A comprehensive recycling method of skarn type magnetite tailings
By combining screening, weak magnetic separation, strong magnetic separation, gravity separation and flotation, the problem of insufficient purity and recovery rate of various minerals in skarn-type magnetite tailings has been solved, achieving high-purity and high-recovery product separation and comprehensive utilization, and reducing production costs.
Patent Information
- Application Number
- CN202311810077.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-26
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-26
AI Technical Summary
Existing technologies are insufficient to effectively separate and purify various economically valuable minerals such as garnet, quartz, and biotite in skarn-type magnetite tailings, resulting in insufficient product purity and recovery rate.
A combination of screening, weak magnetic separation, strong magnetic separation, gravity separation and flotation is adopted. By controlling the magnetic field strength and slurry concentration, minerals such as magnetite, garnet, quartz and biotite in skarn-type iron ore tailings are separated and enriched. Different collectors are used and the parameters of each step are optimized to improve the separation effect.
It achieves high purity and high recovery rate separation of multiple minerals, and the resulting products can be used in building materials. It solves the problem that it is difficult to achieve both high purity and high recovery rate of multiple minerals in tailings at the same time, reduces production costs and reduces environmental impact.
Smart Images

Figure CN117861844B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of tailings recycling, and more specifically, it relates to a comprehensive recycling method for "silica-type" magnetite tailings. Background Technology
[0002] Due to the complex nature of iron ore tailings after beneficiation and processing into concentrate, they have long been stockpiled in reservoirs without being comprehensively utilized.
[0003] Due to the complex mineral composition of skarn-type magnetite tailings, current domestic recycling efforts mainly focus on purifying easily separable minerals such as garnet. The purification method involves: passing the iron tailings into a flat-plate high-intensity magnetic separator for tailings separation, yielding magnetic and non-magnetic minerals; passing the magnetic minerals into a drum magnetic separator, separating strongly magnetic and weakly magnetic minerals under a magnetic field strength of 350-400 mt; classifying the weakly magnetic minerals by screening, and then separating them according to particle size using jigging and shaking tables to separate garnet particles with large density differences from silicate minerals; finally, dry high-intensity magnetic separation of the garnet particles to separate concentrated garnet and weakly magnetic minerals with lower magnetic susceptibility than the concentrated garnet, thus obtaining concentrated garnet.
[0004] The above purification method can only extract garnet products from tailings. Although the product purity is relatively good, the yield of garnet products is very low. Other products, such as magnetite, quartz, and biotite, which are also economically valuable, cannot be effectively separated, and the technical problem of balancing the purity and yield of each extracted product cannot be solved. Summary of the Invention
[0005] This application provides a comprehensive recycling method for skarn-type magnetite tailings, which can separate, enrich, and purify economically valuable garnet, quartz, and biotite minerals from skarn-type iron ore tailings, respectively, to obtain high-purity garnet, quartz, and biotite products. This solves the problem that it is difficult to separate multiple economically valuable minerals in tailings to obtain multiple products, and also enables the purified products to have both high purity and high recovery rate. Furthermore, it solves the problem that the products obtained after separating or purifying multiple economically valuable minerals in tailings cannot simultaneously achieve high purity and high recovery rate.
[0006] The comprehensive recycling method for "silica-type" magnetite tailings provided in this application adopts the following technical solution: A comprehensive recycling method for "silica-type" magnetite tailings, the method comprising: Screening: The magnetite tailings are screened to obtain mineral I with a particle size greater than 0.30 mm, mineral II with a particle size between 0.1 and 0.3 mm, and mineral III with a particle size less than 0.1 mm. Weak magnetic separation: Mineral I, mineral II, and mineral III are slurried to a mass concentration of 20-30%, and weak magnetic separation is performed at least once under a magnetic field strength of 0.2-0.3T to obtain strong magnetic mineral I and weak magnetic separation tailings I, strong magnetic mineral II and weak magnetic separation tailings II, and strong magnetic mineral III and weak magnetic separation tailings III, respectively. Strong magnetic mineral I, strong magnetic mineral II, and strong magnetic mineral III are mixed to obtain magnetite concentrate product; Strong magnetic separation: Weak magnetic separation tailings I, weak magnetic separation tailings II, and weak magnetic separation tailings III are slurried to a mass concentration of 20-50%, and subjected to strong magnetic separation at least once under a magnetic field strength of 1-1.2T to obtain weak magnetic mineral I and non-magnetic mineral I, weak magnetic mineral II and non-magnetic mineral II, weak magnetic mineral III and non-magnetic mineral III. Gravity separation: Weakly magnetic mineral I, weakly magnetic mineral II, and weakly magnetic mineral III are subjected to gravity separation to obtain gravity separation tailings, garnet rough concentrate, and biotite rough concentrate. The garnet rough concentrate is then ground and gravity separated to obtain garnet concentrate and mineral waste. Flotation: Non-magnetic mineral I, non-magnetic mineral II, and non-magnetic mineral III are floated to obtain quartz product and flotation waste I; Biotite rough concentrate and gravity separation tailings were subjected to flotation to obtain biotite product and flotation waste II.
[0007] Furthermore, mineral waste, flotation waste I, and flotation waste II are mixed to obtain building materials.
[0008] Furthermore, the number of times for weak magnetic separation, strong magnetic separation, and re-separation is 2-3.
[0009] The minerals in skarn magnetite tailings can be divided into two main categories: magnetic minerals and non-magnetic minerals. Magnetic minerals can be further divided into strongly magnetic minerals and weakly magnetic minerals. The strongly magnetic minerals in magnetite tailings are mainly magnetite, while the weakly magnetic minerals are mainly mixtures of garnet, diopside, tremolite, chlorite, biotite, etc. The non-magnetic minerals are mainly mixtures of quartz, calcite, feldspar, mica, etc. Magnetic minerals, especially strongly magnetic magnetite, exhibit magnetic properties. During magnetic separation, magnetic mineral particles are subjected to magnetic forces in the magnetic field, leading to magnetic agglomeration. The finer the magnetic mineral particles and the stronger the magnetic force, the more severe the magnetic agglomeration, making the resulting clumps more difficult to separate. Furthermore, this magnetic agglomeration process can also cause non-magnetic minerals to be adsorbed, severely affecting the effective separation of various products. This application adopts a method of first classifying and screening the magnetite tailings, then performing weak magnetic separation, followed by strong magnetic separation, and then gravity separation and flotation. This method is beneficial for simultaneously obtaining four products with excellent economic value: magnetite concentrate, quartz, biotite, and garnet concentrate.
[0010] This application, through experimental research, has discovered that during weak and strong magnetic separation, when the mass concentration of a certain particle size of magnetic material in the slurry exceeds a certain range, magnetic agglomeration will occur or the magnetic agglomeration will be drastically aggravated. By strictly controlling the magnetic field strength and slurry concentration during weak and strong magnetic separation in the process flow, magnetic agglomeration can be avoided and exacerbated, thereby significantly reducing the adverse effects of magnetic agglomeration and saving enterprise costs. Combined with gravity separation and flotation steps, the purity and recovery rate of magnetite concentrate, quartz products, biotite products, and garnet concentrate can be effectively improved.
[0011] After screening, magnetite tailings yield three different particle sizes of minerals to be magnetically separated. The magnetic field strength of the weak magnetic separation is controlled at 0.2-0.3T, combined with wet pulse magnetic separation. This allows for the initial separation of strongly magnetic minerals from the skarn magnetite tailings, resulting in a magnetite concentrate product with high total iron content. This maximizes the separation of strongly magnetic minerals, leading to a magnetite concentrate product with high recovery and purity. The magnetic field strength of the strong magnetic separation is controlled at 1-1.2T, combined with wet high-gradient strong magnetic separation. This maximizes the separation of weakly magnetic minerals (containing garnet and biotite) from non-magnetic minerals (containing quartz), achieving the enrichment of garnet, quartz, and biotite respectively. After the garnet and biotite in weakly magnetic minerals I, II, and III are enriched, subsequent grinding and gravity separation steps can simultaneously yield garnet and biotite products with high purity and good recovery. After the quartz in non-magnetic mineral I, non-magnetic mineral II, and non-magnetic mineral III is enriched, and with the subsequent quartz flotation step, a quartz product with high silica content and good recovery rate can be obtained at the same time, and the purity of quartz can be effectively improved.
[0012] The method described in this application allows for the comprehensive and systematic utilization of different types and sizes of skarn iron ore tailings. It enables the separate, enrichment, and purification of economically valuable products such as magnetite concentrate, garnet, quartz, and biotite from these tailings. High-purity magnetite concentrate, garnet, quartz, and biotite products are obtained. The resulting mineral waste, flotation waste I, and flotation waste II can be mixed to produce building materials for cement, concrete admixtures, and non-fired bricks. This method solves the problem of separating multiple economically valuable minerals from tailings to obtain various products. Furthermore, it ensures that the purified products simultaneously possess high purity and high recovery rates, further addressing the challenge of achieving both high purity and high recovery rates when separating or purifying multiple economically valuable minerals from tailings. The method described in this application has low processing costs and high economic benefits, eliminating the safety hazards and adverse environmental impacts of long-term tailings accumulation.
[0013] Furthermore, the weak magnetic separation method adopts wet pulse magnetic separation; the strong magnetic separation method adopts wet strong magnetic separation.
[0014] The weak magnetic separation method uses wet pulse magnetic separation, and the equipment is a semi-countercurrent pulse drum magnetic separator. The strong magnetic separation method uses wet strong magnetic separation, and the equipment is a wet high-gradient pulse strong magnetic separator. The separation effect of weak magnetic separation and strong magnetic separation is better than that of dry magnetic separation, strong magnetic separation using a flat plate strong magnetic separator, and weak magnetic separation using a barrel-type weak magnetic separator.
[0015] Furthermore, the gravity separation equipment selected is a suspended vibrating conical grooved concentrator. Compared with a slime shaking table, the suspended vibrating conical grooved concentrator has the advantages of larger single-unit processing capacity, easier operation, wider range of requirements for mineral processing parameters, and higher purity and recovery rate of the concentrate when processing minerals with fine particle size.
[0016] Furthermore, in the re-selection step, the particle size of the garnet concentrate obtained is <0.04 mm.
[0017] Furthermore, non-magnetic minerals I and II are first ground to a particle size of less than 0.1 mm before flotation. Similarly, gravity separation tailings are first ground to a particle size of less than 0.1 mm before flotation. This initial grinding facilitates the maximum separation of quartz from other minerals, garnet concentrate from other minerals, and biotite from other minerals. This improves the separation efficiency of quartz, garnet concentrate, and biotite from other mineral components during flotation and gravity separation, thereby increasing the silica content and recovery rate in quartz products, garnet content and recovery rate in garnet products, and biotite content and recovery rate in biotite products. This results in quartz products with higher purity and better recovery rates for each of these minerals.
[0018] Preferably, the process of flotation of non-magnetic mineral I, non-magnetic mineral II, and non-magnetic mineral III to obtain quartz product and flotation waste I includes: grinding non-magnetic mineral I and non-magnetic mineral II to a particle size of less than 0.1 mm, then mixing them with non-magnetic mineral III, adjusting the slurry to a mass concentration of 30-40%, adjusting the pH to 6.5-7.5, and using a fatty acid anionic collector for flotation.
[0019] Furthermore, the fatty acid anionic collector is sodium oleate or oleic acid.
[0020] Sodium oleate is selected as the preferred fatty acid anion collector.
[0021] By adopting the above technical solution, non-magnetic mineral I and non-magnetic mineral II are first ground to a particle size of less than 0.1 mm. This facilitates the maximum separation of quartz from other minerals, increasing the silica content in the quartz product. The flotation pulp is then conditioned to obtain a quartz product with better purity and recovery rate. Experimental studies have shown that when the conditioned pulp concentration exceeds 40%, the flotation pulp becomes too viscous, resulting in poor removal of aluminosilicate minerals and a decrease in the quality of the quartz product. Conversely, lower concentrations result in smaller batch sizes, reducing production efficiency and increasing production costs.
[0022] Sodium oleate is selected as the collector in this step. Sodium oleate can act as a collector and a foaming agent. Sodium oleate reacts with aluminum ions on the surface of aluminosilicate minerals to form hydrophobic aluminum oleate, which adheres to the surface of aluminosilicate minerals, making the aluminosilicate minerals hydrophobic. Under stirring, a large number of small bubbles are generated at the bottom of the flotation machine. The bubbles rise from the bottom to the surface of the solution. As the bubbles rise, the aluminosilicate minerals with hydrophobic aluminum oleate attached to them are adsorbed onto the bubbles and carried to the surface of the pulp solution. The hydrophilic quartz remains in the pulp solution and precipitates at the bottom of the flotation cell, thus achieving the purpose of separation from aluminosilicate minerals. Experiments have shown that adding 200-400g of sodium oleate per 1t of magnetic mineral solids results in better flotation. When the amount of sodium oleate is less than 200g / t, the purity of the quartz product will drop sharply. When the amount of sodium oleate is more than 400g / t, more foam will be generated and it will be difficult to defoam, which will cause trouble for subsequent processes and increase production costs.
[0023] Preferably, the biotite rough concentrate and gravity separation tailings are subjected to flotation separately. The flotation conditions are as follows: after adjusting the pulp to a mass concentration of 30-40%, a depressant is added and the pH is adjusted to 7.5-8.5. Acetate amine cationic collectors and fatty acid anionic collectors are used for flotation.
[0024] Preferably, the inhibitor comprises one of calcium lignosulfonate, sodium carbonate, and water glass.
[0025] Preferably, the acetic acid amine cationic collector includes at least one of laurylamine, octadecylamine, and dodecyl cocoylamine.
[0026] Furthermore, the acetic acid amine cationic collector is a mixture of octadecylamine and laurylamine.
[0027] Preferably, the fatty acid anionic collector is oleic acid or sodium oleate.
[0028] Furthermore, the fatty acid anionic collector is sodium oleate.
[0029] By employing the above technical solution, flotation is carried out under alkaline conditions. First, inhibitors are added and pre-adsorbed onto the surface of weakly magnetic minerals, significantly reducing the adsorption of acetic acid amine cationic collectors on the surface of weakly magnetic minerals. This inhibits the flotation of weakly magnetic minerals. Meanwhile, after the layered structure of biotite dissociates, a large number of anions (O3) are exposed on its surface. 2-A mixture of laurylamine and octadecylamine was used as an acetic acid amine cationic collector, which was adsorbed onto the surface of biotite by electrostatic means. The fatty acid anionic collector neutralized the charge of the hydrolyzed components of laurylamine and octadecylamine, reducing the critical micelle concentration of the laurylamine and octadecylamine cationic collectors. This resulted in better flotation performance and more effective separation of biotite, yielding a biotite product with good recovery rate and high purity.
[0030] Optimizing the selection of components for acetic acid amine cationic collectors and fatty acid anionic collectors improves the collection effect in the flotation step, thereby increasing the purity of each product. Using a mixture of laurylamine and octadecylamine in combination with sodium oleate as a collector for flotation achieves a flotation recovery rate of ≥85%, and the purity of the obtained biotite product can reach ≥75%. Laurylamine, octadecylamine, and sodium oleate are readily available, widely sourced, and inexpensive, effectively reducing enterprise costs and bringing better economic value.
[0031] Preferably, based on the flotation pulp, the dosage of the acetic acid amine cationic collector is 0.4-1.0 L / t, and the dosage of the fatty acid anionic collector is 1.0-1.3 L / t.
[0032] More preferably, the dosage of the acetic acid amine cationic collector is 0.5-0.9 L / t; the dosage of the fatty acid anionic collector is 1.05-1.25 L / t.
[0033] By adopting the above technical solution, it is found that using a mixture of cationic and anionic collectors in the flotation process increases the difficulty of flotation, makes it difficult to control product quality, and results in unstable and fluctuating product quality. Experimental studies have shown that only by strictly controlling the ratio between amine acetate cationic collectors and fatty acid anionic collectors within the above-mentioned dosage range can excellent collection effects be achieved and product quality be significantly improved.
[0034] Preferably, in the gravity separation step, the weakly magnetic mineral I, weakly magnetic mineral II, and weakly magnetic mineral III are first slurried to a mass concentration of 40-50%, 30-40%, and 20-30% respectively before gravity separation. After grinding the garnet rough concentrate, the slurry is first slurried to a mass concentration of 20-30% before gravity separation.
[0035] By adopting the above technical solution, the mass concentration of each component after slurry conditioning during the gravity separation process is optimized, thereby improving the separation effect of the gravity separation method on the components.
[0036] Preferably, in the weak magnetic separation step, the magnetic field strength for weak magnetic separation of mineral I is 0.2-0.25T, the magnetic field strength for weak magnetic separation of mineral II is 0.2-0.3T, and the magnetic field strength for weak magnetic separation of mineral III is 0.25-0.3T.
[0037] Preferably, in the strong magnetic separation step, the magnetic field strength for strong magnetic separation of tailings I under weak magnetic separation is 1-1.1T, the magnetic field strength for strong magnetic separation of tailings II under weak magnetic separation is 1.05-1.15T, and the magnetic field strength for strong magnetic separation of tailings III under weak magnetic separation is 1.1-1.2T.
[0038] By adopting the above technical solution, different magnetic field strengths can be selected for minerals of different particle sizes, which can maximize the separation of various products and achieve the purpose of enrichment. This is beneficial to the subsequent steps and yields magnetite concentrate, garnet, quartz and biotite products with high recovery rate and good purity.
[0039] Furthermore, the mass concentrations of the weak magnetic separation tailings I, weak magnetic separation tailings II, and weak magnetic separation tailings III subjected to strong magnetic separation are 40-50%, 30-40%, and 20-30%, respectively.
[0040] By adopting the above technical solution, the mass concentration of each component after slurry conditioning during the high-intensity magnetic separation process is optimized, thereby improving the separation effect of the high-intensity magnetic separation method on the components.
[0041] Preferably, in the screening step, the magnetite tailings are slurryed to form a slurry with a mass concentration of 40-50% before screening.
[0042] By adopting the above technical solution, the mass concentration of magnetite tailings after slurry conditioning in the screening step is optimized, which is beneficial to improving the screening effect of tailings.
[0043] In summary, this application has the following beneficial effects: 1. This application employs a method of first classifying and screening magnetite tailings, then performing weak magnetic separation followed by strong magnetic separation, combined with gravity separation and flotation. This approach facilitates the simultaneous acquisition of four economically valuable products: magnetite concentrate, quartz, biotite, and garnet concentrate. Strict control of the magnetic field strength during the weak and strong magnetic separation processes significantly reduces the adverse effects of magnetic agglomeration. Combined with gravity and flotation steps, this effectively improves the purity and recovery rate of magnetite concentrate, quartz, biotite, and garnet concentrate. Furthermore, the production process is suitable for processing various types and particle sizes of skarn-type iron ore tailings, without limitations or requirements regarding the type or particle size of the skarn-type iron ore tailings.
[0044] 2. The method described in this application allows for the comprehensive and systematic utilization of skarn-type iron ore tailings. It enables the separate, enrichment, and purification of economically valuable products such as magnetite concentrate, garnet, quartz, and biotite from the tailings, yielding high-purity magnetite concentrate, garnet, quartz, and biotite products. The resulting mineral waste, flotation waste I, and flotation waste II can be mixed to produce building materials for use in cement, concrete admixtures, and non-fired bricks. This method solves the problem of separating multiple economically valuable minerals from tailings to obtain various products, and further addresses the challenge of simultaneously achieving high purity and high recovery rates in the products obtained after separation or purification of multiple economically valuable minerals from tailings. Attached Figure Description
[0045] Figure 1 This is a flowchart of the comprehensive recycling method for "silica-type" magnetite tailings in this application. Detailed Implementation
[0046] The embodiments of the present invention will be described in detail below with reference to the examples. However, those skilled in the art will understand that the following examples are only for illustrating the present invention and should not be regarded as limiting the scope of the present invention. Specific conditions not specified in the examples shall be carried out according to conventional conditions or conditions recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially. Example Example 1
[0047] The content of multiple elements in the tailings used in this embodiment is shown in Table 1-1, and the mineral composition in the tailings is shown in Table 1-2.
[0048] Table 1-1 Multi-element content of iron tailings
[0049] Table 1-2 Mineral composition and relative content of tailings
[0050] A comprehensive recycling method for "silica-type" magnetite tailings includes the following steps: Screening: 1000 kg of magnetite tailings was mixed with water to obtain a slurry with a mass concentration of 40%. The slurry was screened using a high-frequency fine screen to obtain mineral I with a particle size greater than 0.30 mm, mineral II with a particle size between 0.1 and 0.3 mm, and mineral III with a particle size less than 0.1 mm. Weak magnetic separation: Mineral I is mixed with water to obtain a slurry with a mass concentration of 30%, and then subjected to two weak magnetic separations under a magnetic field strength of 0.2T. Mineral II is mixed with water to obtain a slurry with a mass concentration of 30%, and then subjected to two weak magnetic separations under a magnetic field strength of 0.25T. Mineral III is mixed with water to obtain a slurry with a mass concentration of 30%, and then subjected to two weak magnetic separations under a magnetic field strength of 0.25T. The results are strong magnetic mineral I and weak magnetic separation tailings I, strong magnetic mineral II and weak magnetic separation tailings II, and strong magnetic mineral III and weak magnetic separation tailings III, respectively. The magnetite concentrate product is obtained by mixing strongly magnetic mineral I, strongly magnetic mineral II and strongly magnetic mineral III. High-intensity magnetic separation: Tailings I from weak magnetic separation are slurried to obtain a slurry with a mass concentration of 40% and subjected to two high-intensity magnetic separations under a magnetic field strength of 1T. Tailings II from weak magnetic separation are slurried to obtain a slurry with a mass concentration of 30% and subjected to two high-intensity magnetic separations under a magnetic field strength of 1.15T. Tailings III from weak magnetic separation are slurried to obtain a slurry with a mass concentration of 20% and subjected to two high-intensity magnetic separations under a magnetic field strength of 1.2T. This yields weakly magnetic mineral I and non-magnetic mineral I, weakly magnetic mineral II and non-magnetic mineral II, and weakly magnetic mineral III and non-magnetic mineral III. The weak magnetic separation method uses wet pulse magnetic separation, and the equipment is a semi-countercurrent pulse drum magnetic separator. The high-intensity magnetic separation method uses wet high-intensity magnetic separation, and the equipment is a wet high-gradient pulse high-intensity magnetic separator. Gravity separation: Weakly magnetic mineral I, weakly magnetic mineral II, and weakly magnetic mineral III are slurried to obtain slurries with mass concentrations of 50%, 40%, and 30%, respectively, and then subjected to gravity separation twice, yielding gravity separation tailings, garnet rough concentrate, and biotite rough concentrate. The garnet rough concentrate is slurried to a mass concentration of 60% and then ground to a particle size of less than 0.04 mm. After two more gravity separations, garnet concentrate and mineral waste are obtained. Flotation: Non-magnetic mineral I and non-magnetic mineral II are mixed and screened to obtain two particle sizes of non-magnetic minerals, one larger than 0.10 mm and the other smaller than 0.10 mm. The non-magnetic minerals with a particle size greater than 0.1 mm are ground to a particle size of less than 0.1 mm and then mixed with the non-magnetic minerals with a particle size of less than 0.10 mm obtained after screening and non-magnetic mineral III. The slurry is adjusted to a mass concentration of 30% to obtain flotation slurry I. The pH is adjusted to 6.5, and sodium oleate is used as the collector for flotation. Based on the amount of non-magnetic minerals per ton of flotation slurry I, the amount of sodium oleate added is 300 g, and the flotation is performed twice to obtain quartz product and flotation waste I. The gravity separation tailings were ground to a particle size of less than 0.1 mm and mixed with biotite rough concentrate to a mass concentration of 30% to obtain flotation pulp II and flotation pulp III. Sodium carbonate was added to adjust the pH to 7.5. Two flotation processes were carried out using acetic acid amine cationic collectors and fatty acid anionic collectors to obtain biotite product and flotation waste II. Based on flotation pulp II, the addition amount of amine acetate cationic collector is 0.6 L / t, and the dosage of fatty acid anionic collector is 1 L / t; Acetamide cationic collectors are obtained by uniformly mixing laurylamine, octadecylamine and water in a mass ratio of 3.5:1.5:95. Fatty acid anionic collectors are selected from sodium oleate solutions with a mass concentration of 5%. The building materials are obtained by mixing mineral waste, flotation waste I, and flotation waste II.
[0051] Example 2 A comprehensive recycling method for "silica-type" magnetite tailings includes the following steps: Screening: 1000 kg of magnetite tailings was mixed with water to obtain a slurry with a mass concentration of 50%. A high-frequency fine screen was used for screening to obtain mineral I with a particle size greater than 0.30 mm, mineral II with a particle size between 0.1 and 0.3 mm, and mineral III with a particle size less than 0.1 mm. Weak magnetic separation: Mineral I is mixed with water to obtain a slurry with a mass concentration of 25%, and then subjected to two weak magnetic separations under a magnetic field strength of 0.25T. Mineral II is mixed with water to obtain a slurry with a mass concentration of 25%, and then subjected to two weak magnetic separations under a magnetic field strength of 0.3T. Mineral III is mixed with water to obtain a slurry with a mass concentration of 28%, and then subjected to two weak magnetic separations under a magnetic field strength of 0.3T. The results are strong magnetic mineral I and weak magnetic separation tailings I, strong magnetic mineral II and weak magnetic separation tailings II, and strong magnetic mineral III and weak magnetic separation tailings III, respectively. The magnetite concentrate product is obtained by mixing strongly magnetic mineral I, strongly magnetic mineral II and strongly magnetic mineral III. High-intensity magnetic separation: Weak magnetic separation tailings I are slurried to obtain a 50% slurry concentration and subjected to two high-intensity magnetic separations under a magnetic field strength of 1.1T. Weak magnetic separation tailings II are slurried to obtain a 40% slurry concentration and subjected to two high-intensity magnetic separations under a magnetic field strength of 1.05T. Weak magnetic separation tailings III are slurried to obtain a 30% slurry concentration and subjected to two high-intensity magnetic separations under a magnetic field strength of 1.1T. This yields weakly magnetic mineral I and non-magnetic mineral I, weakly magnetic mineral II and non-magnetic mineral II, and weakly magnetic mineral III and non-magnetic mineral III. The weak magnetic separation method uses wet pulse magnetic separation, and the equipment is a semi-countercurrent pulse drum magnetic separator. The high-intensity magnetic separation method uses wet high-intensity magnetic separation, and the equipment is a wet high-gradient pulse high-intensity magnetic separator. Gravity separation: Weakly magnetic mineral I, weakly magnetic mineral II, and weakly magnetic mineral III are slurried to obtain slurries with mass concentrations of 40%, 30%, and 20%, respectively, and then subjected to three gravity separations to obtain gravity separation tailings, garnet rough concentrate, and biotite rough concentrate. The garnet rough concentrate is slurried to a mass concentration of 70% and then ground to a particle size of less than 0.04 mm. After three more gravity separations, garnet concentrate and mineral waste are obtained. Flotation: Non-magnetic mineral I and non-magnetic mineral II are ground to a particle size of less than 0.1 mm, then mixed with non-magnetic mineral III, and the slurry is adjusted to a mass concentration of 40% and the pH is adjusted to 7.5. Sodium oleate is selected as the collector for flotation. Based on the mass of non-magnetic mineral solids per ton, the amount of sodium oleate added is 400 g, and the number of flotation times is 3 times to obtain quartz product and flotation waste I. Biotite rough concentrate and gravity separation tailings were adjusted to a mass concentration of 40% to obtain flotation slurry. Sodium carbonate was added to adjust the pH to 8.5. Acetate amine cationic collector and fatty acid anionic collector were used for three flotation processes to obtain biotite product and flotation waste II. Based on flotation pulp, the addition amount of acetic acid amine cationic collector is 0.4 L / t, and the dosage of fatty acid anionic collector is 1.3 L / t; Acetamide cationic collectors are obtained by uniformly mixing laurylamine, octadecylamine and water in a mass ratio of 1.5:3.5:95. Fatty acid anionic collectors are selected from sodium oleate solutions with a mass concentration of 5%. The building materials are obtained by mixing mineral waste, flotation waste I, and flotation waste II.
[0052] Example 3 The difference from Example 1 is that, in the flotation process: non-magnetic mineral I and non-magnetic mineral II are ground to a particle size of less than 0.1 mm, then mixed with non-magnetic mineral III, and the slurry is adjusted to a mass concentration of 50%, the pH is adjusted to 7.5, and oleic acid is used as the collector for flotation. Based on the total amount of non-magnetic mineral solids per ton, the amount of sodium oleate added is 200 g, and the number of flotation times is 3, to obtain quartz product and flotation waste I. Everything else is the same as in Example 1.
[0053] Example 4 Flotation: The biotite rough concentrate and gravity separation tailings are adjusted to a mass concentration of 35% to obtain flotation slurry. Water glass is added to adjust the pH to 8.5. Two flotation processes are carried out using amine acetate cationic collectors to obtain biotite product and flotation waste II. Based on the flotation pulp, the addition amount of amine acetate cationic collector is 1.4 L / t; Everything else is the same as in Example 1.
[0054] Example 5 The difference from Example 1 is that in the flotation step, the mass concentration of the pulp is 50% and the number of flotation steps is 2.
[0055] Example 6 The difference from Example 1 is that in the gravity separation step, weakly magnetic mineral I, weakly magnetic mineral II, and weakly magnetic mineral III are respectively slurried to obtain slurries with mass concentrations of 60%, 50%, and 40%, and are respectively subjected to two gravity separations; the garnet rough concentrate is slurried to a mass concentration of 40% and then ground, and the gravity separation is performed twice. The remaining steps and conditions are the same as in Example 1.
[0056] Comparative Example 1 The difference from Example 1 is that after the tailings are screened, they are first subjected to strong magnetic separation, followed by weak magnetic separation. The remaining steps are the same as in Example 1. The strong magnetic separation process is as follows: mineral I is slurried to obtain a slurry with a mass concentration of 40%, and then subjected to two strong magnetic separations under a magnetic field strength of 1T; mineral II is slurried to obtain a slurry with a mass concentration of 30%, and then subjected to two strong magnetic separations under a magnetic field strength of 1.15T; mineral III is slurried to obtain a slurry with a mass concentration of 20%, and then subjected to two strong magnetic separations under a magnetic field strength of 1.2T, resulting in strong magnetic mineral I and weak magnetic mineral I, strong magnetic mineral II and weak magnetic mineral II, and strong magnetic mineral III and weak magnetic mineral III. The weak magnetic separation process is as follows: Weakly magnetic mineral I is mixed with water to obtain a slurry with a mass concentration of 30%, and then subjected to two weak magnetic separations under a magnetic field strength of 0.2T. Weakly magnetic mineral II is mixed with water to obtain a slurry with a mass concentration of 30%, and then subjected to two weak magnetic separations under a magnetic field strength of 0.2T. Weakly magnetic mineral III is mixed with water to obtain a slurry with a mass concentration of 30%, and then subjected to two weak magnetic separations under a magnetic field strength of 0.25T. This yields weakly magnetic mineral I and non-magnetic mineral I, weakly magnetic mineral II and non-magnetic mineral II, and weakly magnetic mineral III and non-magnetic mineral III, respectively.
[0057] Comparative Example 2 The difference from Example 1 is that, Weak magnetic separation: Mineral I is subjected to two weak magnetic separations under a magnetic field strength of 0.35T, mineral II is subjected to two weak magnetic separations under a magnetic field strength of 0.4T, and mineral III is subjected to two weak magnetic separations under a magnetic field strength of 0.45T, to obtain strong magnetic mineral I and weak magnetic separation tailings I, strong magnetic mineral II and weak magnetic separation tailings II, and strong magnetic mineral III and weak magnetic separation tailings III, respectively. Strong magnetic separation: Weak magnetic separation tailings I are subjected to two strong magnetic separations under a magnetic field strength of 1.3T, weak magnetic separation tailings II are subjected to two strong magnetic separations under a magnetic field strength of 1.4T, and weak magnetic separation tailings III are subjected to two strong magnetic separations under a magnetic field strength of 1.5T, to obtain weak magnetic mineral I and non-magnetic mineral I, weak magnetic mineral II and non-magnetic mineral II, weak magnetic mineral III and non-magnetic mineral III; Everything else is the same as in Example 1.
[0058] Comparative Example 3 The difference from Example 1 is that the tailings are directly subjected to weak magnetic separation, strong magnetic separation, gravity separation and flotation, and the corresponding steps and conditions are the same as in Example 1.
[0059] Comparative Example 4 Weak magnetic separation: Mineral I, mineral II, and mineral III are subjected to two weak magnetic separations at a slurry concentration of 40%, respectively, to obtain strong magnetic mineral I and weak magnetic separation tailings I, strong magnetic mineral II and weak magnetic separation tailings II, and strong magnetic mineral III and weak magnetic separation tailings III. Strong magnetic separation: Weak magnetic separation tailings I, weak magnetic separation tailings II, and weak magnetic separation tailings III are subjected to two strong magnetic separations at pulp mass concentrations of 60%, 50%, and 40%, respectively, to obtain weak magnetic mineral I and non-magnetic mineral I, weak magnetic mineral II and non-magnetic mineral II, and weak magnetic mineral III and non-magnetic mineral III. Everything else is the same as in Example 1.
[0060] Comparative Example 5 The difference from Example 1 is that all grinding steps are omitted, while the rest are the same as in Example 1.
[0061] Comparative Example 6 The difference from Example 1 is that in the flotation steps of biotite rough concentrate and gravity separation tailings, sodium hydroxide solution is used to adjust the pH value and no inhibitor is added; otherwise, it is the same as Example 1.
[0062] The purity and recovery rate of the products obtained from Examples 1-6 and Comparative Examples 1-6 are shown in Table 2.
[0063] Table 2
[0064] As can be seen from Examples 1-6 of this application and Table 2, the specific process method of this application can simultaneously obtain garnet products, quartz products, biotite products, and magnetite concentrate products with high purity and high recovery rate.
[0065] As can be seen from Example 1 and Comparative Example 1, combined with Table 2, the recovery rates of garnet, quartz, and biotite products obtained by the method of first performing strong magnetic separation and then weak magnetic separation decreased, and the total iron content of the magnetite concentrate product decreased significantly compared with Example 1. This is because the strong magnetic separation followed by weak magnetic separation caused magnetic agglomeration, and non-magnetic and weakly magnetic minerals in the tailings entered the magnetite concentrate product, resulting in a decrease in the recovery rate of garnet, quartz, and biotite products, and a decrease in the purity of the magnetite concentrate product.
[0066] As can be seen from Example 1 and Comparative Example 2, combined with Table 2, the purity of garnet products, biotite products, and magnetite concentrate products obtained by increasing the magnetic field strength during weak and strong magnetic separation, as well as the recovery rates of garnet products, biotite products, and quartz products, all decreased. This indicates that increasing the magnetic field strength during weak and strong magnetic separation caused some minerals (intergrowths between strongly magnetic minerals, weak magnetic minerals, and non-magnetic minerals) in the tailings to remain undissociated. Due to the increased magnetic field strength, after weak magnetic separation, some weak magnetic minerals (intergrowths with strongly magnetic minerals) and non-magnetic minerals (intergrowths with strongly magnetic minerals) entered the magnetite concentrate, and after strong magnetic separation, some non-magnetic minerals (intergrowths with weak magnetic minerals) entered the garnet and biotite products.
[0067] As can be seen from Example 1 and Comparative Example 3, and in conjunction with Table 2, the purity and recovery rate of the four products obtained by using the non-screening step decreased significantly. This indicates that there are strict requirements on particle size when minerals are sorted. At the same time, process conditions such as pulp concentration, magnetic field strength, pulp pH value, and collector are also required to obtain the best sorting effect and improve the purity and recovery rate of the four products.
[0068] As can be seen from Examples 1 and 4, and in conjunction with Table 2, the purity of biotite and magnetite concentrate products, as well as the recovery rates of biotite, garnet, and quartz products, decreased to some extent when the slurry concentration was increased during weak and strong magnetic separation. This is because increasing the slurry concentration during weak and strong magnetic separation increases the viscosity of the slurry and causes magnetic agglomeration, leading to the adhesion or agglomeration of some minerals (strongly magnetic, weakly magnetic, and non-magnetic minerals) in the tailings. After weak magnetic separation, some weakly magnetic and non-magnetic minerals enter the magnetite product, while after strong magnetic separation, some non-magnetic minerals enter the weakly magnetic minerals (garnet and biotite products).
[0069] As can be seen from Example 1 and Comparative Example 5, combined with Table 2, omitting all grinding steps resulted in a significant decrease in the purity and recovery rate of the magnetite concentrate product, while the purity and recovery rate of the other products were basically unaffected. This is because the absence of grinding steps caused some minerals (strongly magnetic minerals, weakly magnetic minerals, and non-magnetic minerals) in the tailings to remain intergrowths and not to separate, thus preventing them from entering the (garnet product, quartz product, and biotite product) individually.
[0070] As can be seen from Example 1 and Comparative Example 6, and in conjunction with Table 2, the purity of the biotite product obtained in Comparative Example 6 is significantly poor. This is because the absence of inhibitors allows some weakly magnetic minerals in the pulp to be captured and incorporated into the biotite product during flotation.
[0071] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A comprehensive recycling method for "silica-type" magnetite tailings, characterized in that, The method includes: Screening: The magnetite tailings are screened to obtain mineral I with a particle size greater than 0.30 mm, mineral II with a particle size between 0.1 and 0.3 mm, and mineral III with a particle size less than 0.1 mm. Weak magnetic separation: Mineral I, mineral II, and mineral III are slurried to a mass concentration of 20-30%, and mineral I is subjected to at least one weak magnetic separation at a magnetic field strength of 0.2-0.25T, mineral II at a magnetic field strength of 0.2-0.3T, and mineral III at a magnetic field strength of 0.25-0.3T, respectively, to obtain strong magnetic mineral I and weak magnetic separation tailings I, strong magnetic mineral II and weak magnetic separation tailings II, and strong magnetic mineral III and weak magnetic separation tailings III, respectively. Strong magnetic mineral I, strong magnetic mineral II, and strong magnetic mineral III are mixed to obtain magnetite concentrate product; Strong magnetic separation: Weak magnetic separation tailings I, II, and III are slurried to a mass concentration of 20-50%. Weak magnetic separation tailings I are subjected to strong magnetic separation at least once under a magnetic field strength of 1-1.1T, weak magnetic separation tailings II under a magnetic field strength of 1.05-1.15T, and weak magnetic separation tailings III under a magnetic field strength of 1.1-1.2T, to obtain weak magnetic mineral I and non-magnetic mineral I, weak magnetic mineral II and non-magnetic mineral II, and weak magnetic mineral III and non-magnetic mineral III. Gravity separation: Weakly magnetic mineral I, weakly magnetic mineral II, and weakly magnetic mineral III are first slurried to a mass concentration of 40-50%, 30-40%, and 20-30%, respectively, and then gravity separation is performed separately to obtain gravity separation tailings, garnet rough concentrate, and biotite rough concentrate. The garnet rough concentrate is ground to a particle size of less than 0.04 mm, slurried to a mass concentration of 20-30%, and then gravity separation is performed to obtain garnet concentrate and mineral waste. Flotation: Non-magnetic mineral I, non-magnetic mineral II, and non-magnetic mineral III are floated. The flotation conditions include: grinding non-magnetic mineral I and non-magnetic mineral II to a particle size of less than 0.1 mm, then mixing them with non-magnetic mineral III, adjusting the slurry to a mass concentration of 30-40%, adjusting the pH to 6.5-7.5, and using fatty acid anionic collectors for flotation. Biotite rough concentrate and gravity separation tailings were subjected to flotation separately. The flotation conditions included: adjusting the pulp to a mass concentration of 30-40% to obtain flotation pulp, adding depressants and adjusting the pH to 7.5-8.5, and using acetic acid amine cationic collectors and fatty acid anionic collectors for flotation.
2. The comprehensive recycling method for "silica-type" magnetite tailings according to claim 1, characterized in that... The inhibitors include one of calcium lignosulfonate, sodium carbonate, and water glass.
3. The comprehensive recycling method for "silica-type" magnetite tailings according to claim 1, characterized in that: The acetic acid amine cationic collectors include at least one of laurylamine, octadecylamine, and dodecacoamine.
4. The comprehensive recycling method for "silica-type" magnetite tailings according to claim 1, characterized in that: The fatty acid anionic collector is oleic acid or sodium oleate.
5. The comprehensive recycling method for "silica-type" magnetite tailings according to claim 1, characterized in that: Based on the flotation pulp, the dosage of the acetic acid amine cationic collector is 0.4-1 L / t, and the dosage of the fatty acid anionic collector is 1.0-1.3 L / t.
Citation Information
Patent Citations
Rutile ore part size fraction benefication joint production process
CN102728451A
Magnetic levitation combined beneficiation method for biotite type ore containing rubidium
CN108816499A
Pyrophyllite dry method magnetic separation spiral propulsion continuous processing technology
CN115608497A