Random copolymerized polypropylene pipe and its preparation method and application

By adding homopolymer polypropylene and block copolymer polypropylene to random copolymer polypropylene pipes and using a β-nucleating agent to control the crystallization process, β-type hybrid tandem crystals are formed, solving the problem of the difficulty in balancing toughness and strength of random copolymer polypropylene pipes at low temperatures, and achieving the effect of strengthening and toughening the pipes.

CN117866337BActive Publication Date: 2026-11-24PETROCHINA CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311612927.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2026-11-24
Estimated Expiration
2043-11-29

AI Technical Summary

Technical Problem

Existing random copolymer polypropylene pipes cannot achieve both toughness and strength at low temperatures. Traditional toughening methods suffer from the problem of uneven dispersion of reinforcing fillers and the competing effect of β-nucleating agents.

Method used

By adding homopolymer polypropylene and block copolymer polypropylene to random copolymer polypropylene pipes and using a β nucleating agent to control the melting and cooling process, a large number of β-type hybrid tandem crystals are formed, which improves the strength and low-temperature toughness of the pipes.

Benefits of technology

This study achieved an improvement in the strength and toughness of random copolymer polypropylene pipes at low temperatures, forming a large number of β-type hybrid tandem crystals, which enhanced the overall performance of the pipes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117866337B_ABST
    Figure CN117866337B_ABST
Patent Text Reader

Abstract

This invention provides a random copolymer polypropylene pipe, its preparation method, and its application, comprising the following components: 78-98.99 parts by weight of random copolymer polypropylene; 1-20 parts by weight of homopolymer polypropylene and / or block copolymer polypropylene; and 0.01-2 parts by weight of β-nucleating agent. The preparation method includes the following steps: Step 1, mixing the random copolymer polypropylene, homopolymer polypropylene and / or block copolymer polypropylene, and β-nucleating agent, melting, and extruding; the melting temperature is 230-250℃, and the extrusion temperature is 170-200℃; Step 2, cooling the molten preform extruded in Step 1 to 120-138℃ within 2-10 seconds, and then cooling and shaping to obtain the random copolymer polypropylene pipe. The pipe of the present invention comprises homopolymer polypropylene or block copolymer polypropylene. The crystal nuclei generated by homopolymer polypropylene and block copolymer polypropylene induce the epigenetic crystallization of random copolymer polypropylene, thereby forming a large number of β-type hybrid tandem crystals inside the random copolymer polypropylene pipe. This improves the low-temperature toughness while ensuring the improvement of the pipe strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of pipes, specifically to a random copolymer polypropylene pipe, its preparation method, and its application. Background Technology

[0002] Random copolymer polypropylene (PPR) is a high-quality plastic obtained by random copolymerization of propylene and an appropriate amount of olefin monomers, widely used for hot and cold water transmission. The introduction of olefin monomers into the molecular backbone increases the flexibility of the molecular chain, thus giving PPR superior toughness and resistance to environmental stress cracking compared to homopolymer polypropylene; however, its low-temperature toughness still needs improvement. In cold northern regions during winter, PPR pipes often crack during construction. Furthermore, due to the introduction of conventional olefin monomers such as ethylene, the regularity of the PPR molecular chain is lower, resulting in lower strength and rigidity compared to homopolymer polypropylene. Therefore, achieving the fabrication of random copolymer polypropylene pipes that combine both strength and rigidity is of great significance.

[0003] Currently, the main methods for preparing high-performance random copolymer polypropylene pipes include: 1. Adding a rubber phase to the PPR matrix to achieve toughening. Wang et al. used polyolefin elastomer (POE) to toughen PPR, increasing its impact toughness to 3.6 kJ / m. 2 (Wang X, Hu S, Guo Y, Li G, Xu R. Polymers 2019; 11:1976.). However, rubber hardens at low temperatures and cannot exert its toughening effect. The improvement in PPR toughness is limited and it will cause a decrease in PPR strength. There are also methods that introduce reinforcing fillers and elastomers to synergistically toughen PPR. Guan Peng used nano-attapulgite and polyolefin elastomer (POE) to synergistically modify PPR, which refined its α crystal form and was beneficial to improving the toughness of the material (Guan Peng, Wang Jingjing, Yang Yingchao, Engineering Plastics Application, 2020, 48(3):5.). However, this method has problems such as the difficulty of uniformly dispersing inorganic particles in polymers and the competition between the α nucleation effect of inorganic particles and the β nucleation effect of β nucleating agents. II. Introducing β nucleating agents to regulate the crystal structure inside PPR pipes, promote the growth of β crystals, and improve its impact toughness. However, PPR chains have poor regularity and weak crystallization ability. Even under the action of β nucleating agents, it cannot effectively promote the formation of β crystals. For example, Yang et al. studied the effect of β nucleating agent content on the crystallization properties of PPR. The results showed that under the condition that the maximum β nucleating agent content was 0.4%, only 15.6% of β crystals were formed (Yang X, Chang J, Fang W, Yu Z, Li M, Li Q. PolymerComposites. 2021; 42:3169-3183.).

[0004] CN102146183A discloses a β-crystalline polypropylene nucleating agent, its preparation method, and a special material for β-crystalline polypropylene pipes manufactured therefrom. The dispersion of the β-nucleating agent in polypropylene is solved by surface modification. This technology has a good effect on isotactic polypropylene, but the effect on random copolymer polypropylene (PPR) with poor crystallinity needs to be improved.

[0005] Therefore, there is an urgent need for a simpler and more effective method that can simultaneously improve the strength and low-temperature toughness of PPR pipes. Summary of the Invention

[0006] The main objective of this invention is to provide a random copolymer polypropylene pipe, its preparation method, and its application, so as to overcome the problem that random copolymer polypropylene pipes in the prior art cannot simultaneously achieve both strength and low-temperature toughness.

[0007] To achieve the above objectives, the present invention provides a random copolymer polypropylene pipe, comprising the following components:

[0008] Random copolymer polypropylene 78–98.99 parts by weight;

[0009] 1 to 20 parts by weight of homopolymer polypropylene and / or block copolymer polypropylene;

[0010] 0.01 to 2 parts by weight of β nucleating agent.

[0011] The random copolymer polypropylene pipe of the present invention has a melting temperature of not more than 150°C; the homopolymer polypropylene and block copolymer polypropylene have melting temperatures of 138-170°C.

[0012] The random copolymer polypropylene pipe of the present invention has a crystallization temperature of 170-200°C for the β nucleating agent.

[0013] The random copolymer polypropylene pipe of the present invention comprises 8 to 12 parts by weight of homopolymer polypropylene and / or block copolymer polypropylene, 0.05 to 0.1 parts by weight of β nucleating agent, and 87.9 to 91.95 parts by weight of random copolymer polypropylene.

[0014] To achieve the above objectives, the present invention also provides a method for preparing the above-mentioned random copolymer polypropylene pipe, comprising the following steps:

[0015] Step 1: Mix random copolymer polypropylene, homopolymer polypropylene and / or block copolymer polypropylene, and β nucleating agent, melt and extrude, with a melt temperature of 230-250℃ and an extrusion temperature of 170-200℃.

[0016] Step 2: Cool the molten tube preform extruded in Step 1 to 120-138°C within 2-10 seconds, and then cool and shape it to obtain random copolymer polypropylene tube.

[0017] The method for preparing random copolymer polypropylene pipes according to the present invention, wherein the wall thickness of the molten pipe preform is 1-50 mm and the diameter-to-thickness ratio is not less than 5.

[0018] The method for preparing random copolymer polypropylene pipes according to the present invention includes melting and extrusion in a screw extruder, the screw extruder comprising a melting section and a die section, the length of the die section being 10-20 cm and the screw speed being 5-100 rpm.

[0019] The method for preparing random copolymer polypropylene pipes according to the present invention includes the cooling of the molten pipe preform in an air ring cooling device, wherein the air ring cooling device provides an air cooling field with a length of 5 to 20 cm in the extrusion direction of the molten pipe preform, the wind speed in the air cooling field is 0.5 to 10 m / s, and the outlet air temperature is 0 to 25°C.

[0020] The method for preparing random copolymer polypropylene pipes according to the present invention includes a cooling and shaping process performed in a vacuum sizing and cooling device.

[0021] To achieve the above objectives, the present invention further provides applications of the above-mentioned random copolymer polypropylene pipes in urban water supply and drainage, gas transmission, power and optical cable sheathing, industrial fluid transmission, and agricultural irrigation.

[0022] The beneficial effects of this invention are:

[0023] (1) The pipe of the present invention includes homopolymer polypropylene or block copolymer polypropylene. The crystal nuclei generated by homopolymer polypropylene and block copolymer polypropylene induce the epigenetic crystallization of random copolymer polypropylene, thereby forming a large number of β-type hybrid tandem crystals inside the random copolymer polypropylene pipe, which improves the low temperature toughness while ensuring the improvement of the pipe strength.

[0024] (2) The present invention cools the molten material of the pipe in stages, so that the β nucleating agent, homopolymer polypropylene, block copolymer polypropylene and random copolymer polypropylene crystallize in sequence, thereby further increasing the amount of β-type hybrid crystals generated inside the random copolymer polypropylene pipe, and further improving the strength and low temperature impact toughness of the random copolymer polypropylene pipe. Attached Figure Description

[0025] Figure 1 The image shows the DSC non-isothermal crystallization curves of homopolymer polypropylene containing β-nucleating agent and random copolymer polypropylene containing β-nucleating agent.

[0026] Figure 2 Polarized photographs of the random copolymer polypropylene pipe (left) prepared for Comparative Example 2 and the random copolymer polypropylene pipe (right) prepared for Example 2 of the present invention.

[0027] Figure 3 This is a schematic diagram of the process flow for the preparation method of random copolymer polypropylene pipes according to the present invention.

[0028] Figure 4 This is a bar chart comparing the tensile strength and impact toughness of the pipe samples prepared in Comparative Example 1 and Examples 1-4 of this invention. Detailed Implementation

[0029] The technical solution of the present invention will be described in detail below. The following embodiments are implemented under the premise of the technical solution of the present invention and a detailed implementation process is given. However, the protection scope of the present invention is not limited to the following embodiments. Structures or experimental methods that do not specify specific conditions in the following embodiments are generally performed under conventional conditions.

[0030] This invention provides a random copolymer polypropylene pipe, comprising the following components:

[0031] Random copolymer polypropylene 78–98.99 parts by weight;

[0032] 1 to 20 parts by weight of homopolymer polypropylene and / or block copolymer polypropylene;

[0033] 0.01 to 2 parts by weight of β nucleating agent.

[0034] In one embodiment, the random copolymer polypropylene, homopolymer polypropylene, block copolymer polypropylene, and β-nucleating agent of the present invention comprise a total of 100 parts by weight.

[0035] The pipe of this invention induces the epigenetic crystallization of random copolymer polypropylene by crystal nuclei generated from homopolymer polypropylene and block copolymer polypropylene, thereby forming a large number of β-type hybrid tandem crystals inside the random copolymer polypropylene pipe, thus improving the strength and low-temperature toughness of the pipe.

[0036] Random copolymer polypropylene is a raw material commonly used in the field of pipe manufacturing. Preferably, it is random copolymer polypropylene with a melting temperature window not exceeding 150°C. It can be commercially available or prepared using existing technology, as long as it meets the above specifications. To better illustrate the invention, a reference embodiment is provided. The random copolymer polypropylene includes, but is not limited to, the following types: PA14D (Daqing Petrochemical), PA14D-2 (Daqing Petrochemical), T4401 (Dushanzi Petrochemical), R4220 (Yanshan Petrochemical), M250E (Shanghai Jinshan), R200P (Hyosung, South Korea), R701 (Hyosung, South Korea), R370Y (SK, South Korea), and R520Y (SK, South Korea).

[0037] Homopolymer polypropylene and block copolymer polypropylene are homopolymer or block copolymer polypropylene with a melting temperature window of 138-170℃, and are sourced from commercially available products or prepared according to existing technologies to meet the above specifications. To better illustrate the invention, a reference embodiment is provided, wherein the homopolymer polypropylene includes, but is not limited to, T30S (Dushanzi Petrochemical), F401 (Yangzi Petrochemical), T300 (Shanghai Jinshan), S1003 (Yanshan Petrochemical), Y600 (Shanghai Petrochemical), and H7300F (Korea SK), and the block copolymer polypropylene includes, but is not limited to, B8101 (Yanshan Petrochemical), PPB4228 (Daqing Refining & Chemical), DY-ZK0640P (Dushanzi Petrochemical), PB240P (Korea Hyosung), and B8001 (Taiwan Petrochemical).

[0038] β-nucleating agents are functional additives used in polypropylene to induce crystallization in molten homopolymer and block copolymer polypropylene. Preferably, they are β-nucleating agents with a crystallization temperature window of 170–200°C, sourced from commercially available sources or those conforming to the above-mentioned applicable range as described in existing literature. To better illustrate the present invention, a reference technical solution is provided. β-nucleating agents include, but are not limited to, inorganic nucleating agents such as calcium carbonate and nano-zinc oxide; fused-ring compound nucleating agents such as 2-mercaptobenzimidazole (MBIM); amide compound nucleating agents such as TMB series compounds and N,N'-dicyclohexylterephthalamide (DCHT); dicarboxylate nucleating agents such as zinc adipic acid; rare earth nucleating agents such as WBG series compounds; and polymer nucleating agents such as main-chain liquid crystal polyester (PBDPS).

[0039] In the pipe of this invention, when the amounts of homopolymer polypropylene and block copolymer polypropylene are within a certain range, the amount of β-crystals formed by random copolymer polypropylene increases with the increase of the amounts of homopolymer polypropylene and block copolymer polypropylene, thus enhancing the low-temperature toughness and rigidity of the pipe. Beyond this range, further increases in the amounts of homopolymer polypropylene and block copolymer polypropylene lead to saturation of their induced epigenetic crystallization effect on random copolymer polypropylene, and the amount of β-crystals formed by random copolymer polypropylene no longer increases significantly. Conversely, the brittleness of homopolymer polypropylene and block copolymer polypropylene reduces the impact toughness of the pipe, resulting in a decrease in the low-temperature toughness and rigidity of the pipe. Therefore, when the random copolymer polypropylene is 78–98.99 parts by mass and the homopolymer polypropylene and / or block copolymer polypropylene is 1–20 parts by mass, the random copolymer polypropylene pipe of this invention can balance low-temperature toughness and rigidity.

[0040] In one embodiment, the random copolymer polypropylene pipe of the present invention comprises the following components:

[0041] Random copolymer polypropylene 87.9–91.95 parts by weight;

[0042] 8-12 parts by weight of homopolymer polypropylene and / or block copolymer polypropylene;

[0043] 0.05 to 0.1 parts by weight of β nucleating agent.

[0044] Thus, the random copolymer polypropylene pipe of the present invention will have better low-temperature toughness and rigidity.

[0045] In one embodiment, the random copolymer polypropylene pipe of the present invention is composed of random copolymer polypropylene, homopolymer polypropylene and / or block copolymer polypropylene, and a β-nucleating agent. In another embodiment, in addition to random copolymer polypropylene, homopolymer polypropylene and / or block copolymer polypropylene, and a β-nucleating agent, the random copolymer polypropylene pipe of the present invention also includes other components, such as antioxidants, stabilizers, compatibilizers, and other known functional additives and processing aids, as well as other known fillers that contribute to further enhancing the performance of the pipe. Preferably, the random copolymer polypropylene pipe of the present invention is composed of random copolymer polypropylene, homopolymer polypropylene and / or block copolymer polypropylene, and a β-nucleating agent.

[0046] In one embodiment, the present invention cools the molten state of the random copolymer polypropylene pipe components in stages to allow the homopolymer polypropylene and / or block copolymer polypropylene to crystallize first, and then induce the random copolymer polypropylene to form epigenetic crystals, thereby further increasing the amount of β-type hybrid tandem crystals generated inside the random copolymer polypropylene pipe, and further improving the pipe strength and low-temperature toughness.

[0047] The present invention also provides a method for preparing the above-mentioned random copolymer polypropylene pipe, comprising the following steps:

[0048] Step 1: Mix random copolymer polypropylene, homopolymer polypropylene and / or block copolymer polypropylene, and β nucleating agent, melt and extrude, with a melt temperature of 230-250℃ and an extrusion temperature of 170-200℃.

[0049] Step 2: Cool the molten tube preform extruded in Step 1 to 120-138°C within 2-10 seconds, and then cool and shape it to obtain random copolymer polypropylene tube.

[0050] This invention involves stepwise cooling of the molten material in the pipe, causing the β-nucleating agent, homopolymer polypropylene, block copolymer polypropylene, and random copolymer polypropylene to crystallize sequentially. This further increases the amount of β-type hybrid crystals generated inside the random copolymer polypropylene pipe, thereby improving the strength and low-temperature impact toughness of the random copolymer polypropylene pipe.

[0051] Figure 1 This is a DSC non-isothermal crystallization curve of homopolymer polypropylene containing a β-nucleating agent and random copolymer polypropylene containing a β-nucleating agent. Figure 1As shown, there is a gap between the crystallization temperature of homopolymer polypropylene containing β nucleating agent and the crystallization temperature of random copolymer polypropylene containing β nucleating agent, thus providing a theoretical basis for the stepwise crystallization of the present invention.

[0052] Figure 3 This is a schematic diagram of the process flow for the preparation method of random copolymer polypropylene pipes according to the present invention. It should be noted that the process flow shown in the diagram is for illustrative purposes only; in actual operation, it can be a continuous process. For example, the distance between the air ring cooling device and the die and vacuum cooling sizing box should only retain the reasonable distance between industrial continuous equipment.

[0053] In one embodiment, the melting and extrusion of the present invention are carried out in a screw extruder, which includes a melting section and a die section. The temperature of the melting section is 230-250°C (i.e., melting temperature), the temperature of the die section is 170-200°C (i.e., extrusion temperature), the length of the die section is 10-20 cm, and the screw speed is 5-100 rpm.

[0054] In detail, this invention involves adding a mixture of random copolymer polypropylene, block copolymer polypropylene, homopolymer polypropylene, and a β-nucleating agent into a screw extruder for extrusion. The extrusion is performed under the following conditions: a melt section temperature of 230–250°C and a die section temperature of 170–200°C. The screw speed is 5–100 rpm, and a molten preform is obtained through extrusion through the die section. In one embodiment, the melt section temperature of 230–250°C in this invention is achieved through the heating function of the screw extruder itself or through a screw extruder heating kit known in the art. The melt section temperature can be adjusted according to the specific melting parameters of the selected homopolymer polypropylene and block copolymer polypropylene, or it can be any value within this temperature range, such as 231°C, 235°C, 240°C, 245°C, 249°C, or any range or point value between them. In one embodiment, the die section temperature of 170–200°C in the method of the present invention is achieved through the heating function of the screw extruder itself or through a screw extruder heating kit known in the art. The selection of the die section temperature can be adjusted according to the melt parameters of the selected homopolymer polypropylene or block copolymer polypropylene, or it can be any value within this temperature range, such as 171°C, 175°C, 180°C, 185°C, 190°C, 195°C, 199°C, or any range or point value between them. In one embodiment, the screw speed in the method is 5–100 rpm, which can be adjusted according to the conventional operating parameters or process habits of the selected screw extruder, or it can be any value within this screw speed range, such as 6 rpm, 10 rpm, 20 rpm, 30 rpm, 40 rpm, 50 rpm, 60 rpm, 70 rpm, 80 rpm, 90 rpm, 99 rpm, or any range or point value between them. It should be noted that the melting section temperature and the die section temperature mentioned in the method of the present invention are set temperatures rather than real-time temperatures. Preferably, the length of the die section is 10-20 cm to improve the cooling gradient.

[0055] In one embodiment, a molten tube blank is obtained by extrusion through a die segment. Preferably, the molten tube blank obtained by extrusion through a die segment has a wall thickness of 1 to 50 mm and a diameter-to-thickness ratio of not less than 5. This preference is made considering the influence of the tube blank wall thickness on the internal cooling delay of the tube wall during subsequent step-by-step controlled cooling of the tube blank. For example, the wall thickness is 2 mm, 5 mm, 10 mm, 20 mm, 30 mm, 40 mm, 45 mm, 49 mm, or any range or point value between them. Those skilled in the art will recognize that if the prior art can cool the tube blank to 120 to 138°C within 2 to 10 seconds when the wall thickness is higher than 50 mm, the tube blank wall thickness can also be selected to be higher than 50 mm; the diameter-to-thickness ratio can also be selected in the same way.

[0056] This invention involves uniformly mixing the main raw material components, including random copolymer polypropylene, block copolymer polypropylene, homopolymer polypropylene, and a β-nucleating agent, in the high-temperature melting section of a screw extruder. The random copolymer polypropylene serves as the matrix, while the homopolymer polypropylene, block copolymer polypropylene, and β-nucleating agent are uniformly distributed as dispersed phases within the matrix. When the composite melt reaches the slightly lower temperature die section, the molten β-nucleating agent recrystallizes to form a fibrous structure. At this point, the random copolymer polypropylene, homopolymer polypropylene, and block copolymer polypropylene are in a molten state.

[0057] After extrusion through a die to obtain a molten tube preform, it is immediately cooled to 120–138°C within 2–10 seconds. Because the melting temperatures of homopolymer and block copolymer polypropylene are higher than those of random copolymer polypropylene, their crystallization temperatures are also higher. Under the action of the β-nucleating agent, they first form β-crystals in a regular arrangement. Therefore, within the molten tube preform, homopolymer and block copolymer polypropylene undergo epigenetic crystallization under the induction of the fibrous β-nucleating agent, forming highly oriented β-crystals. At this time, the random copolymer polypropylene remains in a molten state.

[0058] In one embodiment, the molten preform is immediately cooled to 120-138°C within 2-10 seconds after extrusion through the die section. This immediate cooling to 120-138°C is achieved through continuous process operation to ensure that the molten preform is cooled immediately after extrusion through the die section. The target cooling temperature can be adjusted according to the specific random copolymer polypropylene melting parameters selected, or it can be any value within this temperature range, such as 121°C, 125°C, 130°C, 135°C, 137°C, or any range or point value between them. The cooling time can be adjusted according to the specific molten preform wall thickness parameters to be cooled, or it can be any value within this cooling time range, such as 3s, 4s, 5s, 6s, 7s, 8s, 9s, or any range or point value between them. It should be noted that the cooling to 120-138°C mentioned in the method refers to the temperature that the molten tube blank needs to reach after cooling. This temperature range can be the temperature measured on the outer wall of the molten tube blank within 2-10 seconds of cooling, or the average temperature measured on the outer wall of the molten tube blank within a continuous length within 2-10 seconds of cooling.

[0059] The molten tubular preform is immediately cooled to 120-138°C within 2-10 seconds after extrusion through the die. The cooling technique, designed to avoid affecting the component composition and subsequent preform shaping, includes, but is not limited to, air cooling and refrigerant cooling. Refrigerant cooling can utilize liquid or gaseous refrigerants. Preferably, air cooling, such as a ring-type cooling device, is used. To better illustrate the invention, a reference embodiment is provided where the molten tubular preform is immediately cooled to 120-138°C within 2-10 seconds by a ring-type cooling device after extrusion through the die. This ring-type cooling device provides a cooling field covering a length of 5-20 cm along the extrusion direction of the molten tubular preform, and the preform is pulled through this cooling field at a rate of 2-100 cm / min by a traction machine to achieve cooling to 120-138°C. More preferably, the air velocity of the ring-type cooling device is set to 0.5-10 m / s, and the outlet air temperature is 0-25°C.

[0060] In one embodiment, the air ring cooling device provides an air cooling field covering a length of 5-20 cm in the extrusion direction of the molten tube preform. The air ring cooling device has a circular structure and includes multiple air nozzles, which together form the air cooling field. The outlet air temperature is 0-25°C. This device can be a conventionally used cooling device in industrial applications, such as the cooling device provided in Chinese Utility Model Patent "A Cooling Device for Polypropylene Pipes" (Application No. 202022427349.7) (but excluding the inclusion of conveyor rollers), or it can be a self-made device based on the principle of air cooling field. However, it should be noted that the above description of the air ring cooling device does not imply limitation of the present invention. Based on the inventive principle of the present invention, any cooling device that can provide an air cooling field of 5-20 cm in length and is suitable for pipe preparation, provided that it can achieve the goal of cooling to 120-138°C within 2-10 seconds, can be applied to the present invention.

[0061] Then, cooling and shaping are performed to obtain random copolymer polypropylene pipes. In one embodiment, cooling and shaping are achieved using a vacuum sizing and cooling device. The vacuum sizing and cooling device is a conventional piece of equipment used in pipe manufacturing, for shaping the pipe during the manufacturing process. Its specific selection and process parameters can refer to existing technologies in the field, or the matching vacuum sizing and cooling device and process parameter settings can be directly used when implementing this invention on a pipe manufacturing production line.

[0062] The β crystals that form on the fibrous β nucleating agent in homopolymer polypropylene and block copolymer polypropylene further induce and promote the crystallization of random copolymer polypropylene, forming a large number of highly oriented β-type hybrid tandem crystals. This significantly increases the β crystal content in random copolymer polypropylene, making the random copolymer polypropylene pipe stronger and tougher.

[0063] In one embodiment, the method for preparing the random copolymer polypropylene pipe of the present invention is a continuous production process.

[0064] This invention is based on the temperature differences in crystallization of homopolymer polypropylene, block copolymer polypropylene, and random copolymer polypropylene under the induction of a β-nucleating agent. By controlling the cooling process of the pipe blank in stages, the crystallization sequence of the β-nucleating agent, homopolymer polypropylene, block copolymer polypropylene, and random copolymer polypropylene is controlled. Specifically, the β-nucleating agent recrystallizes first in the die section at a slightly lower temperature, forming a fibrous structure. Then, immediately after extrusion through the die section, it is cooled to 120-138°C within 2-10 seconds. Utilizing the heterogeneous nucleation induction effect of the β-nucleating agent on the β-crystal form, the homopolymer polypropylene or block copolymer polypropylene is guided to form fibrous β-crystals. Finally, through a vacuum sizing and cooling device, the epigenetic crystallization of homopolymer polypropylene and block copolymer polypropylene on the β-nucleating agent promotes further crystallization of random copolymer polypropylene, ultimately forming a large number of β-type hybrid crystals. This achieves simultaneous reinforcement and toughening of the pipe.

[0065] In this invention, homopolymer polypropylene or block copolymer polypropylene has a similar molecular chain structure to random copolymer polypropylene, exhibiting good compatibility and avoiding the problem of traditional additives being difficult to disperse uniformly within the polymer matrix, thus effectively preventing a decrease in pipe strength. Furthermore, the preparation method provided by this invention can be implemented by modifying existing polypropylene pipe manufacturing production lines, resulting in a simple manufacturing process and excellent prospects for industrial application.

[0066] The random copolymer polypropylene pipe of this invention can be used for urban water supply and drainage, gas transmission, power and optical cable sheathing, industrial fluid transmission, agricultural irrigation, etc., and has high application value.

[0067] The following detailed description of the embodiments of this application is provided in conjunction with examples. However, those skilled in the art will understand that the following examples are for illustrative purposes only and should not be construed as limiting the scope of this application. Where specific conditions are not specified in the examples, conventional conditions or conditions recommended by the manufacturer shall apply. Where the manufacturers of reagents or instruments are not specified, they are all commercially available conventional products. This application should not be construed as being limited to the specific embodiments described.

[0068] Evaluation and analysis methods: The tensile strength of the pipe was determined according to the test standard GB / T 8804-2003 using an RGL-10 mechanical property tester manufactured by Shenzhen Ruigeer Co., Ltd. The impact toughness of the pipe at 0℃ was determined according to the test standard GB / T 14153-93 using a drop hammer impact tester manufactured by Chengde Precision Instruments Co., Ltd.

[0069] Unless otherwise specified below, "parts" in the examples and comparative examples refer to parts by mass.

[0070] Example 1

[0071] Step 1: Mix 94.9 parts of random copolymer polypropylene (PA14D), 5 parts of homopolymer polypropylene (T30S), and 0.1 parts of β-nucleating agent (DCHT), and melt and extrude them in a screw extruder. The melt temperature is 230-250℃, the extrusion temperature is 170-200℃, the length of the die section is 20cm, and the screw speed is 50rpm.

[0072] Step 2: The molten tube preform extruded in Step 1 is cooled to 125°C within 2-10 seconds in an air cooling device. The length of the air cooling field is 8cm, the wind speed in the air cooling field is 5m / s, and the outlet air temperature is 10°C. Then, it is cooled and shaped to obtain a random copolymer polypropylene tube with a wall thickness of 20mm and an outer diameter of 200mm.

[0073] Example 2

[0074] Step 1: Mix 89.9 parts of random copolymer polypropylene (PA14D), 10 parts of homopolymer polypropylene (T30S), and 0.1 parts of β-nucleating agent (DCHT), and melt and extrude them in a screw extruder. The melt temperature is 230-250℃, the extrusion temperature is 170-200℃, the length of the die section is 20cm, and the screw speed is 50rpm.

[0075] Step 2: The molten tube preform extruded in Step 1 is cooled to 125°C within 2-10 seconds in an air cooling device. The length of the air cooling field is 8cm, the wind speed in the air cooling field is 5m / s, and the outlet air temperature is 10°C. Then, it is cooled and shaped to obtain a random copolymer polypropylene tube with a wall thickness of 20mm and an outer diameter of 200mm.

[0076] Example 3

[0077] Step 1: Mix 84.9 parts of random copolymer polypropylene (PA14D), 15 parts of homopolymer polypropylene (T30S), and 0.1 parts of β-nucleating agent (DCHT), and melt and extrude them in a screw extruder. The melt temperature is 230-250℃, the extrusion temperature is 170-200℃, the length of the die section is 10cm, and the screw speed is 50rpm.

[0078] Step 2: The molten tube preform extruded in Step 1 is cooled to 125°C within 2-10 seconds in an air cooling device. The length of the air cooling field is 8cm, the wind speed in the air cooling field is 5m / s, and the outlet air temperature is 10°C. Then, it is cooled and shaped to obtain a random copolymer polypropylene tube with a wall thickness of 20mm and an outer diameter of 200mm.

[0079] Example 4

[0080] Step 1: Mix 79.9 parts of random copolymer polypropylene (PA14D), 20 parts of homopolymer polypropylene (T30S), and 0.1 parts of β-nucleating agent (DCHT), and melt and extrude them in a screw extruder. The melt temperature is 230-250℃, the extrusion temperature is 170-200℃, the length of the die section is 10cm, and the screw speed is 50rpm.

[0081] Step 2: The molten tube preform extruded in Step 1 is cooled to 125°C within 2-10 seconds in an air cooling device. The length of the air cooling field is 8cm, the wind speed in the air cooling field is 5m / s, and the outlet air temperature is 10°C. Then, it is cooled and shaped to obtain a random copolymer polypropylene tube with a wall thickness of 20mm and an outer diameter of 200mm.

[0082] Example 5

[0083] Step 1: Mix 89.9 parts of random copolymer polypropylene (PA14D), 10 parts of block copolymer polypropylene (DY-ZK0640P), and 0.2 parts of β-nucleating agent (DCHT), and melt and extrude them in a screw extruder. The melt temperature is 230-250℃, the extrusion temperature is 170-200℃, the die length is 20cm, and the screw speed is 50rpm.

[0084] Step 2: The molten tube preform extruded in Step 1 is cooled to 125°C within 2-10 seconds in an air cooling device. The length of the air cooling field is 8cm, the wind speed in the air cooling field is 5m / s, and the outlet air temperature is 10°C. Then, it is cooled and shaped to obtain a random copolymer polypropylene tube with a wall thickness of 20mm and an outer diameter of 200mm.

[0085] Example 6

[0086] Step 1: Mix 94.9 parts of random copolymer polypropylene (PA14D), 5 parts of block copolymer polypropylene (DY-ZK0640P), and 0.01 parts of β-nucleating agent (DCHT), and melt and extrude them in a screw extruder. The melt temperature is 230-250℃, the extrusion temperature is 170-200℃, the die length is 20cm, and the screw speed is 50rpm.

[0087] Step 2: The molten tube preform extruded in Step 1 is cooled to 125°C within 2-10 seconds in an air cooling device. The length of the air cooling field is 8cm, the wind speed in the air cooling field is 5m / s, and the outlet air temperature is 10°C. Then, it is cooled and shaped to obtain a random copolymer polypropylene tube with a wall thickness of 20mm and an outer diameter of 200mm.

[0088] Comparative Example 1

[0089] Step 1: Mix 99.9 parts of random copolymer polypropylene (PA14D) and 0.1 parts of β nucleating agent (DCHT), melt and extrude in a screw extruder, with a melt temperature of 230-250°C, an extrusion temperature of 170-200°C, a die length of 20 cm, and a screw speed of 50 rpm.

[0090] Step 2: The molten tube preform extruded in Step 1 is cooled to 125°C within 2-10 seconds in an air-cooling device. The length of the air-cooling field is 8cm, the wind speed in the air-cooling field is 5m / s, and the outlet air temperature is 10°C. Then, it is cooled and shaped to obtain a random copolymer polypropylene tube with a wall thickness of 20mm and an outer diameter of 200mm.

[0091] Example 7

[0092] Step 1: Mix 89.9 parts of random copolymer polypropylene (PA14D), 10 parts of homopolymer polypropylene (T30S), and 0.1 parts of β-nucleating agent (DCHT), and melt and extrude them in a screw extruder. The melt temperature is 230-250℃, the extrusion temperature is 170-200℃, the length of the die section is 10cm, and the screw speed is 5rpm.

[0093] Step 2: The molten tube preform extruded in Step 1 is cooled to 120°C within 2-10 seconds in an air-cooling device. The length of the air-cooling field is 8cm, the wind speed in the air-cooling field is 10m / s, and the outlet air temperature is 0°C. Then, it is cooled and shaped to obtain a random copolymer polypropylene tube with a wall thickness of 50mm and an outer diameter of 300mm.

[0094] Example 8

[0095] Step 1: Mix 89.9 parts of random copolymer polypropylene (PA14D), 10 parts of homopolymer polypropylene (T30S), and 0.1 parts of β-nucleating agent (DCHT), and melt and extrude them in a screw extruder. The melt temperature is 230-250℃, the extrusion temperature is 170-200℃, the length of the die section is 10cm, and the screw speed is 100rpm.

[0096] Step 2: The molten tube preform extruded in Step 1 is cooled to 130°C within 2-10 seconds in an air-cooling device. The length of the air-cooling field is 8cm, the wind speed in the air-cooling field is 5m / s, and the outlet air temperature is 20°C. Then, it is cooled and shaped to obtain a random copolymer polypropylene tube with a wall thickness of 20mm and an outer diameter of 200mm.

[0097] Example 9

[0098] Step 1: Mix 89.9 parts of random copolymer polypropylene (PA14D), 10 parts of homopolymer polypropylene (T30S), and 0.1 parts of β-nucleating agent (DCHT), and melt and extrude them in a screw extruder. The melt temperature is 230-250℃, the extrusion temperature is 170-200℃, the length of the die section is 10cm, and the screw speed is 50rpm.

[0099] Step 2: The molten tube preform extruded in Step 1 is cooled to 138°C within 2-10 seconds in an air-cooling device. The length of the air-cooling field is 8cm, the wind speed in the air-cooling field is 0.5m / s, and the outlet air temperature is 25°C. Then, it is cooled and shaped to obtain a random copolymer polypropylene tube with a wall thickness of 1mm and an outer diameter of 10mm.

[0100] Example 10

[0101] Step 1: Mix 89.9 parts of random copolymer polypropylene (PA14D), 10 parts of homopolymer polypropylene (T30S), and 0.1 parts of β-nucleating agent (DCHT), and melt and extrude them in a screw extruder. The melt temperature is 230-250℃, the extrusion temperature is 170-200℃, the length of the die section is 10cm, and the screw speed is 50rpm.

[0102] Step 2: The molten tube preform extruded in Step 1 is cooled to 135°C within 2-10 seconds in an air-cooling device. The length of the air-cooling field is 5cm, the wind speed in the air-cooling field is 5m / s, and the outlet air temperature is 20°C. Then, it is cooled and shaped to obtain a random copolymer polypropylene tube with a wall thickness of 20mm and an outer diameter of 200mm.

[0103] Example 11

[0104] Step 1: Mix 89.9 parts of random copolymer polypropylene (PA14D), 10 parts of homopolymer polypropylene (T30S), and 0.1 parts of β-nucleating agent (DCHT), and melt and extrude them in a screw extruder. The melt temperature is 230-250℃, the extrusion temperature is 170-200℃, the length of the die section is 10cm, and the screw speed is 50rpm.

[0105] Step 2: The molten tube preform extruded in Step 1 is cooled to 126°C within 2-10 seconds in an air-cooling device. The length of the air-cooling field is 10cm, the wind speed in the air-cooling field is 5m / s, and the outlet air temperature is 20°C. Then, it is cooled and shaped to obtain a random copolymer polypropylene tube with a wall thickness of 20mm and an outer diameter of 200mm.

[0106] Comparative Example 2

[0107] Step 1: Mix 89.9 parts of random copolymer polypropylene (PA14D), 10 parts of homopolymer polypropylene (T30S), and 0.1 parts of β-nucleating agent (DCHT), and melt and extrude them in a screw extruder. The melt temperature is 230-250℃, the extrusion temperature is 170-200℃, the length of the die section is 10cm, and the screw speed is 50rpm.

[0108] Step 2: The molten tube preform extruded in Step 1 is cooled and shaped to obtain a random copolymer polypropylene tube with a wall thickness of 20 mm and an outer diameter of 200 mm.

[0109] Examples 1-6 and Comparative Example 1 are random copolymer polypropylene pipes prepared according to the raw material mass parts in Table 1.

[0110] Table 1 Raw material composition of random copolymer polypropylene pipe

[0111]

[0112] The random copolymer polypropylene pipes prepared in Examples 1-6 and Comparative Example 1 were tested, and the test results are shown in Table 2 and... Figure 4 As shown.

[0113] Table 2 Tensile strength and impact toughness of random copolymer polypropylene pipes

[0114]

[0115] From Table 2 and Figure 4 As shown, the present invention can simultaneously improve the strength and low-temperature toughness of random copolymer polypropylene pipes, thereby expanding their application range in low-temperature environments.

[0116] Furthermore, the tensile strength of random copolymer polypropylene pipes gradually increases with the increase of homopolymer polypropylene content. This is because the higher strength of homopolymer polypropylene is more conducive to improving the strength of the pipe. In addition, the β-type hybrid tandem crystals induced by the fibrous β-nucleating agent after recrystallization are arranged axially, and the synergistic effect of these two factors significantly increases the tensile strength of the pipe. However, the low-temperature impact toughness shows a different trend. (See Table 2 and...) Figure 4 As shown, the random copolymer polypropylene pipe prepared in Example 2 exhibits higher impact toughness than those in Examples 1, 3, and 4. The observed trend is as follows: with the addition of homopolymer polypropylene, the impact toughness of the random copolymer polypropylene pipe increases, and within a certain range, the increase increases with the increase in homopolymer polypropylene content; however, when the homopolymer polypropylene content exceeds a certain threshold, the impact toughness begins to decrease rapidly. Specific analysis is as follows:

[0117] (1) When no homopolymer polypropylene or block copolymer polypropylene is added, the random copolymer polypropylene has poor regularity of random copolymer molecular chains. Even under the action of β nucleating agent, it is difficult to arrange them in a regular manner to form β crystals. Therefore, the impact toughness of the pipe is at a low level.

[0118] (2) With the addition of homopolymer polypropylene or block copolymer polypropylene components, fibrous β-nucleating agents after recrystallization first crystallize to form β-crystal nuclei. These nuclei further induce epigenetic crystallization of random copolymer polypropylene, thereby forming a large number of β-type hybrid tandem crystals inside the random copolymer polypropylene pipe. This ensures improved pipe strength while enhancing low-temperature toughness. When the weight of homopolymer polypropylene components increases from 5 parts to 10 parts, the impact toughness of the sample shows a significant increasing trend. This is because, within a certain range, high content of homopolymer polypropylene or block copolymer polypropylene is more conducive to the formation of β-crystals in random copolymer polypropylene, resulting in a significant enhancement of the pipe's impact toughness.

[0119] (3) When the weight of homopolymer polypropylene component increased from 10 parts to 15 parts, the impact toughness of the sample showed a more obvious decreasing trend. This is because the effect of homopolymer polypropylene on the induction of epigenetic crystallization of random copolymer polypropylene has become saturated. Even if more homopolymer polypropylene is added, it is difficult to achieve a significant increase in β crystal content. On the contrary, higher content of homopolymer polypropylene may even reduce the impact toughness of the pipe due to its brittle properties. When the weight of homopolymer polypropylene component increased from 15 parts to 20 parts, the impact toughness of the sample continued to show a decreasing trend. Until 20 parts, the impact toughness of the pipe was only slightly higher than that of the comparative example 1 without the addition of homopolymer polypropylene.

[0120] As shown in Tables 2 and 5, the addition of block copolymer polypropylene is more beneficial to improving impact strength, but its effect on tensile strength is not as significant as that of homopolymer polypropylene. Furthermore, the above discussion focuses on the interaction between the components of the pipe based on changes in the amount of homopolymer polypropylene added. The effect of changes in the amount of block copolymer polypropylene added on the pipe is similar to that of homopolymer polypropylene, and will not be elaborated further here.

[0121] Therefore, when the homopolymer polypropylene and / or block copolymer polypropylene in the pipe of the present invention is 8 to 12 parts by mass, the β nucleating agent is 0.05 to 0.1 parts by mass, and the random copolymer polypropylene is 87.9 to 91.95 parts by mass, the pipe has preferred low-temperature toughness and rigidity.

[0122] In addition, Examples 7-11 and Comparative Example 2 are similar to Example 2, except that the parameters for cooling to 120-138°C within 2-10 seconds during pipe preparation are changed (cooling air temperature in the air ring, i.e., outlet air temperature; air cooling field length; cooling temperature of molten pipe blank). In Comparative Example 2, the molten pipe blank was not cooled to 120-138°C within 2-10 seconds, but was directly extruded and then cooled and shaped, as shown in Table 3.

[0123] Table 3 Different Cooling Processes for Random Copolymer Polypropylene Pipes

[0124]

[0125] The random copolymer polypropylene pipes prepared in Examples 2, 7-11 and Comparative Example 2 were tested, and the test results are shown in Table 4.

[0126] Table 4 Tensile strength and impact toughness of random copolymer polypropylene pipes

[0127]

[0128] As shown in Table 4, the stepwise cooling crystallization process of this invention can significantly improve the strength and low-temperature impact toughness of random copolymer polypropylene pipes. If the cooling intensity is too high, the homopolymer polypropylene molecular chains do not have enough time to arrange themselves into a regular crystal structure, resulting in an excessively low content of β-precursors for β-nucleating agent-induced epigenetic crystallization. This makes it difficult to exert a sufficient crystallization-promoting effect and induce the formation of β-crystals in the random copolymer polypropylene. The performance of the prepared sample is only slightly higher than that of Comparative Example 2. If the cooling intensity is too low, the β-precursors formed by the homopolymer polypropylene are larger in size and have a smaller specific surface area, which is not conducive to the epigenetic crystallization of the random copolymer polypropylene and increases site and equipment costs.

[0129] Figure 2 Polarized photographs of the random copolymer polypropylene pipe prepared in Comparative Example 2 (left) and the random copolymer polypropylene pipe prepared in Example 2 of this invention (right). Figure 2 It can be seen that the crystal form of the random copolymer polypropylene pipe prepared in Comparative Example 2 is mainly α crystal, while the random copolymer polypropylene pipe prepared in Example 2 contains a large number of oriented one-dimensional β-type hybrid tandem crystals.

[0130] Therefore, when the cooling air temperature inside the air ring is 10–25℃ and the length of the air cooling field is 5–8cm, the β-crystal regulation effect inside the pipe is better, and the mechanical properties of the random copolymer polypropylene are higher.

[0131] The above description uses pipes containing homopolymer polypropylene to illustrate the cooling intensity law. The cooling intensity law for pipes containing block copolymer polypropylene is similar and will not be repeated here.

[0132] Of course, the present invention may have other various embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications according to the present invention, but these corresponding changes and modifications should all fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing random copolymer polypropylene pipe, characterized in that, Includes the following steps: Step 1: Mix random copolymer polypropylene, homopolymer polypropylene and / or block copolymer polypropylene, and β nucleating agent, melt and extrude, with a melt temperature of 230~250℃ and an extrusion temperature of 170~200℃. Step 2: Cool the molten tube preform extruded in Step 1 to 120-138°C within 2-10 seconds, and then cool and shape it to obtain random copolymer polypropylene tube. The amount of random copolymer polypropylene is 78 to 98.99 parts by mass; the amount of homopolymer polypropylene and / or block copolymer polypropylene is 1 to 20 parts by mass; and the amount of β nucleating agent is 0.01 to 2 parts by mass. The cooling of the molten tube blank is carried out in an air ring cooling device, which provides an air cooling field with a length of 5 to 20 cm in the extrusion direction of the molten tube blank. The air velocity in the air cooling field is 0.5 to 10 m / s and the outlet air temperature is 0 to 25℃. The random copolymer polypropylene has a melting temperature not higher than 150°C; the homopolymer polypropylene and block copolymer polypropylene have melting temperatures of 138~170°C; and the β-nucleating agent has a crystallization temperature of 170~200°C.

2. The method for preparing random copolymer polypropylene pipe according to claim 1, characterized in that, The amount of homopolymer polypropylene and / or block copolymer polypropylene used is 8-12 parts by mass, the amount of β nucleating agent used is 0.05-0.1 parts by mass, and the amount of random copolymer polypropylene used is 87.9-91.95 parts by mass.

3. The method for preparing random copolymer polypropylene pipe according to claim 1, characterized in that, The wall thickness of the molten tube blank is 1~50mm, and the diameter-to-thickness ratio is not less than 5.

4. The method for preparing random copolymer polypropylene pipe according to claim 1, characterized in that, The melting and extrusion are carried out in a screw extruder, which includes a melting section and a die section. The length of the die section is 10-20 cm, and the screw speed is 5-100 rpm.

5. The method for preparing random copolymer polypropylene pipe according to claim 1, characterized in that, The cooling and shaping process is carried out in a vacuum sizing and cooling device.

6. The application of the random copolymer polypropylene pipe obtained by the preparation method according to any one of claims 1-5 in urban water supply and drainage, gas transmission, power and optical cable sheathing, industrial fluid transmission, and agricultural irrigation.

Citation Information

Patent Citations

  • Beta nucleating agent for polypropylene, preparation method thereof, and beta polypropylene pipe special material prepared from same

    CN102146183A

  • Cooling device for polypropylene pipe

    CN214395357U

  • Low-temperature impact resistance PP-R tubing and preparation method thereof

    CN103360686A

  • Special material for high-toughness and high-water pressure resistance polypropylene randon copolymer (PPR) pipe material and preparation process thereof

    CN103709522A

  • Polypropylene composition, preparation method thereof and pipe prepared from polypropylene composition