymer. The hydrophilic polymer is selected from water-soluble polymers, and the contact is carried out in an aqueous solution containing the hydrophilic polymer; The preparation method further includes an optional crosslinking step: In the crosslinking step, the polypropylene fiber cloth obtained by contacting the polypropylene fiber cloth matrix with the hydrophilic polymer is subjected to a crosslinking reaction in a solution containing a crosslinking agent; the crosslinking temperature does not exceed the glass transition temperature of the hydrophilic polymer.

10. The preparation method according to claim 9, characterized in that: The contact utilizes intermolecular forces to enable the hydrophilic polymer to self-assemble on the surface of the polypropylene fiber cloth, resulting in an ultra-spreadable polypropylene fiber cloth with polypropylene fibers coated with hydrophilic polymer.

11. The preparation method according to claim 9, characterized in that: The hydrophilic polymer content in the solution is 0.1-4.5 wt%.

12. The preparation method according to claim 9, characterized in that: The preparation method further includes a step of drying the polypropylene fiber cloth matrix after it comes into contact with the hydrophilic polymer.

13. The preparation method according to claim 12, characterized in that: The contact temperature and the drying temperature do not exceed the melting temperatures of the fiber cloth matrix and the hydrophilic polymer.

14. The preparation method according to claim 12, characterized in that: The contact temperature and the drying temperature both do not exceed the glass transition temperature of the hydrophilic polymer.

15. The preparation method according to claim 9, characterized in that: The external force is applied in a manner that includes one or more of the following methods: ultrasonication, rolling, filtration, lamination, and molding.

16. The preparation method according to claim 15, characterized in that: The conditions for ultrasound include: the ultrasound frequency is not less than 5 kHz, and / or the ultrasound duration is not less than 1 minute; and / or, The conditions for vacuum filtration include: The vacuum level is not less than 5 Pa, and / or the filtration time is not less than 1 second; and / or, The conditions for roller pressing include: The pressure shall not be less than 5 Pa; the number of roller pressing cycles shall not be less than 1.

17. The preparation method according to claim 15, characterized in that: The conditions for ultrasound include: the ultrasound frequency is not less than 10 kHz, and / or the ultrasound duration is not less than 5 minutes; and / or, The conditions for vacuum filtration include: The vacuum level is not less than 10 Pa, and / or the filtration time is not less than 5 seconds, and / or The conditions for roller pressing include: The pressure shall be no less than 10 Pa; the number of roller pressing cycles shall be no less than 1.

18. The preparation method according to claim 15, characterized in that: The conditions for ultrasound include: ultrasound time of 10-120 minutes.

19. The preparation method according to claim 9, characterized in that: The hydrophilic polymer is at least one of the following: polyvinyl alcohol, polyacrylamide, polyethyleneimine, sodium polyacrylate, polyacrylic acid, maleic anhydride copolymer, and polyethylene glycol; and / or, The areal density of the polypropylene fiber fabric matrix is ​​10-60 g / m³. 2 .

20. The preparation method according to claim 9, characterized in that: The hydrophilic polymer is at least one selected from sodium polyacrylate, maleic anhydride copolymer, polyvinyl alcohol, and polyethylene glycol; and / or, The areal density of the polypropylene fiber cloth matrix is ​​20-50 g / m³. 2 And / or, the fiber diameter is less than 10 micrometers.

21. The preparation method according to claim 9, characterized in that: The polypropylene fiber fabric matrix has a fiber diameter of 0.1-10 micrometers.

22. The preparation method according to any one of claims 9-18, characterized in that: The crosslinking agent is selected from at least one of polybasic acids and polybasic aldehydes; and / or, The crosslinking agent content in the solution is 0.005-0.8 wt%; and / or, The pH of the solution containing the crosslinking agent is 4-7; the crosslinking reaction time is 1 min-120 min.

23. The preparation method according to any one of claims 9-18, characterized in that: The crosslinking agent is at least one of glutaraldehyde and boric acid; and / or, The crosslinking agent content in the solution is 0.01-0.5 wt%; and / or, The temperature conditions for crosslinking include: the crosslinking temperature is 30-70℃; and / or the pH of the solution containing the crosslinking agent is 4-7; and the crosslinking reaction time is 1 min-90 min.

24. A super-spreadable polypropylene fiber cloth prepared by the preparation method according to any one of claims 9-23.

25. The application of the super-spreadable polypropylene fiber cloth according to any one of claims 1-8 or the super-spreadable polypropylene fiber cloth according to claim 24 in the following fields: Oil-water separation, brine desalination, ion concentration or extraction, and suspended solids filtration.

26. The application of the super-spreadable polypropylene fiber cloth according to any one of claims 1-8 or the super-spreadable polypropylene fiber cloth according to claim 24 in the following fields: Wastewater treatment, diapers, waterproof pads, sanitary napkins.

Citation Information

Patent Citations

  • Bionic super-spreading surface and preparation method thereof

    CN114133612A

  • Polyolefin non-woven fabric treated with hydrophilic treating agent

    JP1998053955A

  • Super-wet surface and preparation method therefor and application thereof

    US20220282054A1