A waterproof self-heating food packaging lunch box and a preparation method thereof
By preparing a waterproof and breathable membrane using modified carbon fiber-hydroxyapatite composite and PBO fiber, the problem of structural instability of waterproof and breathable membranes in self-heating food packaging boxes due to thermal expansion was solved, achieving higher structural stability and food safety.
Patent Information
- Application Number
- CN202311771740.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-21
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-21
AI Technical Summary
Existing self-heating food packaging containers, in their fully sealed state, are susceptible to damage from the waterproof and breathable membrane caused by the thermal expansion of water vapor, leading to structural instability and affecting food safety.
A waterproof and breathable membrane was prepared using modified carbon fiber-hydroxyapatite composite and PBO fiber. The structural stability of the membrane was improved by gradient transition of thermal expansion coefficient and stress transmission, and the bonding strength between the fiber and the composite was enhanced by pretreatment.
It significantly improves the structural stability of the waterproof and breathable membrane under thermal expansion, ensuring the safety and durability of self-heating food packaging boxes.
Smart Images

Figure BDA0004621358220000061 
Figure BDA0004621358220000071 
Figure BDA0004621358220000081
Abstract
Description
Technical Field
[0001] This application relates to the field of food packaging technology, and more specifically, to a waterproof self-heating food packaging container and its preparation method. Background Technology
[0002] Self-heating food packaging containers typically use a heating agent packaged in non-woven fabric inside the container to react with water to generate heat, thus quickly heating the food. Because no external heat source or appliance is required, and it is convenient and quick to use, it is widely used in self-heating foods such as self-heating rice, self-heating hot pot, and self-heating rice noodles.
[0003] Currently, commonly used self-heating food packaging boxes typically include an outer box, an inner box, and a lid. A self-heating pack is placed between the outer and inner boxes, and ventilation holes are provided along the upper edges of both boxes. When in use, water is added to the outer box, and the self-heating pack generates steam upon contact with the water. This steam enters the inner box through the ventilation holes, heating the food. However, the self-heating pack usually uses non-woven fabric to package the heating agent. During the actual heat release process upon contact with water, the chemical components produced by the reaction of the heating agent inevitably come into contact with the food along with the steam, potentially leading to food safety issues. Therefore, Chinese invention patent application CN116062317A discloses a safe and highly efficient self-heating packaging box. This box uses a fully sealed design between the inner and outer boxes. After the heating pack generates steam upon contact with water, the ventilation holes and waterproof breathable membrane ensure heat transfer while isolating the steam. This prevents food safety hazards caused by harmful substances (quicklime, aluminum powder) mixed in with the steam coming into direct contact with the food due to packaging damage.
[0004] Regarding the aforementioned technologies, the inventors believe that because heating packs often react violently when exposed to water, a large amount of water vapor is rapidly generated after the water boils. In the case of a fully sealed inner and outer box, the strong water vapor effect will cause a relatively violent thermal expansion of the waterproof and breathable membrane, which can easily lead to damage to the structure of the waterproof and breathable membrane, thus greatly reducing the expected effect. Therefore, it is urgent to propose a solution to the above-mentioned technical problems. Summary of the Invention
[0005] In order to improve the structural stability of the waterproof and breathable membrane in the self-heating packaging box under thermal expansion, this application provides a waterproof self-heating food packaging box and its preparation method.
[0006] In a first aspect, this application provides a waterproof self-heating food packaging box, employing the following technical solution: A waterproof self-heating food packaging box includes an outer box, an inner box, and a heating pack. The inner box is sealed and suspended inside the outer box. The heating pack is disposed between the bottom of the inner box and the bottom of the outer box. The inner box is provided with ventilation holes and a waterproof and breathable membrane covering the ventilation holes. The waterproof and breathable membrane is made of raw materials comprising the following parts by weight: 50-70 parts of polyurethane acrylate; 2-4 parts coupling agent; 3-5 parts dispersant; 10-15 parts of filler; 5-10 parts antibacterial agent; 4-7 parts of modified carbon fiber-hydroxyapatite composite; The modified carbon fiber-hydroxyapatite composite was prepared by the following method: S1. Take carbon fiber raw material, heat it to 300-500℃ and hold for 20-30 minutes. After cooling, soak it in acid solution and alkaline solution in sequence. The soaking temperature is 70-80℃ and the soaking time is 18-24 hours each time. After soaking, wash and dry to obtain pretreated carbon fiber. Mix deionized water and hydroxyapatite powder in a weight ratio of 1:(0.4-0.5). Then add sodium hexametaphosphate accounting for 4%-6% of the weight of hydroxyapatite powder. After ball milling, obtain hydroxyapatite slurry. S2. Immerse the pretreated carbon fiber from step S1 in hydroxyapatite slurry, quickly pull it up and then quickly dry it at 80-90℃. Repeat the above process 4-6 times to obtain the modified carbon fiber-hydroxyapatite composite material.
[0007] By adopting the above technical solution, in the preparation process of modified carbon fiber-hydroxyapatite composite, the carbon fiber raw material is first oxidized at a high temperature to improve its activity; then, it undergoes acid and alkali treatments to make the carbon fiber surface rougher, resulting in more uneven grooves and an increased specific surface area; finally, during the repeated lifting and drying process of the pretreated carbon fiber immersed in hydroxyapatite slurry, the pretreated carbon fiber and hydroxyapatite slurry exhibit high bonding strength, and a high-strength coating is formed on the carbon fiber surface, thus obtaining the modified carbon fiber-hydroxyapatite composite. Applying the modified carbon fiber-hydroxyapatite composite to the preparation of waterproof and breathable membranes allows for a gradient transition of thermal expansion coefficients when subjected to hot steam impact, buffering thermal expansion. Furthermore, the tight bonding between the modified carbon fiber-hydroxyapatite composite and its constituent raw materials, along with the stress transmission effect of the modified carbon fiber-hydroxyapatite composite, enables the waterproof and breathable membrane to maintain excellent structural stability under thermal expansion, which is beneficial for ensuring the practical application effect of waterproof self-heating food packaging containers.
[0008] Preferably, the raw material of the waterproof and breathable membrane also contains 3-5 parts by weight of PBO fiber.
[0009] By adopting the above technical solution, the addition of PBO fiber can play an excellent role in compounding and synergistic effect with modified carbon fiber-hydroxyapatite composite material. By forming an inter-adhesive and cross-shaped network structure in the waterproof and breathable membrane, it can strengthen the overall structure of the waterproof and breathable membrane and significantly improve the structural stability of the waterproof and breathable membrane under thermal expansion.
[0010] Preferably, the weight ratio of the modified carbon fiber-hydroxyapatite composite to PBO fiber is 5:4.
[0011] By adopting the above technical solution, the modified carbon fiber-hydroxyapatite composite material and PBO fiber in the above weight ratio can play a better synergistic role in the application process, so that the waterproof and breathable membrane can perform optimally in the application of hot steam impact, and thus play a more stable role in the application process, so that the waterproof self-heating food packaging box has a high quality.
[0012] Preferably, the PBO fibers are pretreated before use, and the pretreatment steps are as follows: Take PBO fiber raw material, soak it in a 50%-70% methanesulfonic acid solution, maintain it at 50-80℃ for 4-8 hours, wash and dry it, then soak it in a polyphosphoric acid-acetic acid composite solution with a polyphosphoric acid content of 6%-8%, maintain it at 30-40℃ for 3-5 minutes, wash and dry it to obtain pretreated PBO fiber.
[0013] By employing the above-mentioned technical solution, PBO fibers are pretreated and then sequentially treated with methanesulfonic acid solution and polyphosphoric acid-acetic acid composite solution. On the one hand, this improves the surface roughness of the PBO fibers, enabling a tighter bond with polyurethane acrylate. On the other hand, it also allows the formation of active groups on the surface of the PBO fibers, resulting in a more stable adhesion between the fibers and the modified carbon fiber-hydroxyapatite composite material. The combined effect of these two treatments is significantly enhanced. Therefore, the application of pretreated PBO fibers can significantly improve the thermal expansion resistance of waterproof and breathable membranes, and make the actual application effect of waterproof self-heating food packaging boxes more stable.
[0014] Preferably, the coupling agent is one or a combination of several of the following: silane coupling agents, titanate coupling agents, aluminate coupling agents, and phosphate coupling agents.
[0015] By adopting the above technical solutions, the above-mentioned coupling agents are all suitable for the preparation of waterproof and breathable membranes, and can play an excellent and stable corresponding role in the application process, so that the raw materials of each component can be more tightly bound, thereby obtaining a high-quality waterproof and breathable membrane, and ensuring that the resulting waterproof self-heating food packaging lunch box is also of good quality.
[0016] Preferably, the dispersant is a composition of polyethylene wax and stearate in any weight ratio.
[0017] By adopting the above technical solution, the dispersant composed of polyethylene wax and stearate can uniformly disperse the raw materials of each component during the application process and form a stable bond state, thereby giving the obtained waterproof and breathable membrane better quality.
[0018] Preferably, the filler is one or a combination of several of alumina, silicon dioxide, calcium carbonate, talc, silica powder and bentonite.
[0019] By adopting the above technical solutions, the above-mentioned fillers can improve the dimensional stability and surface smoothness of the waterproof and breathable membrane, enabling the waterproof and breathable membrane to maintain structural stability when subjected to hot steam impact, and the application of the above-mentioned fillers can also reduce costs.
[0020] Secondly, this application provides a method for preparing a waterproof self-heating food packaging container, which adopts the following technical solution: A method for preparing a waterproof self-heating food packaging container includes the following steps: (1) Prepare raw materials containing polyurethane acrylate, coupling agent, dispersant, filler, antibacterial agent and modified carbon fiber-hydroxyapatite composite material according to the formula; (2) After the polyurethane acrylate, coupling agent, dispersant, filler, antibacterial agent and modified carbon fiber-hydroxyapatite composite material in step (1) are mixed evenly, the mixture is heated, extruded and granulated, and then cast and stretched to obtain a waterproof and breathable membrane. (3) Fix the waterproof and breathable membrane to the inner box with adhesive and cover the ventilation holes. Then assemble the outer box, inner box and heating pack to obtain a waterproof self-heating food packaging box.
[0021] By adopting the above technical solution, the above preparation method is simple to operate and can obtain a waterproof and breathable membrane of excellent quality and stability. Then, the waterproof and breathable membrane is fixed on the inner box with an adhesive and the ventilation holes are covered, which is more convenient and can ensure that the waterproof and breathable membrane plays a stable role at the ventilation holes, thereby obtaining a waterproof self-heating food packaging box of excellent quality and stability.
[0022] In summary, this application has the following beneficial effects: 1. This application uses a specially prepared modified carbon fiber-hydroxyapatite composite material, which is applied to the preparation of waterproof and breathable membrane. It can not only form a gradient transition of thermal expansion coefficient, but also play an excellent stress transmission role. Therefore, when the waterproof and breathable membrane is subjected to thermal expansion, it can maintain relatively good structural stability, which is conducive to ensuring that the final waterproof self-heating food packaging box has a stable practical application effect. 2. This application uses PBO fiber. Through the compounding effect between PBO fiber and modified carbon fiber-hydroxyapatite composite material, the structural stability of the waterproof and breathable membrane under thermal expansion is significantly improved. Furthermore, the PBO fiber is pretreated to further enhance its corresponding effects, making the actual application effect of the waterproof self-heating food packaging box more stable. Detailed Implementation
[0023] The present application will be further described in detail below with reference to preparation examples and embodiments.
[0024] Unless otherwise specified, all raw materials used in the preparation examples and embodiments of this application are commercially available. The polyurethane acrylate was purchased from Langbowan polyurethane acrylate PUA901; The polyethylene wax was purchased from Honeywell as polyethylene wax A-C617A; The carbon fiber has a diameter of 7μm and a length of 0.5mm; The PBO fiber has a diameter of 0.2 mm and a length of 1 mm.
[0025] Preparation examples of raw materials and / or intermediates Preparation Example 1 A modified carbon fiber-hydroxyapatite composite material is prepared by the following method: S1. Take carbon fiber raw material, heat it to 400℃ and keep it for 25 minutes. After cooling, soak it in acid solution and alkaline solution in sequence. The soaking temperature is 75℃ and the soaking time is 21 hours each time. After soaking, wash and dry to obtain pretreated carbon fiber. Deionized water and hydroxyapatite powder were mixed at a weight ratio of 1:0.45, and then sodium hexametaphosphate (5% by weight of hydroxyapatite powder) was added. After ball milling, hydroxyapatite slurry was obtained. S2. Immerse the pretreated carbon fiber from step S1 in hydroxyapatite slurry, quickly pull it up and then quickly dry it at 85°C. Repeat the above process 5 times to obtain the modified carbon fiber-hydroxyapatite composite material.
[0026] Note: The acid solution used in the above operation is a 5% hydrochloric acid solution and the alkali solution is an 8% sodium hydroxide solution. The ball milling process uses a YNL-650 ball mill with a mill speed of 20 r / min and a milling time of 10 h.
[0027] Preparation Example 2 A modified carbon fiber-hydroxyapatite composite material, which differs from Preparation Example 1 in that it is prepared by the following method: S1. Take carbon fiber raw material, heat it to 300°C and hold it for 30 min, cool it and then soak it in acid solution and alkaline solution in sequence. The soaking temperature is 70°C and the soaking time is 24 h each time. After soaking, wash and dry to obtain pretreated carbon fiber. Deionized water and hydroxyapatite powder were mixed at a weight ratio of 1:0.4, and then sodium hexametaphosphate, accounting for 4% of the weight of hydroxyapatite powder, was added. After ball milling, hydroxyapatite slurry was obtained. S2. Immerse the pretreated carbon fiber from step S1 in hydroxyapatite slurry, quickly pull it up and then quickly dry it at 80°C. Repeat the above process 6 times to obtain the modified carbon fiber-hydroxyapatite composite material.
[0028] Preparation Example 3 A modified carbon fiber-hydroxyapatite composite material, which differs from Preparation Example 1 in that it is prepared by the following method: S1. Take carbon fiber raw material, heat it to 500℃ and hold it for 20 min, cool it and then soak it in acid solution and alkaline solution in sequence. The soaking temperature is 80℃ and the soaking time is 18 h each time. After soaking, wash and dry to obtain pretreated carbon fiber. Deionized water and hydroxyapatite powder were mixed at a weight ratio of 1:0.5, and then sodium hexametaphosphate, accounting for 6% of the weight of hydroxyapatite powder, was added. After ball milling, hydroxyapatite slurry was obtained. S2. Immerse the pretreated carbon fiber from step S1 in hydroxyapatite slurry, quickly pull it up and then quickly dry it at 90°C. Repeat the above process 4 times to obtain the modified carbon fiber-hydroxyapatite composite material.
[0029] Preparation Example 4 A pretreated PBO fiber is prepared by the following method: PBO fiber raw material was soaked in a 60% methanesulfonic acid solution and maintained at 65°C for 6 hours. After washing and drying, it was soaked in a 7% polyphosphoric acid-acetic acid composite solution and maintained at 35°C for 4 minutes. After washing and drying, pretreated PBO fiber was obtained.
[0030] Preparation Example 5 A pretreated PBO fiber is prepared by the following method: PBO fiber raw material was soaked in a 50% methanesulfonic acid solution and maintained at 50°C for 8 hours. After washing and drying, it was soaked in a 6% polyphosphoric acid-acetic acid composite solution and maintained at 30°C for 5 minutes. After washing and drying, pretreated PBO fiber was obtained.
[0031] Preparation Example 6 A pretreated PBO fiber is prepared by the following method: PBO fiber raw material was soaked in a 70% methanesulfonic acid solution and maintained at 80°C for 4 hours. After washing and drying, it was soaked in a polyphosphoric acid-acetic acid composite solution with a polyphosphoric acid content of 8% and maintained at 40°C for 3 minutes. After washing and drying, pretreated PBO fiber was obtained. Example
[0032] Example 1 A waterproof self-heating food packaging container includes an outer box, an inner box, and a heating pack. The inner box is sealed and suspended inside the outer box. The heating pack is located between the bottom of the inner box and the bottom of the outer box. The inner box has ventilation holes and a waterproof and breathable membrane covering the ventilation holes. The components of the waterproof and breathable membrane and their corresponding weights are shown in Table 1. The preparation steps of the waterproof self-heating food packaging container are as follows: (1) Prepare raw materials containing polyurethane acrylate, coupling agent, dispersant, filler, antibacterial agent and modified carbon fiber-hydroxyapatite composite material according to the formula; (2) After the polyurethane acrylate, coupling agent, dispersant, filler, antibacterial agent and modified carbon fiber-hydroxyapatite composite material in step (1) are mixed evenly, the mixture is heated to 270°C, extruded and granulated, and then cast and stretched to obtain a waterproof and breathable membrane. (3) Fix the waterproof and breathable membrane to the inner box with adhesive and cover the ventilation holes. Then assemble the outer box, inner box and heating pack to obtain a waterproof self-heating food packaging box.
[0033] Note: In the above operations, the modified carbon fiber-hydroxyapatite composite material was obtained in Preparation Example 1; the coupling agent was silane coupling agent KH560; the dispersant was composed of polyethylene wax and stearate in a weight ratio of 3:1, and the stearate was selected as calcium stearate; the filler was silica powder; the antibacterial agent was silver oxide; the thickness of the obtained waterproof and breathable membrane was 0.8 mm; and the adhesive was Kraft 706 silicone adhesive.
[0034] Example 2-3 A waterproof self-heating food packaging box differs from Example 1 in that the components of the waterproof and breathable membrane and their corresponding weights are shown in Table 1.
[0035] Table 1. Components and their weight percentages (kg / part) of the waterproof and breathable membranes in Examples 1-3. Example 4 A waterproof self-heating food packaging box, which differs from Example 1 in that the modified carbon fiber-hydroxyapatite composite material is obtained in Preparation Example 2.
[0036] Example 5 A waterproof self-heating food packaging box, which differs from Example 1 in that the modified carbon fiber-hydroxyapatite composite material is obtained in Preparation Example 3.
[0037] Example 6 A waterproof self-heating food packaging box, which differs from Example 1 in that the waterproof and breathable membrane also contains 4 parts by weight of PBO fiber.
[0038] Example 7 A waterproof self-heating food packaging box, which differs from Example 1 in that the waterproof and breathable membrane also contains 3 parts by weight of PBO fiber.
[0039] Example 8 A waterproof self-heating food packaging box, which differs from Example 1 in that the waterproof and breathable membrane also contains 5 parts by weight of PBO fiber.
[0040] Example 9 A waterproof self-heating food packaging box differs from Example 6 in that the total amount of modified carbon fiber-hydroxyapatite composite and PBO fiber remains unchanged, but their weight ratio is adjusted to 5:4.
[0041] Example 10 A waterproof self-heating food packaging box, which differs from Example 6 in that the PBO fiber is replaced with pretreated PBO fiber of equal mass, and the pretreated PBO fiber is obtained in Preparation Example 4.
[0042] Example 11 A waterproof self-heating food packaging container, which differs from Example 10 in that the pretreated PBO fiber is obtained from Preparation Example 5.
[0043] Example 12 A waterproof self-heating food packaging box, which differs from Example 10 in that the pretreated PBO fiber is obtained from Preparation Example 6.
[0044] Comparative Example Comparative Example 1 A waterproof self-heating food packaging box, which differs from Example 1 in that the waterproof and breathable membrane does not contain modified carbon fiber-hydroxyapatite composite material in its raw material.
[0045] Comparative Example 2 A waterproof self-heating food packaging box, which differs from Example 6 in that the waterproof and breathable membrane does not contain modified carbon fiber-hydroxyapatite composite material in its raw material.
[0046] Comparative Example 3 A waterproof self-heating food packaging box, which differs from Example 10 in that the waterproof and breathable membrane does not contain modified carbon fiber-hydroxyapatite composite material in its raw material.
[0047] Performance testing samples: The waterproof self-heating food packaging boxes obtained in Examples 1-12 were used as test samples 1-12, and the waterproof self-heating food packaging boxes obtained in Comparative Examples 1-3 were used as control samples 1-3. The self-heating food packaging boxes were manufactured according to the Chinese invention patent application document with publication number CN116062317A. The heating packs were purchased from Shenzhen Xinzhiyuan Technology Co., Ltd., product number SPFRB, with a single pack weighing 70g.
[0048] Test Method: For the waterproof and breathable membranes used in test samples 1-12 and control samples 1-3, tensile strength was measured using a PSHG-D2501 tensile strength tester. Each sample was measured five times, and the average value was recorded as the initial tensile strength of the corresponding sample. A heating pack was mixed with 200ml of water, and the generated water vapor caused thermal expansion of the waterproof and breathable membrane until the water stopped boiling. The waterproof and breathable membrane was then removed and dried, and the tensile strength was measured in the same way. Each sample was measured five times, and the average value was recorded as the test tensile strength of the corresponding sample. Then, the tensile strength loss rate of each sample was calculated. Tensile strength loss rate (%) = (initial tensile strength - test tensile strength) / initial tensile strength. The higher the tensile strength loss rate, the worse the structural stability of the waterproof and breathable membrane when subjected to water vapor impact.
[0049] Table 2 Test results of test samples 1-12 and control samples 1-3 As can be seen from Examples 1-3 and Comparative Example 1, and Table 2, the use of specially prepared modified carbon fiber-hydroxyapatite composite material in the waterproof and breathable membrane can greatly cope with the structural damage caused by water vapor impact. The tensile strength loss rate measured in the experiment is also greatly reduced. It can be seen that the waterproof and breathable membrane can maintain excellent structural stability when subjected to thermal expansion, and thus can play its role in a relatively stable manner, so that the resulting waterproof self-heating food packaging box has a stable practical application effect.
[0050] As can be seen from Examples 1 and 6-8, and Table 2, the use of PBO fibers can significantly reduce the tensile strength loss rate of the waterproof and breathable membrane, thereby significantly improving its resistance to thermal expansion. Furthermore, as can be seen from Comparative Examples 1-2 and Table 2, the addition of PBO fibers has an excellent synergistic effect with the modified carbon fiber-hydroxyapatite composite, and the resulting effect is far greater than the sum of the effects of using either material alone. Finally, as can be seen from Example 9 and Table 2, when the weight ratio of the modified carbon fiber-hydroxyapatite composite to PBO fibers is 5:4, the combined effect is particularly excellent.
[0051] As can be seen from Examples 1 and 10-12, and Table 2, pretreatment of PBO fibers before use can further reduce the tensile strength loss rate of the waterproof and breathable membrane, thereby further improving its resistance to thermal expansion. Furthermore, as can be seen from Comparative Example 3 and Table 2, pretreated PBO fibers exhibit better compatibility with modified carbon fiber-hydroxyapatite composites compared to raw PBO fibers.
[0052] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A waterproof self-heating food packaging container, characterized in that, The device includes an outer box, an inner box, and a heating pack. The inner box is sealed and suspended inside the outer box. The heating pack is positioned between the bottom of the inner box and the bottom of the outer box. The inner box has ventilation holes and a waterproof and breathable membrane covering the ventilation holes. The waterproof and breathable membrane is made of raw materials comprising the following parts by weight: 50-70 parts of polyurethane acrylate; 2-4 parts coupling agent; 3-5 parts dispersant; 10-15 parts of filler; 5-10 parts antibacterial agent; 4-7 parts of modified carbon fiber-hydroxyapatite composite; The modified carbon fiber-hydroxyapatite composite was prepared by the following method: S1. Take carbon fiber raw material, heat it to 300-500℃ and keep it for 20-30 minutes. After cooling, soak it in acid solution and alkaline solution in sequence. The soaking temperature is 70-80℃ and the soaking time is 18-24 hours each time. After soaking, wash and dry to obtain pretreated carbon fiber. Deionized water and hydroxyapatite powder are mixed at a weight ratio of 1:(0.4-0.5), and then sodium hexametaphosphate, accounting for 4%-6% of the weight of hydroxyapatite powder, is added. After ball milling, hydroxyapatite slurry is obtained. S2. Immerse the pretreated carbon fiber from step S1 in hydroxyapatite slurry, quickly pull it up and then quickly dry it at 80-90℃. Repeat the above process 4-6 times to obtain the modified carbon fiber-hydroxyapatite composite material. The waterproof and breathable membrane also contains 3-5 parts by weight of PBO fiber in its raw materials; The weight ratio of the modified carbon fiber-hydroxyapatite composite to PBO fiber is 5:
4. The PBO fibers are pretreated before use. The pretreatment steps are as follows: Take PBO fiber raw material, soak it in a 50%-70% methanesulfonic acid solution, maintain it at 50-80℃ for 4-8 hours, wash and dry it, then soak it in a polyphosphoric acid-acetic acid composite solution with a polyphosphoric acid content of 6%-8%, maintain it at 30-40℃ for 3-5 minutes, wash and dry it to obtain pretreated PBO fiber.
2. The waterproof self-heating food packaging container according to claim 1, characterized in that: The coupling agent is one or a combination of several of the following: silane coupling agents, titanate coupling agents, aluminate coupling agents, and phosphate coupling agents.
3. The waterproof self-heating food packaging container according to claim 1, characterized in that: The dispersant is a composition of polyethylene wax and stearate in any weight ratio.
4. The waterproof self-heating food packaging container according to claim 1, characterized in that: The filler is one or a combination of several of the following: alumina, silicon dioxide, calcium carbonate, talc, silica powder, and bentonite.
5. The method for preparing the waterproof self-heating food packaging container according to claim 1, characterized in that: Includes the following steps: (1) Prepare raw materials containing polyurethane acrylate, coupling agent, dispersant, filler, antibacterial agent, modified carbon fiber-hydroxyapatite composite and pretreated PBO fiber according to the formula; (2) After the polyurethane acrylate, coupling agent, dispersant, filler, antibacterial agent, modified carbon fiber-hydroxyapatite composite and pretreated PBO fiber in step (1) are mixed evenly, the mixture is heated, extruded and granulated, and then cast and stretched to obtain a waterproof and breathable membrane. (3) Fix the waterproof and breathable membrane to the inner box with adhesive and cover the ventilation holes. Then assemble the outer box, inner box and heating pack to obtain a waterproof self-heating food packaging box.
Citation Information
Patent Citations
Preparation method of gradient carbon fiber / hydroxyapatite (HA) composite material
CN103693985A
PBO (poly-p-phenylene benzobisoxazole) fiber molecular structure modification method
CN105755803A
Safe self-heating packaging box with high thermal efficiency
CN116062317A
Waterproof breathable film with heat insulation function
CN116852836A