Viscosity-controllable polyamide acid solution, preparation method and application thereof

By reacting modified acid anhydrides with diamines, a polyamic acid solution with controllable viscosity was prepared, which solved the problem of uncontrollable viscosity of polyamic acid solutions in the prior art, simplified the operation and improved the performance of polyimide films.

CN117866197BActive Publication Date: 2026-11-24AEROSPACE INTELLIGENT MANUFACTURING TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311798121.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2026-11-24
Estimated Expiration
2043-12-25

AI Technical Summary

Technical Problem

The viscosity of polyamic acid solutions in existing technologies is uncontrollable, resulting in poor quality of polyimide films. Furthermore, existing viscosity reduction methods are cumbersome to operate, require a variety of raw materials, and are time-consuming.

Method used

By reacting modified acid anhydrides with diamines to prepare modified acid anhydrides, and then mixing them with a reaction solution of diamine and tetracarboxylic acid dianhydrides, the molar ratio of amine to acid is controlled at around 1, simplifying the operation steps and obtaining a polyamic acid solution with controllable viscosity.

Benefits of technology

This technology enables controllable viscosity of polyamic acid solutions, simplifies operating procedures, reduces equipment requirements, and improves the glass transition temperature and mechanical properties of polyimide films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117866197B_ABST
    Figure CN117866197B_ABST
Patent Text Reader

Abstract

This invention relates to the field of polymer materials, specifically disclosing a viscosity-controllable polyamic acid solution, its preparation method, and its applications. The invention first modifies an anhydride to obtain a modified anhydride, then adds the modified anhydride to a reaction system of diamine and anhydride to obtain a viscosity-controllable polyamic acid solution. Polyimide films are successfully prepared using the obtained polyamic acid solution. The preparation method of the viscosity-controllable polyamic acid solution provided by this invention is simple, requires no complex organic raw materials, has a simple operation procedure, and requires minimal equipment, making it convenient for industrial applications in the preparation of polyimide films. This invention effectively solves the problem of uncontrollable viscosity in the preparation of polyamic acid solutions in existing technologies, which leads to poor quality polyimide films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer materials, and specifically discloses a viscosity-controllable polyamic acid solution, its preparation method, and its application. Background Technology

[0002] Polyimide films possess excellent comprehensive properties such as high temperature resistance and solvent resistance, and have wide applications in aerospace, optics, and electronics. Polyimide is a polymer material with imide rings as its structural units. It is prepared by reacting acid anhydrides and diamines in an aprotic polar solvent to obtain a polyamic acid solution, which is then cast into a wet film and imidized to obtain the polyimide film. Currently, researchers mainly control the degree of polymerization of the resulting polyamic acid precursor by controlling the feed ratio of acid anhydrides and diamines. When the theoretical ratio of anhydride to amine in the polyamic acid solution is 1, the resulting polyimide film exhibits good mechanical properties. However, at this point, the polyamic acid solution has a high viscosity, which is difficult to control during casting and other processes, leading to coating defects and requiring more sophisticated equipment.

[0003] To reduce the viscosity of polyamic acid solutions and improve processing performance, existing technologies generally reduce the viscosity of the resin solution by decreasing the molecular weight or solid content of the polyamic acid resin. However, reducing the molecular weight of the resin can negatively impact the overall performance of polyimide; reducing the solid content of the resin leads to problems such as decreased film thickness, prolonged film formation time, and increased organic solvent usage. Other methods to reduce the viscosity of polyamic acid solutions include staged synthesis, batch feeding, and solution blending, but these all suffer from cumbersome procedures, variable raw material types, and long processing times. Therefore, developing a polyamic acid solution that is simple to operate, uses readily available raw materials, and exhibits good performance is of great significance for the preparation of polyimide films. Summary of the Invention

[0004] To address the problem of uncontrollable viscosity in the preparation of polyamic acid solutions in existing technologies, which leads to poor quality polyimide films, this invention provides a method for preparing polyamic acid solutions with controllable viscosity. This invention uses modified acid anhydrides and diamines as raw materials, and obtains a polyamic acid solution with adjustable viscosity through a simple polymerization reaction. The method for preparing polyamic acid solutions provided by this invention does not require the introduction of complex organic raw materials, has simple operating procedures, requires minimal equipment, and is convenient for industrial applications in the preparation of polyimide films.

[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution.

[0006] The first aspect of this invention provides a method for preparing a polyamic acid solution with controllable viscosity, comprising the following steps:

[0007] Step 1: Disperse the acid anhydride in water under an inert atmosphere and react at 80℃-120℃ for 0.5h-2h. Filter, dry, and grind to obtain the modified acid anhydride.

[0008] Step 2: Under an inert atmosphere, dissolve the diamine in an aprotic polar solvent, add acid anhydride, and react at 10℃-80℃ for 0.5h-5h to obtain a polyamic acid precursor solution.

[0009] Step 3: Mix the modified acid anhydride and the polyamic acid precursor solution evenly, and react at 10℃-80℃ for 0.5h-2h to obtain the polyamic acid solution.

[0010] Compared to existing technologies, the polyamic acid solution provided by this invention has the advantage of controllable viscosity. The preparation of the polyamic acid solution in this invention mainly involves two steps: first, preparing a modified acid anhydride by reacting an acid anhydride with water; second, adding the modified acid anhydride to the reaction solution of diamine and tetracarboxylic dianhydride to obtain an amine-to-acid molar ratio of approximately 1, thus obtaining the polyamic acid solution. The inventors discovered that the amount of diamine and dianhydride added affects the viscosity of the polyamic acid solution. Furthermore, when water is directly reacted with diamine and tetracarboxylic dianhydride to prepare the polyamic acid solution, the solution exhibits varying degrees of blackening. However, the inventors accidentally obtained a modified acid anhydride by reacting an acid anhydride with water, and found that adding the modified acid anhydride, after reacting with water, to the reaction solution of diamine and anhydride yields a polyamic acid solution with controllable viscosity, without causing the solution to turn black. Based on this, the inventors derived the technical solution of this invention. The preparation method of this invention is simple, the reaction conditions are easy, there is no need to introduce complex organic raw materials, the equipment requirements are simple, and the obtained polyamic acid solution is easy to use in industrial applications to prepare polyimide films, providing a new approach to the preparation of polyimide films.

[0011] Preferably, in steps one and two, the acid anhydride is any one or both of aromatic acid anhydrides and aliphatic acid anhydrides.

[0012] More preferably, the anhydride is any one or two of biphenyltetracarboxylic dianhydride, cyclopentanetetracarboxylic dianhydride, or dicyclohexyltetracarboxylic dianhydride.

[0013] Preferably, in step two, the diamine is any one or both of aromatic diamines or aliphatic diamines.

[0014] More preferably, the diamine is any one or both of p-phenylenediamine or 1,4-cyclohexyldiamine.

[0015] Preferably, in step two, the aprotic polar solvent is any one or more of N,N-dimethylacetamide, N,N-dimethylformamide, or N-methylpyrrolidone.

[0016] Preferably, in step one, the mass ratio of the acid anhydride to water is 1-3:7-10.

[0017] Preferably, in step two, the molar ratio of the diamine to the acid anhydride is 0.9-1:1.

[0018] Preferably, in step three, the molar ratio of the modified acid anhydride to the diamine in the polyamic acid precursor solution is 1:0.95-1.05.

[0019] Preferably, the mass ratio of the diamine to the aprotic polar solvent is 5-8:120-140.

[0020] A second aspect of the present invention provides a viscosity-controllable polyamic acid solution, which is prepared using the aforementioned method for preparing the viscosity-controllable polyamic acid solution.

[0021] A third aspect of the present invention provides a polyimide film prepared from the aforementioned viscosity-controllable polyamic acid solution.

[0022] The fourth aspect of the present invention provides a method for preparing the polyimide film, comprising the following steps: coating a glass substrate with a viscosity-controllable polyamic acid solution, gradually heating to 415℃-425℃ under an inert atmosphere, holding at the temperature for 8min-12min, cooling, and peeling to obtain a polyimide film.

[0023] Preferably, the coating thickness is 0.5mm-1mm.

[0024] Preferably, the gradient heating is performed using a programmed heating method, specifically the following steps: heating at a rate of 2℃ / min-3℃ / min to 100℃-110℃, holding for 50min-70min; heating at a rate of 1.5℃ / min-2℃ / min to 145℃-155℃, holding for 50min-70min; heating at a rate of 3℃ / min-3.5℃ / min to 245℃-255℃, holding for 50min-70min; heating at a rate of 3℃ / min-3.5℃ / min to 345℃-355℃, holding for 50min-70min; and finally heating at a rate of 2℃ / min-2.5℃ / min to 415℃-425℃.

[0025] In summary, this invention provides a method for preparing a polyamic acid solution with controllable viscosity. First, an acid anhydride is reacted with water to obtain a modified acid anhydride. Then, the modified acid anhydride is added to a reaction system of diamine and the acid anhydride to obtain a polyamic acid solution with controllable viscosity. The preparation method of this invention is simple, requires no complex organic compounds, uses simple reaction equipment, and allows for easy reaction conditions. The obtained polyimide film exhibits a stable glass transition temperature, effectively solving the problem of uncontrollable viscosity in the preparation of polyamic acid solutions in existing technologies, which leads to poor quality polyimide films. Attached Figure Description

[0026] Figure 1 The graph shows the glass transition temperature changes of polyimide films prepared using the viscosity-controllable polyamic acid solutions obtained in Examples 1-6. Detailed Implementation

[0027] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0028] Example 1

[0029] This embodiment provides a method for preparing a polyamic acid solution with controllable viscosity, specifically including the following steps:

[0030] Step 1: Under an inert atmosphere, weigh 40g of biphenyltetracarboxylic acid dianhydride into a 250mL round-bottom flask, pour 140g of pure water into the flask, stir at 90℃ for 150min, then filter the above solution with a funnel and neutral filter paper, dry the filter residue in an oven at 100℃ for 3h, grind it into powder to obtain modified acid anhydride;

[0031] Step 2: Under an inert atmosphere, add 5.95g of p-phenylenediamine to a flask containing 130g of N-methyl-2-pyrrolidone, stir at 100r / min at 0℃ until the p-phenylenediamine is completely dissolved, add 15.78g of biphenyltetracarboxylic acid dianhydride to the solution, and react at 10℃ for 3.5h to obtain a polyamic acid precursor solution;

[0032] Step 3: Mix 0.45g of the modified acid anhydride and the polyamic acid precursor solution evenly, and react at 70°C for 1.5h to obtain the polyamic acid solution.

[0033] Example 2

[0034] This embodiment provides a method for preparing a polyamic acid solution with controllable viscosity, specifically including the following steps:

[0035] Step 1: Under an inert atmosphere, weigh 40g of biphenyltetracarboxylic acid dianhydride into a 250mL round-bottom flask, pour 140g of pure water into the flask, stir at 90℃ for 150min, then filter the above solution with a funnel and neutral filter paper, dry the filter residue in an oven at 100℃ for 3h, grind it into powder to obtain modified acid anhydride;

[0036] Step 2: Under an inert atmosphere, 6.28 g of 1,4-cyclohexyldiamine was added to a flask containing 130 g of N,N-dimethylacetamide. The mixture was stirred at 100 r / min at 0 °C until the 1,4-cyclohexyldiamine was completely dissolved. 15.78 g of biphenyltetracarboxylic acid dianhydride was added to the solution, and the mixture was reacted at 10 °C for 3.5 h to obtain a polyamic acid precursor solution.

[0037] Step 3: Mix 0.48g of the modified acid anhydride and the polyamic acid precursor solution evenly, and react at 65°C for 1.5h to obtain the polyamic acid solution.

[0038] Example 3

[0039] This embodiment provides a method for preparing a polyamic acid solution with controllable viscosity, specifically including the following steps:

[0040] Step 1: Under an inert atmosphere, weigh 40g of cyclopentanetetracarboxylic acid dianhydride into a 250mL round-bottom flask, pour 140g of pure water into the flask, stir at 90℃ for 150min, then filter the above solution with a funnel and neutral filter paper, dry the filter residue in an oven at 100℃ for 3h, grind it into powder to obtain modified acid anhydride;

[0041] Step 2: Under an inert atmosphere, add 8.11g of p-phenylenediamine to a flask containing 130g of N,N-dimethylformamide, and stir at 100r / min at 0℃ until the p-phenylenediamine is completely dissolved. Add 15.37g of cyclopentanetetracarboxylic acid dianhydride to the solution and react at 10℃ for 3.5h to obtain a polyamic acid precursor solution.

[0042] Step 3: Mix 0.46g of the modified acid anhydride and the polyamic acid precursor solution evenly, and react at 65°C for 1.5h to obtain the polyamic acid solution.

[0043] Example 4

[0044] This embodiment provides a method for preparing a polyamic acid solution with controllable viscosity, specifically including the following steps:

[0045] Step 1: Under an inert atmosphere, weigh 40g of cyclopentanetetracarboxylic acid dianhydride into a 250mL round-bottom flask, pour 140g of pure water into the flask, stir at 90℃ for 150min, then filter the above solution with a funnel and neutral filter paper, dry the filter residue in an oven at 100℃ for 3h, grind it into powder to obtain modified acid anhydride;

[0046] Step 2: Under an inert atmosphere, 7.14 g of 1,4-cyclohexyldiamine was added to a flask containing 130 g of N-methyl-2-pyrrolidone. The mixture was stirred at 100 r / min at 0 °C until the 1,4-cyclohexyldiamine was completely dissolved. 15.35 g of cyclopentanetetracarboxylic acid dianhydride was added to the solution, and the mixture was reacted at 10 °C for 3.5 h to obtain a polyamic acid precursor solution.

[0047] Step 3: Mix 0.48g of the modified acid anhydride and the polyamic acid precursor solution evenly, and react at 65°C for 1.5h to obtain the polyamic acid solution.

[0048] Example 5

[0049] This embodiment provides a method for preparing a polyamic acid solution with controllable viscosity, specifically including the following steps:

[0050] Step 1: Under an inert atmosphere, weigh 40g of dicyclohexyltetracarboxylic acid dianhydride into a 250mL round-bottom flask, pour 140g of pure water into the flask, stir at 90℃ for 150min, then filter the above solution with a funnel and neutral filter paper, dry the filter residue in an oven at 100℃ for 3h, grind it into powder to obtain modified acid anhydride;

[0051] Step 2: Under an inert atmosphere, add 5.68 g of p-phenylenediamine to a flask containing 140 g of N,N-dimethylformamide, and stir at 100 r / min at 0 °C until the p-phenylenediamine is completely dissolved. Add 15.64 g of dicyclohexyltetracarboxylic acid dianhydride to the solution and react at 10 °C for 3.5 h to obtain a polyamic acid precursor solution.

[0052] Step 3: Mix 0.45g of the modified acid anhydride and the polyamic acid precursor solution evenly, and react at 65°C for 1.5h to obtain the polyamic acid solution.

[0053] Example 6

[0054] This embodiment provides a method for preparing a polyamic acid solution with controllable viscosity, specifically including the following steps:

[0055] Step 1: Under an inert atmosphere, weigh 40g of dicyclohexyltetracarboxylic acid dianhydride into a 250mL round-bottom flask, pour 140g of pure water into the flask, stir at 90℃ for 150min, then filter the above solution with a funnel and neutral filter paper, dry the filter residue in an oven at 100℃ for 3h, grind it into powder to obtain modified acid anhydride;

[0056] Step 2: Under an inert atmosphere, 6.00 g of 1,4-cyclohexyldiamine was added to a flask containing 120 g of N-methyl-2-pyrrolidone. The mixture was stirred at 100 r / min at 0 °C until the 1,4-cyclohexyldiamine was completely dissolved. 15.66 g of dicyclohexyltetracarboxylic acid dianhydride was added to the solution, and the mixture was reacted at 10 °C for 3.5 h to obtain a polyamic acid precursor solution.

[0057] Step 3: Mix 0.47g of the modified acid anhydride and the polyamic acid precursor solution evenly, and react at 65°C for 1.5h to obtain the polyamic acid solution.

[0058] Application examples

[0059] This embodiment provides a polyimide film prepared using the viscosity-controllable polyamic acid solution obtained in Examples 1-6, specifically including the following steps:

[0060] The obtained polyamic acid solution with controllable viscosity was uniformly coated onto a clean and dry glass substrate with a coating thickness of 0.5 mm to 1 mm. After coating, it was transferred to a muffle furnace continuously purged with nitrogen and a programmed heating process was set: the temperature was increased to 100 °C at a heating rate of 2.5 °C / min and held for 60 min, then increased to 150 °C at a heating rate of 1.7 °C / min and held for 55 min, then increased to 250 °C at a heating rate of 3.3 °C / min and held for 60 min, then increased to 350 °C at a heating rate of 3 °C / min and held for 60 min, and finally increased to 420 °C at a heating rate of 2.5 °C / min and held for 10 min. After cooling to room temperature, the glass plate was immersed in deionized water to peel off the polyimide film on it and dried to obtain the polyimide film.

[0061] Comparative Example 1

[0062] This comparative example provides a method for preparing a polyamic acid solution, which differs from Example 1 in that the modified acid anhydride is replaced with an unmodified acid anhydride. The specific steps are as follows:

[0063] Step 1: Under an inert atmosphere, add 5.95g of p-phenylenediamine to a flask containing 130g of N-methyl-2-pyrrolidone, stir at 100r / min at 0℃ until the p-phenylenediamine is completely dissolved, add 15.78g of biphenyltetracarboxylic acid dianhydride to the solution, and react at 10℃ for 3.5h to obtain a polyamic acid precursor solution;

[0064] Step 2: Mix 0.40g of biphenyltetracarboxylic acid dianhydride and the polyamic acid precursor solution evenly, and react at 70°C for 1.5h to obtain the polyamic acid solution.

[0065] Comparative Example 2

[0066] This comparative example provides a method for preparing a polyamic acid solution, which differs from Example 1 in that the modified acid anhydride is replaced with biphenyl tetracarboxylic acid. The specific steps are as follows:

[0067] Step 1: Under an inert atmosphere, add 5.95g of p-phenylenediamine to a flask containing 130g of N-methyl-2-pyrrolidone, stir at 100r / min at 0℃ until the p-phenylenediamine is completely dissolved, add 15.78g of biphenyltetracarboxylic acid dianhydride to the solution, and react at 10℃ for 3.5h to obtain a polyamic acid precursor solution;

[0068] Step 2: Mix 0.45g of biphenyltetracarboxylic acid and the polyamic acid precursor solution evenly, and react at 70°C for 1.5h. The biphenyltetracarboxylic acid cannot be dissolved, and the reaction fails.

[0069] Comparative Example 3

[0070] This comparative example provides a method for preparing a polyamic acid solution, which differs from Example 1 in that the acid anhydride in step one is dissolved in anhydrous ethanol. The specific steps are as follows:

[0071] Under an inert atmosphere, 40g of biphenyltetracarboxylic acid dianhydride was weighed and placed in a 250mL round-bottom flask. 140g of anhydrous ethanol was poured into the flask and stirred at 90℃ for 150min. During the stirring process, the solution turned black, and the reaction failed.

[0072] To further demonstrate the technical effects of the present invention, the viscosity of the polyamic acid solutions with controllable viscosity obtained in Examples 1-6 and Comparative Example 1 was tested. The viscosity values ​​were measured using a rotational viscometer (TV-22E-type manufactured by TokiSangyo Co., Ltd.) at a shear rate of 20 sec-1 at 2525°C. The results are shown in Table 1.

[0073] Table 1 Viscosity test results

[0074] project Viscosity (cp) Example 1 5211 Example 2 5212 Example 3 5223 Example 4 5215 Example 5 5209 Example 6 5211 Comparative Example 1 16142

[0075] As can be seen from Table 1, the viscosity of the polyamic acid solution obtained in Examples 1-6 of the present invention is basically stable at around 5200, while the viscosity of the polyamic acid solution obtained in Comparative Example 1 is as high as 16142. It can be seen that modified acid anhydride is crucial for obtaining polyamic acid solution with controllable viscosity.

[0076] This invention also conducted application tests on the viscosity-controllable polyamic acid solutions obtained in Examples 1-6. Following the preparation methods of the application examples, the obtained polyamic acid solutions were used to prepare polyimide films. The glass transition temperature of the polyimide films obtained in each example was determined using a NETZSCH DMA 242E dynamic thermomechanical analyzer at a heating rate of 5°C / min in air. The test frequency was 1.0 Hz, the sample strip width was 4 mm, and the peak value of the loss tangent tanδ curve was taken as the glass transition temperature of the polyimide film. The results are shown in Table 2 and... Figure 1 As shown.

[0077] Table 2. Test results of glass transition temperature of polyimide films.

[0078]

[0079]

[0080] According to Table 2 and Figure 1 It can be seen that the glass transition temperature of the polyimide film prepared using the polyamic acid solution with controllable viscosity obtained in Examples 1-6 is basically stable between 400℃ and 410℃, which further improves the hardness and mechanical properties of the polyimide film.

[0081] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions or improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a polyamic acid solution with controllable viscosity, characterized in that: Includes the following steps: Step 1: Disperse the acid anhydride in water under an inert atmosphere, react at 90°C for 2.5 h, filter, dry, and grind to obtain the modified acid anhydride; the mass ratio of the acid anhydride to water is 1-3:7-10. Step 2: Under an inert atmosphere, dissolve the diamine in an aprotic polar solvent, add acid anhydride, and react at 10°C for 3.5 h to obtain a polyamic acid precursor solution. The diamine is either p-phenylenediamine or 1,4-cyclohexyldiamine; Step 3: Mix the modified acid anhydride and the polyamic acid precursor solution evenly, and react at 65℃-70℃ for 1.5h to obtain the polyamic acid solution; In step two, the ratio of the total amount of the acid anhydride and the modified acid anhydride to the amount of the diamine is 1:0.95-1.

05. In steps one and two, the anhydride is any one of biphenyltetracarboxylic dianhydride, cyclopentanetetracarboxylic dianhydride, or dicyclohexyltetracarboxylic dianhydride.

2. The method for preparing a viscosity-controllable polyamic acid solution as described in claim 1, characterized in that: In step two, the aprotic polar solvent is any one or more of N,N-dimethylacetamide, N,N-dimethylformamide, or N-methylpyrrolidone.

3. The method for preparing a viscosity-controllable polyamic acid solution as described in claim 1, characterized in that: In step two, the mass ratio of the diamine to the aprotic polar solvent is 5-8:120-140.

Citation Information

Patent Citations

  • Preparation method for polyamide acid solution

    CN105622936A