Reaction type polyurethane hot melt adhesive and preparation method thereof

By adding reactive tackifying resin and polyether-type thermoplastic polyester elastomer to reactive polyurethane hot melt adhesive, the problems of low initial bond strength and short open time are solved, achieving high initial bond strength and long open time. It is suitable for fields such as construction, automobiles, electronics, wood processing, bookbinding and food packaging.

CN117866581BActive Publication Date: 2026-11-24GUANGZHOU BAIYUN CHEM IND +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311796417.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2026-11-24
Estimated Expiration
2043-12-25

AI Technical Summary

Technical Problem

Existing reactive polyurethane hot melt adhesives have low initial bond strength and short open time, resulting in unstable bonding performance. Current methods for improving initial bond strength often lead to increased melt viscosity and shortened open time.

Method used

A polyurethane prepolymer is generated by combining a specific reactive tackifying resin with a polyether-type thermoplastic polyester elastomer. This improves initial tack and extends open time. The initial bonding performance is enhanced by adjusting the segment regularity and crystallinity of the polyurethane prepolymer.

Benefits of technology

It achieves high initial bond strength and long open time, has a simple preparation process, is easy to apply in industrial applications, and has excellent overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004627846290000065
    Figure BDA0004627846290000065
  • Figure BDA0004627846290000071
    Figure BDA0004627846290000071
  • Figure BDA0004627846290000081
    Figure BDA0004627846290000081
Patent Text Reader

Abstract

This invention discloses a reactive polyurethane hot melt adhesive and its preparation method. The reactive polyurethane hot melt adhesive is prepared from raw materials comprising the following components, by weight: 20-50 parts crystalline polyester polyol, 10-40 parts liquid polyester polyol, 10-25 parts amorphous polyester polyol, 5-20 parts reactive tackifying resin, 10-30 parts thermoplastic elastomer, 10-20 parts isocyanate, and 0.01-0.2 parts catalyst; the thermoplastic elastomer is a polyether-type thermoplastic polyester elastomer; the reactive tackifying resin is Reagem 5045 and / or Reagem 5006. The reactive polyurethane hot melt adhesive of this invention has advantages such as long open time, high initial tack, and excellent overall performance, and has good market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of hot melt adhesive technology, and in particular to a reactive polyurethane hot melt adhesive and its preparation method. Background Technology

[0002] Reactive polyurethane hot melt adhesives (PUR) mainly refer to polyurethane hot melt adhesives that utilize moisture in the air for cross-linking and curing. They combine the characteristics of ordinary hot melt adhesives and reactive adhesives. Compared with ordinary hot melt adhesives, they have a lower application temperature, higher bonding strength after curing, and better heat resistance, chemical resistance, and durability. They can exhibit good adhesion to substrates such as wood, ceramics, fabrics, metals, glass, plastics, and rubber. In recent years, they have seen rapid development in fields such as construction, automobiles, electronics, wood processing, bookbinding, and food packaging.

[0003] The curing process of reactive polyurethane hot melt adhesives (PUR) consists of two stages. First, after the PUR is melted and applied to the substrate, it cools and solidifies to generate initial bond strength. Then, the -NCO in the system reacts with moisture in the air to achieve the final viscosity strength. However, because moisture in the air penetrates slowly after PUR is applied, the initial bond strength is usually very low, and complete curing often takes several days. To improve the initial bond strength of PUR, the main methods currently used are to increase the crystallinity of the system or add high molecular weight thermoplastic resins. While these methods improve the initial bond strength, they often lead to problems such as increased melt viscosity, shorter open time, and unstable bonding performance of the PUR product. Summary of the Invention

[0004] Based on this, the purpose of the present invention is to provide a reactive polyurethane hot melt adhesive with high initial bond strength and long open time.

[0005] To achieve the above objectives, the present invention includes the following technical solutions.

[0006] A reactive polyurethane hot melt adhesive, by weight, is prepared from raw materials comprising the following components: 20-50 parts of crystalline polyester polyol, 10-40 parts of liquid polyester polyol, 10-25 parts of amorphous polyester polyol, 5-20 parts of reactive tackifying resin, 10-30 parts of thermoplastic elastomer, 10-20 parts of isocyanate, and 0.01-0.2 parts of catalyst.

[0007] The thermoplastic elastomer is a polyether-type thermoplastic polyester elastomer;

[0008] The reactive tackifying resin is Reagem 5045 and / or Reagem 5006.

[0009] In some embodiments, the reactive polyurethane hot melt adhesive is prepared from raw materials comprising the following components in parts by weight: 25-35 parts of crystalline polyester polyol, 10-20 parts of liquid polyester polyol, 10-20 parts of amorphous polyester polyol, 6-15 parts of reactive tackifying resin, 15-25 parts of thermoplastic elastomer, 10-18 parts of isocyanate, and 0.01-0.2 parts of catalyst.

[0010] In some embodiments, the reactive polyurethane hot melt adhesive is prepared from raw materials comprising the following components in parts by weight: 28-32 parts of crystalline polyester polyol, 13-17 parts of liquid polyester polyol, 13-17 parts of amorphous polyester polyol, 6-10 parts of reactive tackifying resin, 18-22 parts of thermoplastic elastomer, 12-16 parts of isocyanate, and 0.05-0.2 parts of catalyst.

[0011] In some embodiments, the reactive polyurethane hot melt adhesive is prepared from raw materials comprising the following components in parts by weight: 29-31 parts of crystalline polyester polyol, 14-16 parts of liquid polyester polyol, 14-16 parts of amorphous polyester polyol, 7-9 parts of reactive tackifying resin, 19-21 parts of thermoplastic elastomer, 15-16 parts of isocyanate, and 0.05-0.15 parts of catalyst.

[0012] In some embodiments, the hydroxyl value of the crystalline polyester polyol is 10-112 mgKOH / g, preferably 18-60 mgKOH / g, and more preferably 27-34 mgKOH / g.

[0013] In some embodiments, the crystalline polyester polyol is 7360 and / or 7380.

[0014] In some embodiments, the hydroxyl value of the liquid polyester polyol is 10-112 mgKOH / g, preferably 18-60 mgKOH / g, and more preferably 18-34 mgKOH / g.

[0015] In some embodiments, the liquid polyester polyol is 7230 and / or 7250.

[0016] In some embodiments, the hydroxyl value of the amorphous polyester polyol is 10-112 mgKOH / g, preferably 18-60 mgKOH / g, and more preferably 31-46 mgKOH / g.

[0017] In some embodiments, the amorphous polyester polyol is 7130 and / or 7150.

[0018] In some embodiments, the thermoplastic elastomer is 3078 and / or 4056.

[0019] In some embodiments, the isocyanate is at least one of 4,4'-diphenylmethane diisocyanate (MDI), carbodiimide-modified MDI, and MDI-50.

[0020] In some embodiments, the catalyst is at least one of dibutyltin dilaurate (DBTDL), triethylenediamine, and dimorpholinodiethyl ether (DMDEE).

[0021] The present invention also provides a method for preparing the aforementioned reactive polyurethane hot melt adhesive, comprising the following steps:

[0022] (1) The crystalline polyester polyol, liquid polyester polyol, amorphous polyester polyol, reactive tackifying resin and thermoplastic elastomer are put into a reaction vessel and heated to 170°C to 190°C. Vacuum dehydration is carried out for 60 to 180 minutes under stirring.

[0023] (2) Cool down to 100℃~140℃, add the isocyanate, and stir and react for 60 minutes~180 minutes under inert gas protection;

[0024] (3) Add the catalyst and stir and mix at 100℃~140℃ for 20 minutes~40 minutes under inert gas protection;

[0025] (4) Maintain a constant temperature of 100℃~140℃, evacuate until no bubbles appear, and then discharge the material.

[0026] In some embodiments, the method for preparing the reactive polyurethane hot melt adhesive includes the following steps:

[0027] (1) The crystalline polyester polyol, liquid polyester polyol, amorphous polyester polyol, reactive tackifying resin and thermoplastic elastomer are put into a reaction vessel and heated to 175℃~185℃. Vacuum dehydration is carried out for 120 minutes~180 minutes under stirring, and the vacuum degree is -0.095~0.05MPa.

[0028] (2) Cool down to 110℃~130℃, add the isocyanate, and stir and react for 100 minutes~150 minutes under inert gas protection;

[0029] (3) Add the catalyst and stir and mix at 110℃~130℃ for 25 minutes~35 minutes under inert gas protection;

[0030] (4) Maintain a constant temperature of 110℃~130℃, evacuate until no bubbles appear, and then discharge the material.

[0031] The present invention relates to a long-open-time, high-initial-tack reactive polyurethane hot melt adhesive (PUR) with the addition of specific reactive tackifying resins (Reagem 5045 and / or Reagem 5006). These resins react with polyisoesters to form a polyurethane prepolymer. Upon cooling, the prepolymer reacts with crystalline polyester polyols, amorphous polyester polyols, and thermoplastic elastomers to rapidly solidify, thereby increasing the initial tack of the PUR. Simultaneously, the introduction of this specific reactive tackifying resin into the polyurethane prepolymer backbone affects the regularity of the PUR chain segments, reducing the crystallinity of the PUR system and thus extending the open-time of the PUR. Furthermore, the synergistic effect of this specific reactive tackifying resin with polyether-type thermoplastic polyester elastomers can further improve the initial tack of the PUR. Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. The present invention, through the reasonable combination of the above components in a certain ratio, produces a reactive polyurethane hot melt adhesive with advantages such as long open time, high initial tack, and excellent comprehensive performance, and has good market prospects.

[0033] 2. The preparation process of the reactive polyurethane hot melt adhesive of the present invention is simple, easy to operate, and easy to industrialize. Detailed Implementation

[0034] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments are merely illustrative of the present invention and should not be construed as limiting the invention.

[0035] Unless otherwise defined, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to limit the invention.

[0036] The terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion. For example, a process, method, apparatus, product, or device that includes a series of steps is not limited to the steps or modules listed, but may optionally include steps not listed, or may optionally include other steps inherent to such process, method, product, or device.

[0037] In this invention, "multiple" refers to two or more. "And / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A alone, A and B simultaneously, or B alone. The character " / " generally indicates that the preceding and following related objects have an "or" relationship.

[0038] The viscosity mentioned in this invention refers to the viscosity tested at 25°C.

[0039] The following are specific examples.

[0040] The liquid polyester polyol used in the embodiments of this invention was purchased from Evonik. The 7200 series is detailed below:

[0041] 7230, with a hydroxyl value of 27–34 mg KOH / g;

[0042] 7250, with a hydroxyl value of 18-24 mgKOH / g.

[0043] The crystalline polyester polyol used in the embodiments of this invention was purchased from Evonik. The 7300 series is detailed below:

[0044] 7360, with a hydroxyl value of 27–34 mg KOH / g;

[0045] 7380, with a hydroxyl value of 27-34 mgKOH / g.

[0046] The amorphous polyester polyols used in these embodiments were purchased from Evonik Industries. The 7100 series is detailed below:

[0047] 7130, with a hydroxyl value of 31 mg KOH / g to 39 mg KOH / g;

[0048] 7150, with a hydroxyl value of 38mgKOH / g to 46mgKOH / g.

[0049] Thermoplastic elastomers: 3078 4056, purchased from DuPont.

[0050] Reactive tackifying resins: Reagem 5045, Reagem 5006, and Dertophene T 115 were purchased from DRT, France.

[0051] The hydroxyl value of Reagem 5045 is 35mgKOH / g to 45mgKOH / g, the hydroxyl value of Reagem 5006 is 75mgKOH / g, and the hydroxyl value of Dertophene T 115 is 40mgKOH / g to 60mgKOH / g.

[0052] Isocyanates: 2379, purchased from Huntsman Corporation, USA.

[0053] The remaining raw material components are all commercially available products.

[0054] The raw materials used in the embodiments and comparative examples of this invention are shown in Table 1 below:

[0055] Table 1: Distribution ratios (parts by weight) of each group in each embodiment and comparative example

[0056]

[0057]

[0058] The reactive polyurethane hot melt adhesives of Examples 1-3 above were prepared using the following method, with the only difference being the changes in raw materials and their amounts as shown in Table 1:

[0059] (1) Add crystalline polyester polyol, liquid polyester polyol, amorphous polyester polyol, reactive tackifying resin and thermoplastic elastomer into a reactor, heat to 180°C, and vacuum dehydrate for 150 minutes with stirring. The vacuum degree is -0.09MPa.

[0060] (2) Cool down to 120°C, add isocyanate, and stir the reaction for 120 minutes under N2 protection;

[0061] (3) Add the catalyst and stir and mix at 120°C for 30 minutes under N2 protection;

[0062] (4) Maintain a constant temperature of 120℃, evacuate until no bubbles appear, and then discharge the material.

[0063] The preparation method of the reactive polyurethane hot melt adhesive provided in Comparative Examples 1-5 differs from that in the above embodiments in that the corresponding steps are omitted when no corresponding components are added; the other steps are the same as in the embodiments.

[0064] Performance testing: The reactive polyurethane hot melt adhesives prepared in Examples 1-3 and Comparative Examples 1-5 were tested for their open time according to HG / T3716-2003. The initial bond strength (tensile shear strength tested after 10 min, 20 min, and 30 min of sample placement) and final bond strength (tensile shear strength tested after 7 days of moisture curing at 25℃ / 50%RH) were tested according to GB / T 7124-2008.

[0065] The test results are shown in Table 2.

[0066] Table 2. Performance test results of reactive polyurethane hot melt adhesives in Examples 1-3 and Comparative Examples 1-5

[0067]

[0068] Note: During the open time, the reactive polyurethane hot melt adhesive has no initial tack to facilitate construction. After the open time, initial tack is formed quickly. In Example 3 and Comparative Example 2, the initial bond strength is very small at 20 minutes because the open time is greater than 20 minutes.

[0069] As can be seen from the performance comparison of Examples 1-3 and Comparative Examples 1-4 in Table 2, the reactive polyurethane hot melt adhesive (examples) prepared by adding both thermoplastic elastomer and reactive tackifying resin has a significantly improved initial bond strength compared to the comparative examples. At the same time, the open time of Examples 1-3 with added reactive tackifying resin is significantly longer than that of Comparative Examples 3 and 4 without added reactive tackifying resin.

[0070] Compared with Comparative Examples 3 and 4, which did not contain reactive tackifying resin, Comparative Example 5, which added reactive tackifying resin Dertophene T 115, showed little change in open time and initial bond strength.

[0071] Therefore, the reactive polyurethane hot melt adhesive prepared by this invention has the characteristics of long open time, high initial bond strength, and excellent overall performance. Among them, the reactive polyurethane hot melt adhesive of Example 3 has the best overall performance.

[0072] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0073] The above-described embodiments are merely examples of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent.

[0074] The invention is not limited to any particular type of invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the inventive concept, and these all fall within the scope of protection of this invention. Therefore, the scope of protection of this patent should be determined by the appended claims.

Claims

1. A reactive polyurethane hot melt adhesive, characterized in that, It is prepared from the following raw materials in parts by weight: 20-50 parts of crystalline polyester polyol, 10-40 parts of liquid polyester polyol, 10-25 parts of amorphous polyester polyol, 5-20 parts of reactive tackifying resin, 10-30 parts of thermoplastic elastomer, 10-20 parts of isocyanate, and 0.01-0.2 parts of catalyst. The reactive tackifying resin is Reagem 5045 and / or Reagem 5006; The thermoplastic elastomer is Hytrel. ® 3078 and / or Hytrel ® 4056.

2. The reactive polyurethane hot melt adhesive according to claim 1, characterized in that, It is prepared by weight from the following raw materials: 25-35 parts of crystalline polyester polyol, 10-20 parts of liquid polyester polyol, 10-20 parts of amorphous polyester polyol, 6-15 parts of reactive tackifying resin, 15-25 parts of thermoplastic elastomer, 10-18 parts of isocyanate, and 0.01-0.2 parts of catalyst.

3. The reactive polyurethane hot melt adhesive according to claim 2, characterized in that, It is prepared by weight from the following raw materials: 28-32 parts of crystalline polyester polyol, 13-17 parts of liquid polyester polyol, 13-17 parts of amorphous polyester polyol, 6-10 parts of reactive tackifying resin, 18-22 parts of thermoplastic elastomer, 12-16 parts of isocyanate, and 0.05-0.2 parts of catalyst.

4. The reactive polyurethane hot melt adhesive according to claim 3, characterized in that, It is prepared from the following raw materials in parts by weight: 29-31 parts of crystalline polyester polyol, 14-16 parts of liquid polyester polyol, 14-16 parts of amorphous polyester polyol, 7-9 parts of reactive tackifying resin, 19-21 parts of thermoplastic elastomer, 15-16 parts of isocyanate, and 0.05-0.15 parts of catalyst.

5. The reactive polyurethane hot melt adhesive according to any one of claims 1-4, characterized in that, The hydroxyl value of the crystalline polyester polyol is 10-112 mgKOH / g.

6. The reactive polyurethane hot melt adhesive according to claim 5, characterized in that, The hydroxyl value of the crystalline polyester polyol is 18-60 mg KOH / g.

7. The reactive polyurethane hot melt adhesive according to claim 6, characterized in that, The hydroxyl value of the crystalline polyester polyol is 27-34 mgKOH / g.

8. The reactive polyurethane hot melt adhesive according to any one of claims 1-4, characterized in that, The crystalline polyester polyol is Dynacoll. ® 7360 and / or Dynacoll ® 7380.

9. The reactive polyurethane hot melt adhesive according to any one of claims 1-4, characterized in that, The hydroxyl value of the liquid polyester polyol is 10-112 mgKOH / g.

10. The reactive polyurethane hot melt adhesive according to claim 9, characterized in that, The hydroxyl value of the liquid polyester polyol is 18-60 mg KOH / g.

11. The reactive polyurethane hot melt adhesive according to claim 10, characterized in that, The hydroxyl value of the liquid polyester polyol is 18-34 mgKOH / g.

12. The reactive polyurethane hot melt adhesive according to any one of claims 1-4, characterized in that, The liquid polyester polyol is Dynacoll. ® 7230 and / or Dynacoll ® 7250.

13. The reactive polyurethane hot melt adhesive according to any one of claims 1-4, characterized in that, The hydroxyl value of the amorphous polyester polyol is 10-112 mgKOH / g.

14. The reactive polyurethane hot melt adhesive according to claim 13, characterized in that, The hydroxyl value of the amorphous polyester polyol is 18-60 mg KOH / g.

15. The reactive polyurethane hot melt adhesive according to claim 14, characterized in that, The hydroxyl value of the amorphous polyester polyol is 31~46 mgKOH / g.

16. The reactive polyurethane hot melt adhesive according to any one of claims 1-4, characterized in that, The amorphous polyester polyol is Dynacoll. ® 7130 and / or Dynacoll ® 7150.

17. The reactive polyurethane hot melt adhesive according to any one of claims 1-4, characterized in that, The isocyanate is at least one selected from 4,4'-diphenylmethane diisocyanate, carbodiimide-modified MDI, and MDI-50; and / or, The catalyst is at least one of dibutyltin dilaurate, triethylenediamine, and dimorpholinodiethyl ether.

18. A method for preparing a reactive polyurethane hot melt adhesive according to any one of claims 1-17, characterized in that, Includes the following steps: (1) The crystalline polyester polyol, liquid polyester polyol, amorphous polyester polyol, reactive tackifying resin and thermoplastic elastomer are put into a reaction vessel and heated to 170°C to 190°C. Vacuum dehydration is carried out for 60 to 180 minutes under stirring. (2) Cool down to 100℃~140℃, add the isocyanate, and stir and react for 60 minutes~180 minutes under inert gas protection; (3) Add the catalyst and stir and mix at 100℃~140℃ for 20 minutes~40 minutes under inert gas protection; (4) Maintain a constant temperature of 100℃~140℃, evacuate until no bubbles appear, and then discharge the material.

19. The method for preparing the reactive polyurethane hot melt adhesive according to claim 18, characterized in that, Includes the following steps: (1) The crystalline polyester polyol, liquid polyester polyol, amorphous polyester polyol, reactive tackifying resin and thermoplastic elastomer are put into a reaction vessel and heated to 175℃~185℃. Vacuum dehydration is carried out for 120 minutes~180 minutes under stirring, and the vacuum degree is -0.095~0.05MPa. (2) Cool down to 110℃~130℃, add the isocyanate, and stir and react for 100 minutes~150 minutes under inert gas protection; (3) Add the catalyst and stir and mix at 110℃~130℃ for 25 minutes~35 minutes under inert gas protection; (4) Maintain a constant temperature of 110℃~130℃, evacuate until no bubbles appear, and then discharge the material.

Citation Information

Patent Citations

  • Reactive polyurethane hot melt adhesive for edge folding of soft package lithium battery and preparation method of reactive polyurethane hot melt adhesive