A positive electrode precursor with high specific surface and high tap density, a preparation method and application thereof

By combining doping elements with viscosity modifiers, cathode precursor materials with high specific surface area and high tap density were prepared, which solved the contradiction between increasing specific surface area and tap density in ternary cathode materials, simplified the process and reduced costs.

CN117865233BActive Publication Date: 2026-11-20JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311806833.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2026-11-20
Estimated Expiration
2043-12-26

AI Technical Summary

Technical Problem

How to increase the specific surface area of ​​ternary cathode materials while maintaining a high tap density, so as to improve the performance of lithium-ion batteries?

Method used

By working synergistically with dopants and viscosity modifiers, uniform co-precipitation of nickel, cobalt, manganese and dopants is achieved, changing the chemical interlayer spacing and regulating the viscosity of the reaction solution, thereby preparing cathode precursor materials with high specific surface area and high tap density.

Benefits of technology

This method simultaneously increases the specific surface area and tap density of the cathode precursor material, simplifies the preparation process, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117865233B_ABST
    Figure CN117865233B_ABST
Patent Text Reader

Abstract

The application provides a high-specific-surface and high-tapped positive electrode precursor as well as a preparation method and application thereof. The preparation method comprises the following steps: adding a mixed salt solution of nickel-cobalt-manganese and a doping element, a precipitant solution, a complexing agent solution and a viscosity regulator solution into a flow, performing a co-precipitation reaction, and obtaining the high-specific-surface and high-tapped positive electrode precursor. The preparation method provided by the application, through the synergistic cooperation of the doping element and the viscosity regulator, jointly acts on the positive electrode precursor material, so that the positive electrode precursor material with high specific surface area and high tapped density is obtained; and the preparation method is simple to operate, does not need to increase a new preparation process, reduces process transformation, and reduces preparation cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion battery technology, and relates to a positive electrode precursor with high specific surface area and high tap, its preparation method and application. Background Technology

[0002] The demand for high-energy and high-safety lithium-ion batteries has driven the continuous search for battery systems with superior performance. Currently, the most commonly used and relatively mature cathode materials for lithium-ion batteries are lithium cobalt oxide (LiCoO2), lithium nickel oxide, and lithium manganese oxide (Li...). x Lithium iron phosphate (LiFePO4), lithium nickel cobalt manganese oxide (NCO), and other lithium iron phosphate cathode materials have been the subject of extensive basic research and have largely achieved industrialization both domestically and internationally. Compared to these traditional cathode materials, layered lithium nickel cobalt manganese oxide cathode materials (hereinafter referred to as "ternary materials" or "NCM") combine the advantages of lithium cobalt oxide, lithium nickel oxide, and lithium manganese oxide, with the synergistic effect of the ternary structure giving them superior overall performance compared to any single-component compound. Due to their high specific capacity, stable cycle performance, relatively low cost, and good safety performance, they have been proven to be ideal cathode materials for power batteries.

[0003] In principle, the tap density and specific surface area of ​​ternary cathode materials are mutually inhibiting. A high tap density (TD) ensures the volumetric capacity of the material, providing more capacity for the same volume. A high BET provides more ion movement channels, making the material's capacity closer to the theoretical capacity.

[0004] For example, CN115353153A discloses a high specific surface area nickel-cobalt-manganese ternary precursor and its preparation method, belonging to the field of lithium battery material technology. In the co-precipitation process of the nickel-cobalt-manganese ternary precursor, at least one of air, oxygen, or ozone is introduced into the reaction system. By adjusting the flow rate of air, oxygen, or ozone, precipitation and oxidation occur simultaneously, thereby refining the primary particles of the nickel-cobalt-manganese ternary precursor and increasing the specific surface area of ​​the secondary particles.

[0005] For example, CN102280619A discloses a method for preparing a high-taper spherical ternary cathode material precursor. Nickel salt, cobalt salt, manganese salt, alkaline aqueous solution, and a complexing agent are placed in a reaction vessel. A controlled crystallization method is used to stably control the synthesis process parameters, synthesizing a spherical or near-spherical ternary cathode material precursor with the chemical formula Ni. x Co y Mn z(OH)₂, 0.5≤X≤1, 0≤Y≤0.5, 0≤Z≤0.5, X+Y+Z=1, surface treatment by adjusting pH with alkali, followed by washing and drying to obtain the ternary cathode material precursor. This invention improves the processing performance and tap density of ternary cathode materials, overcomes material capacity and stability defects, and controls the physicochemical properties of ternary cathode materials by controlling the morphology and particle size of the precursor, thereby improving material stability.

[0006] In principle, the tap density and specific surface area of ​​ternary cathode materials are mutually inhibiting. However, maintaining a high tap density while seeking a larger specific surface area has always been a pursuit of major manufacturers.

[0007] Therefore, how to obtain a cathode precursor material that combines high specific surface area and high tap density is an urgent technical problem to be solved. Summary of the Invention

[0008] To address the shortcomings of existing technologies, the present invention aims to provide a cathode precursor with high specific surface area and high tap density, its preparation method, and its applications. The preparation method provided by the present invention, through the synergistic effect of doping elements and viscosity modifiers, yields a cathode precursor material possessing both high specific surface area and high tap density. Furthermore, the preparation method is simple to operate, requiring no additional preparation steps, reducing process modifications, and lowering preparation costs.

[0009] To achieve this objective, the present invention adopts the following technical solution:

[0010] In a first aspect, the present invention provides a method for preparing a positive electrode precursor with high specific surface area and high tap, the preparation method comprising the following steps:

[0011] A mixed salt solution of nickel, cobalt, manganese and doping elements, a precipitant solution, a complexing agent solution and a viscosity modifier solution are added in parallel to carry out a co-precipitation reaction to obtain the high specific surface area and high tap positive electrode precursor.

[0012] The preparation method provided by this invention achieves uniform co-precipitation of nickel, cobalt, and manganese with the dopant through the synergistic effect of the dopant element and viscosity modifier. The uniformly doped metal ions change the original chemical interlayer spacing, thereby increasing the BET of the material. The addition of the viscosity modifier regulates the polarity in the solution, changes the viscosity of the reaction solution, and makes the single crystals aggregate more tightly, ensuring the tap density of the material. Thus, a cathode precursor material with both high specific surface area and high tap density is obtained. Moreover, the preparation method is simple to operate. The co-feeding of the ternary solution and the dopant reduces redundant steps, eliminates the need for additional preparation steps, reduces process modification, and lowers the preparation cost.

[0013] In this invention, without co-precipitation of doping elements, it is difficult to increase the specific surface area of ​​the precursor while maintaining tap density; and without adding a viscosity modifier solution, the goal of increasing the tap density of the precursor material cannot be achieved. That is, in this application, doping and viscosity modifier solutions must work together to achieve the effect of simultaneously increasing the specific surface area and tap density of the cathode precursor material.

[0014] Preferably, the concentration of nickel, cobalt, and manganese in the mixed salt solution of nickel, cobalt, and manganese and the doping element is 1.5 to 2 mol / L, such as 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L, or 2 mol / L.

[0015] Preferably, the concentration of the dopant element in the mixed salt solution of nickel, cobalt, manganese and the dopant element is 0.01 to 0.2 mol / L, for example, 0.01 mol / L, 0.03 mol / L, 0.05 mol / L, 0.08 mol / L, 0.1 mol / L, 0.13 mol / L, 0.15 mol / L, 0.18 mol / L or 0.2 mol / L, etc.

[0016] In this invention, by adjusting the concentration of dopant elements in the mixed salt solution, the specific surface area of ​​the precursor is increased. If the concentration is too low, the improvement effect is not obvious, while if the concentration is too high, the capacity of the cathode will be severely lost in the later stage.

[0017] Preferably, the doping element includes any one or a combination of at least two of Al, Mg, Cu, Fe, V, Zr, W, Mo or Ti, with Cu being the most preferred.

[0018] In this invention, Cu is selected as the dopant element, which can better improve the specific surface area of ​​the precursor material.

[0019] Preferably, the precipitant solution comprises a liquid alkali solution.

[0020] Preferably, the liquid alkaline solution includes sodium hydroxide solution and / or potassium hydroxide solution.

[0021] Preferably, the complexing agent solution comprises an aqueous ammonia solution.

[0022] Preferably, the flow rate of the viscosity modifier solution is 1% to 10% of the flow rate of the mixed salt solution of nickel, cobalt, manganese and doping elements, such as 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%.

[0023] In this invention, if the flow rate of the viscosity modifier solution is too small, that is, if too little viscosity modifier is added, it will not be able to improve the compaction. If the flow rate of the viscosity modifier solution is too large, that is, if too much viscosity modifier is added, it will significantly increase the stirring resistance of the reactor and increase the cost, and will have limited effect on improving the compaction density.

[0024] Preferably, the viscosity modifier solution has a mass concentration of 30-99 wt%, such as 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, 95 wt%, or 99 wt%.

[0025] Preferably, the viscosity modifier comprises any one or a combination of at least two of formamide, ethanol, polyethylene glycol, propylene glycol, glycerol, or hexane.

[0026] In this invention, the above-mentioned substances are selected as viscosity modifiers, which can achieve the control of solution polarity without affecting the normal performance of the electrochemical properties of the cathode material in the later stage.

[0027] Preferably, a protective gas is introduced during the coprecipitation reaction.

[0028] Preferably, the reaction temperature of the coprecipitation reaction is 30 to 70°C, for example, 30°C, 40°C, 50°C, 60°C or 70°C.

[0029] Preferably, the stirring rate of the coprecipitation reaction is 100 to 400 rpm, such as 100 rpm, 150 rpm, 200 rpm, 250 rpm, 300 rpm, 350 rpm or 400 rpm.

[0030] Preferably, the pH value of the coprecipitation reaction is 8 to 12, such as 8, 8.3, 8.5, 8.8, 9, 9.3, 9.5, 9.8, 10, 10.3, 10.5, 10.8, 11, 11.3, 11.5, 11.8 or 12.

[0031] Preferably, the solution after the coprecipitation reaction is washed and dried.

[0032] As a preferred technical solution, the preparation method includes the following steps:

[0033] A co-precipitation reaction was carried out in an environment with a pH of 8-12, at 30-70°C and a stirring rate of 100-400 rpm, with a mixed salt solution of nickel, cobalt, manganese and doping elements, a liquid alkali solution, an ammonia solution, and a viscosity modifier solution with a mass concentration of 30-99 wt%. The flow rate of the viscosity modifier solution was 1-10% of the flow rate of the mixed salt solution of nickel, cobalt, manganese and doping elements. The reaction was carried out by stirring at 100-400 rpm to obtain the high specific surface area and high tap positive electrode precursor.

[0034] The doping element includes any one or a combination of at least two of Al, Mg, Cu, Fe, V, Zr, W, Mo, or Ti; the concentration of the doping element in the mixed salt solution of nickel, cobalt, manganese, and the doping element is 0.01–0.2 mol / L; the viscosity modifier includes any one or a combination of at least two of formamide, ethanol, polyethylene glycol, propylene glycol, glycerol, or hexane.

[0035] In a second aspect, the present invention provides a positive electrode precursor with high specific surface area and high tap, wherein the positive electrode precursor with high specific surface area and high tap is prepared by the preparation method described in the first aspect.

[0036] Preferably, the specific surface area of ​​the high specific surface area and high tapping positive electrode precursor is 24–28 m². 2 / g, for example 24m 2 / g、25m 2 / g, 25.5m 2 / g、26m 2 / g, 26.5m 2 / g, 26.53m 2 / g、27m 2 / g, 27.5m 2 / g or 28m 2 / g etc.

[0037] Preferably, the tap density of the high specific surface area and high tap positive electrode precursor is 1.8–2.0 g / cm³. 3 For example, 1.8g / cm 3 1.81 g / cm 3 1.82g / cm 3 1.83g / cm 3 1.84 g / cm 3 1.85g / cm 3 1.86 g / cm 3 1.87 g / cm 3 1.88g / cm 3 1.89 g / cm 3 1.9g / cm 3 Or 2.0g / cm 3 wait.

[0038] Thirdly, the present invention also provides a cathode material, which is obtained by mixing and sintering a cathode precursor with high specific surface area and high tap as described in the second aspect with a lithium source.

[0039] The cathode material provided by this invention, except for cathode precursors with specific requirements, uses conventional techniques for all other raw materials and preparation processes. Those skilled in the art can make adaptive adjustments according to actual needs. Within a reasonable range, this invention applies to all cathode material preparation processes known to those skilled in the art.

[0040] Fourthly, the present invention also provides a lithium-ion battery, the lithium-ion battery comprising the positive electrode material as described in the third aspect.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] The preparation method provided by this invention achieves uniform co-precipitation of nickel, cobalt, and manganese with the dopant through the synergistic effect of the dopant element and viscosity modifier. The uniformly doped metal ions change the original chemical interlayer spacing, thereby increasing the BET of the material. The addition of the viscosity modifier regulates the polarity in the solution, changes the viscosity of the reaction solution, and makes the single crystals aggregate more tightly, ensuring the tap density of the material. Thus, a cathode precursor material with both high specific surface area and high tap density is obtained. Moreover, the preparation method is simple to operate. The co-feeding of the ternary solution and the dopant reduces redundant steps, eliminates the need for additional preparation steps, reduces process modification, and lowers the preparation cost. Attached Figure Description

[0043] Figure 1 SEM image of the cathode precursor material provided in Example 1.

[0044] Figure 2 The image shows a SEM image of the cathode precursor material provided in Example 7.

[0045] Figure 3 SEM image of the cathode precursor material provided for Comparative Example 3. Detailed Implementation

[0046] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0047] Example 1

[0048] This embodiment provides a cathode precursor material, which includes a nickel-cobalt-manganese hydroxide matrix and a dopant element Cu doped in the matrix material.

[0049] The preparation method of the positive electrode precursor material is as follows:

[0050] Step 1: Prepare a ternary mixed salt solution (sulfate, total molar concentration of nickel, cobalt and manganese is 2 mol / L) with a molar ratio of Ni:Co:Mn = 0.8:0.1:0.1 and a concentration of Cu dopant in the ternary mixed salt solution of 0.03 mol / L;

[0051] Step 2: Add the ternary mixed salt solution, sodium hydroxide solution, ammonia solution, and 50wt% polyethylene glycol viscosity modifier solution in parallel into the reactor. The flow rate of the viscosity modifier solution is 5% of the flow rate of the ternary mixed salt solution. Maintain the pH value at 9.5 and carry out a co-precipitation reaction at 40°C and a stirring rate of 280 rpm to obtain the reaction slurry.

[0052] Step 3: Feed the reaction slurry into a centrifuge and wash it with hot water and liquid alkali;

[0053] Step 4: Dry the filter residue obtained by centrifugation and washing in an oven at 150°C to finally obtain the copper-doped nickel-manganese hydroxide precursor.

[0054] Example 2

[0055] This embodiment provides a cathode precursor material, which includes a nickel-cobalt-manganese hydroxide matrix and a dopant element Cu doped in the matrix material.

[0056] The preparation method of the positive electrode precursor material is as follows:

[0057] Step 1: Prepare a ternary mixed salt solution (sulfate, total molar concentration of nickel, cobalt and manganese is 2 mol / L) with a molar ratio of Ni:Co:Mn = 0.8:0.1:0.1 and a concentration of Cu dopant in the ternary mixed salt solution of 0.1 mol / L;

[0058] Step 2: Add the ternary mixed salt solution, sodium hydroxide solution, ammonia solution, and 50wt% polyethylene glycol viscosity modifier solution in parallel into the reactor. The flow rate of the viscosity modifier solution is 1% of the flow rate of the ternary mixed salt solution. Maintain the pH value at 10.3 and carry out a co-precipitation reaction at 50°C and a stirring rate of 400 rpm to obtain a reaction slurry.

[0059] Step 3: Feed the reaction slurry into a centrifuge and wash it with hot water and liquid alkali;

[0060] Step 4: Dry the filter residue obtained by centrifugation and washing in an oven at 150°C to finally obtain the copper-doped nickel-manganese hydroxide precursor.

[0061] Example 3

[0062] This embodiment provides a cathode precursor material, which includes a nickel-cobalt-manganese hydroxide matrix and a dopant element Cu doped in the matrix material.

[0063] The preparation method of the positive electrode precursor material is as follows:

[0064] Step 1: Prepare a ternary mixed salt solution (sulfate, total molar concentration of nickel, cobalt and manganese is 2 mol / L) with a molar ratio of Ni:Co:Mn = 0.8:0.1:0.1 and a concentration of Cu dopant in the ternary mixed salt solution of 0.2 mol / L;

[0065] Step 2: Add the ternary mixed salt solution, sodium hydroxide solution, ammonia solution, and 50wt% polyethylene glycol viscosity modifier solution in parallel into the reactor. The flow rate of the viscosity modifier solution is 10% of the flow rate of the ternary mixed salt solution. Maintain the pH value at 9.5 and carry out a co-precipitation reaction at 40°C and a stirring rate of 280 rpm to obtain the reaction slurry.

[0066] Step 3: Feed the reaction slurry into a centrifuge and wash it with hot water and liquid alkali;

[0067] Step 4: Dry the filter residue obtained by centrifugation and washing in an oven at 150°C to finally obtain the copper-doped nickel-manganese hydroxide precursor.

[0068] Example 4

[0069] The difference between this embodiment and Embodiment 1 is that in this embodiment, the ternary mixed salt solution (sulfate, molar concentration of 2 mol / L) with a molar ratio of Ni:Co:Mn = 0.6:0.2:0.2 is prepared in step 1, and the concentration of the dopant element Zr in the ternary mixed salt solution is 0.03 mol / L.

[0070] In step 2, the viscosity modifier is glycerol.

[0071] The remaining preparation methods and parameters are consistent with those in Example 1.

[0072] Example 5

[0073] The difference between this embodiment and Embodiment 1 is that in step 1 of this embodiment, the concentration of Cu dopant in the ternary mixed salt solution is 0.1 mol / L.

[0074] The remaining preparation methods and parameters are consistent with those in Example 1.

[0075] Example 6

[0076] The difference between this embodiment and Embodiment 1 is that in step 1 of this embodiment, the concentration of Cu dopant in the ternary mixed salt solution is 2.5 mol / L.

[0077] The remaining preparation methods and parameters are consistent with those in Example 1.

[0078] Example 7

[0079] The difference between this embodiment and embodiment 1 is that in step 2 of this embodiment, the flow rate of the viscosity modifier solution is 0.5% of the flow rate of the ternary mixed salt solution.

[0080] The remaining preparation methods and parameters are consistent with those in Example 1.

[0081] Example 8

[0082] The difference between this embodiment and embodiment 1 is that in step 2 of this embodiment, the flow rate of the viscosity modifier solution is 15% of the flow rate of the ternary mixed salt solution.

[0083] The remaining preparation methods and parameters are consistent with those in Example 1.

[0084] Comparative Example 1

[0085] The difference between this comparative example and Example 1 is that the ternary mixed salt solution in step 1 of this comparative example does not contain the dopant element Cu (i.e., the concentration of Cu is 0 mol / L).

[0086] The remaining preparation methods and parameters are consistent with those in Example 1.

[0087] Comparative Example 2

[0088] The difference between this comparative example and Example 1 is that no viscosity modifier is added in step 2 of this comparative example.

[0089] The remaining preparation methods and parameters are consistent with those in Example 1.

[0090] Comparative Example 3

[0091] The difference between this comparative example and Example 1 is that this comparative example does not add a dopant element (i.e., the concentration of Cu is 0 mol / L) in step 1, nor does it add a viscosity modifier in step 2.

[0092] The remaining preparation methods and parameters are consistent with those in Example 1.

[0093] Figure 1 The SEM image of the cathode precursor material provided in Example 1 is shown. It can be seen that the primary crystals of the precursor are relatively small, indicating that its specific surface area is larger and the bonding is tight, indicating that the precursor has a high tap rate.

[0094] Figure 2 SEM images of the cathode precursor material provided in Example 7 are shown. It can be seen that after reducing the flow rate of the viscosity modifier, the primary crystal bonding tightness of the precursor is worse than that in Example 1.

[0095] Figure 3 The SEM image of the cathode precursor material provided in Comparative Example 3 is shown, which has a coarser primary crystal form.

[0096] Depend on Figure 1-3 It can be seen that appropriate doping elements can improve the BET of the precursor. In addition, the appropriate addition of viscosity modifiers can ensure that the BET is increased while the tap density of the precursor is also increased.

[0097] The specific surface area, tap density, and areal density of the cathode precursors provided in Examples 1-8 and Comparative Examples 1-3 were tested under the following conditions:

[0098] Tap density (TD): The tap density was tested using Dandong Baite BT-303: vibration rate 3000 times / min, vibration time 1min, vibration amplitude 3mm±0.1mm;

[0099] Specific surface area (BET): The specific surface area was measured using a US-made Micrometer and tested after degassing at 300°C in a vacuum for 1 hour.

[0100] The results of the above tests are shown in Table 1.

[0101] Table 1

[0102]

[0103]

[0104] As shown in Table 1:

[0105] The data results from Examples 1-4 show that the preparation method provided by the present invention yields a positive electrode precursor material that simultaneously achieves high specific surface area and high tap density.

[0106] The data from Examples 1, 5, and 6 show that if the concentration of the dopant element in the mixed salt solution is too low, it will not be conducive to increasing the specific surface area of ​​the precursor; while if the concentration is too high, the effect of increasing the specific surface area is limited and will reduce the specific capacity of the cathode in the later stage.

[0107] The data from Examples 1, 7, and 8 show that if the flow rate of the viscosity modifier is too small, it cannot increase the tap density of the precursor, while if the flow rate is too large, it will significantly increase the stirring resistance of the reactor and increase the cost, and the improvement in tap density will be limited.

[0108] As can be seen from the data results of Example 1 and Comparative Examples 1-3, the present invention can only achieve the purpose of simultaneously increasing the specific surface area and tap density of the precursor through the synergistic cooperation of doping elements and viscosity modifiers. If either one is missing, it is impossible to obtain a precursor with high specific surface area and high tap density.

[0109] In summary, the preparation method provided by this invention achieves uniform co-precipitation of nickel, cobalt, and manganese with the dopant through the synergistic effect of the dopant element and viscosity modifier. The uniformly doped metal ions alter the original chemical interlayer spacing, increasing the BET of the material. Meanwhile, the addition of the viscosity modifier regulates the polarity in the solution, changing the viscosity of the reaction solution and making the single crystals aggregate more tightly, ensuring the tap density of the material. Thus, a cathode precursor material with both high specific surface area and high tap density is obtained. Furthermore, the preparation method is simple to operate, and the co-feeding of the ternary solution and the dopant reduces redundant steps, eliminates the need for additional preparation steps, reduces process modification, and lowers preparation costs.

[0110] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.

[0111] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.

[0112] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.

Claims

1. A method for preparing a positive electrode precursor with high specific surface area and high tap, characterized in that, The preparation method includes the following steps: A mixed salt solution of nickel, cobalt, manganese and doping elements, a precipitant solution, a complexing agent solution and a viscosity modifier solution are added in parallel to carry out a co-precipitation reaction to obtain the high specific surface area and high tap positive electrode precursor. The concentration of the dopant element in the mixed salt solution of nickel, cobalt, manganese and dopant elements is 0.03~0.2 mol / L; The doping element includes Cu; The flow rate of the viscosity modifier solution is 1 to 10% of the flow rate of the mixed salt solution of nickel, cobalt, manganese and doping elements.

2. The method for preparing a high specific surface area and high tap positive electrode precursor according to claim 1, characterized in that, The concentration of nickel, cobalt, and manganese in the mixed salt solution of nickel, cobalt, manganese, and doping elements is 1.5~2 mol / L.

3. The method for preparing a high specific surface area and high tap positive electrode precursor according to claim 1, characterized in that, The precipitant solution includes a liquid alkali solution.

4. The method for preparing a high specific surface area and high tap positive electrode precursor according to claim 3, characterized in that, The liquid alkaline solution includes sodium hydroxide solution and / or potassium hydroxide solution.

5. The method for preparing a high specific surface area and high tap positive electrode precursor according to claim 1, characterized in that, The complexing agent solution includes an aqueous ammonia solution.

6. The method for preparing a high specific surface area and high tap positive electrode precursor according to claim 1, characterized in that, The viscosity modifier solution has a mass concentration of 30~99wt%.

7. The method for preparing a high specific surface area and high tap positive electrode precursor according to claim 1, characterized in that, The viscosity modifier includes any one or a combination of at least two of formamide, ethanol, polyethylene glycol, propylene glycol, glycerol, or hexane.

8. The method for preparing a positive electrode precursor with high specific surface area and high tap rate according to claim 1, characterized in that, A protective gas is introduced during the coprecipitation reaction.

9. The method for preparing a positive electrode precursor with high specific surface area and high tap according to claim 1, characterized in that, The reaction temperature for the coprecipitation reaction is 30~70℃.

10. The method for preparing a high specific surface area and high tap positive electrode precursor according to claim 1, characterized in that, The stirring rate for the coprecipitation reaction is 100-400 rpm.

11. The method for preparing a high specific surface area and high tap positive electrode precursor according to claim 1, characterized in that, The pH value of the coprecipitation reaction is 8~12.

12. The method for preparing a high specific surface area and high tap positive electrode precursor according to claim 1, characterized in that, The solution after the coprecipitation reaction was washed and dried.

13. The method for preparing a high specific surface area and high tap positive electrode precursor according to claim 1, characterized in that, The preparation method includes the following steps: A co-precipitation reaction is carried out in an environment with a pH of 8-12, at 30-70°C and a stirring rate of 100-400 rpm, with a mixed salt solution of nickel, cobalt, manganese and doping elements, a liquid alkali solution, an ammonia solution, and a viscosity modifier solution with a mass concentration of 30-99 wt%. The flow rate of the viscosity modifier solution is 1-10% of the flow rate of the mixed salt solution of nickel, cobalt, manganese and doping elements. The reaction is carried out by stirring at 100-400 rpm to obtain the high specific surface area and high tap positive electrode precursor. The doping element includes Cu; the concentration of the doping element in the mixed salt solution of nickel, cobalt, manganese and the doping element is 0.03~0.2 mol / L; the viscosity modifier includes any one or a combination of at least two of formamide, ethanol, polyethylene glycol, propylene glycol, glycerol or hexane.

14. A positive electrode precursor with high specific surface area and high tap rate, characterized in that, The high specific surface area and high tap value positive electrode precursor is prepared by the preparation method according to any one of claims 1-13.

15. The high specific surface area and high tapping positive electrode precursor according to claim 14, characterized in that, The specific surface area of ​​the high specific surface area and high tapping positive electrode precursor is 24~28m². 2 / g.

16. The high specific surface area and high tapping positive electrode precursor according to claim 14, characterized in that, The tap density of the high specific surface area and high tap value positive electrode precursor is 1.8~2.0 g / cm³. 3 .

17. A positive electrode material, characterized in that, The cathode material is obtained by mixing and sintering a cathode precursor with high specific surface area and high tap as described in any one of claims 14-16 with a lithium source.

18. A lithium-ion battery, characterized in that, The lithium-ion battery includes the positive electrode material as described in claim 17.

Citation Information

Patent Citations

  • Preparation method of high-strength spherical ternary cathode material precursor

    CN102280619A

  • Nickel-cobalt-manganese ternary precursor with high specific surface area and preparation method thereof

    CN115353153A

  • Single crystal nickel-cobalt-manganese lithium anode material, precursor and preparation methods for single crystal nickel-cobalt-manganese lithium anode material and precursor

    CN109461925A