A method for dephosphorization under high temperature peroxidation condition in the final stage of a converter
By adding magnesite and iron-carbon balls at the end of the converter process, combined with furnace shaking and tapping methods, the problem of difficult dephosphorization under high-temperature peroxidation conditions was solved, achieving effective phosphorus removal and temperature reduction, and improving the dephosphorization success rate.
Patent Information
- Application Number
- CN202311779130.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-22
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-22
AI Technical Summary
In the process of converter steelmaking, dephosphorization is difficult under high-temperature peroxidation conditions, and existing technologies are unable to effectively address the problem of excessive phosphorus content.
Magnesite and iron-carbon balls are added at the end of the converter process. Combined with the furnace shaking operation and steel tapping method, the temperature drop effect of magnesite and the carbon oxidation reaction of iron-carbon balls generate CO gas to remove heat. Dephosphorization is carried out in conjunction with the use of covered ash.
Effective dephosphorization was achieved under high-temperature peroxidation conditions, meeting the internal control requirements of steel grades and improving the dephosphorization success rate. High-efficiency phosphorus removal was achieved by lowering the temperature and providing suitable iron oxide conditions.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of converter steelmaking technology, and more particularly to a dephosphorization method under high-temperature peroxidation conditions at the end of the converter process. Background Technology
[0002] Generally, phosphorus is a harmful element in steel. For steel grades requiring high low-temperature performance and fatigue resistance, in addition to very low sulfur content and other impurity elements, phosphorus must also be controlled at very low levels. Because the blast furnace ironmaking process is a reducing atmosphere, its dephosphorization capacity is poor, making dephosphorization one of the important tasks in the steelmaking process.
[0003] In the thermodynamics of metallurgy, dephosphorization reactions require reaction conditions such as low temperature, high oxidation, and high basicity. Kinetic conditions include enhanced molten pool stirring, increased reaction area, and ensured slag fluidity. When considering temperature, low temperature is favorable for dephosphorization. It should be noted that increasing the molten pool temperature reduces the phosphorus distribution ratio, hindering phosphorus transfer from the metal to the slag. However, higher temperatures reduce slag viscosity and accelerate lime dissolution, thus facilitating phosphorus transfer from the metal to the slag. Theoretical research indicates that the most effective dephosphorization occurs within an optimal temperature range of 1450–1500℃. This necessitates employing different operating procedures based on the temperature of the molten iron during the initial stages of smelting. When considering basicity, practical experience shows that as long as the basicity of the slag reaches around 3.0, the slag is fully smelted and contains an appropriate amount of FeO, dephosphorization of general steel grades is not a problem. When considering the effect of FeO, if FeO is too low, the lime cannot melt well, obviously dephosphorization will not be possible. However, if FeO is too high, it will dilute the dephosphorization effect of CaO. When the basicity is between 2.5 and 4.0, increasing FeO is beneficial to dephosphorization, but excessively high FeO will reduce the dephosphorization capacity.
[0004] In actual production, fully considering dephosphorization conditions is fundamental to flexibly managing the final phosphorus content of molten steel. When converters are smelted under normal conditions, dephosphorization is generally not difficult, and steel mills will adopt various dephosphorization measures according to their own conditions. However, in some abnormal heats, due to charging blockages or raw material problems, high phosphorus levels occur at the smelting endpoint. These situations are often accompanied by high temperatures exceeding 1700℃ and oxidation phenomena, making the converter endpoint unsuitable for dephosphorization. Steel mills urgently need to develop a dephosphorization method that can achieve a high success rate under such high-temperature and oxidizing conditions.
[0005] The paper "Application Practice of Iron-Carbon Composite Pellets in Converter Steelmaking" provides a detailed introduction to the use of iron-carbon pellets in converters, elaborating on four ways of adding them: before iron addition, at the beginning of smelting, during the process of re-drying, and at the end. The paper argues that the optimal method of use is at the beginning of the converter process. While using them in the later stages of the converter process can lower the temperature, it must be combined with a suitable bottom-blowing process to reduce some of the ferrite. Summary of the Invention
[0006] The purpose of this invention is to provide a dephosphorization method under high-temperature peroxidation conditions at the end of converter smelting, in order to overcome the predicament of high phosphorus levels at the end of converter smelting that cannot be addressed.
[0007] To achieve the above objectives, the present invention provides the following technical solution: A dephosphorization method under high-temperature peroxidation conditions at the end of a converter process, specifically including the following: When the converter tapping temperature is 1700~1720℃, magnesite and iron-carbon balls are added to the converter. The amount of magnesite added is 9~11kg / t steel, and the amount of iron-carbon balls added is 14~16kg / t steel. After adding, the furnace is shaken 5~10 times. When the tapping temperature of the converter is 1680~1700℃ (excluding 1700℃), magnesite and iron-carbon balls are added to the converter. The amount of magnesite added is 6~8 kg / t steel, and the amount of iron-carbon balls added is 9~11 kg / t steel. After adding, the converter is shaken 5~10 times. When the converter tapping temperature is 1680~1700℃, iron-carbon balls are added to the converter. The amount of iron-carbon balls added is 1~3kg / t steel. Depending on the type of steel, boiling tapping or killed tapping is selected. After tapping, lime from the cover pot is added to the ladle. The amount of lime from the cover pot added is 2~3kg / t steel.
[0008] The iron-carbon spheres will be made with the following mass percentages: C: 5%~15%, S: ≤0.13%, TFe: 50%~60%, FeO: 30%~40%, MFe: ≤1%, P: ≤0.03%, and the diameter of the iron-carbon spheres will range from 20 to 60 mm.
[0009] Magnesite will be produced using the following mass percentages: CaO: ≤2%, SiO₂ 2: ≤5%, MgO: ≥40%, magnesite diameter range is 5~80mm.
[0010] Compared with the prior art, the beneficial effects of the present invention are: 1. Used for dephosphorization under high-temperature over-oxidation conditions in the later stage of converter. At the end of the converter's high-temperature over-oxidation, it often means phosphorus reversion in the molten steel. The method of adding magnesite and iron-carbon balls and then shaking the furnace not only utilizes the physical temperature drop of the two materials, but also the high carbon content of the iron-carbon balls reacts with iron oxide to form CO gas, which continuously removes heat, ultimately satisfying dephosphorization and achieving temperature drop. This provides an important reference for rescuing phosphorus-reverting steel grades and low-phosphorus steel grades. 2. Using steel mill-supplied iron-carbon balls and magnesite together can improve the success rate of dephosphorization under difficult dephosphorization conditions. Using iron-carbon balls can not only increase the yield of metallic iron, but also play a role in cooling and providing (FeO). Magnesite has a significant temperature-lowering effect. When used in conjunction with iron-carbon balls, the thermodynamic and kinetic conditions of dephosphorization can be fully utilized to achieve the purpose of dephosphorization under unfavorable high-temperature conditions. Detailed Implementation
[0011] The present invention will now be described in detail, but it should be noted that the implementation of the present invention is not limited to the following embodiments.
[0012] A dephosphorization method under high-temperature peroxidation conditions at the end of a converter process, specifically including the following: 1) When the converter tapping temperature is 1680~1700℃ (excluding 1700℃), add magnesite and iron-carbon balls from the high-level silo into the converter. The amount of magnesite added is 6~8 kg / t steel, and the amount of iron-carbon balls added is 9~11 kg / t steel. After adding, shake the furnace 5~10 times. Measure the temperature again. When the converter tapping temperature is 1680~1700℃, add iron-carbon balls into the converter. The amount of iron-carbon balls added is 1~3 kg / t steel. Select boiling tapping or killed tapping according to the type of steel. After tapping, add lime from the cover pot to the ladle. The amount of lime added from the cover pot is 2~3 kg / t steel.
[0013] 2) When the converter tapping temperature is 1700~1720℃, add magnesite and iron-carbon balls from the high-level silo into the converter. The amount of magnesite added is 9~11 kg / t steel, and the amount of iron-carbon balls added is 14~16 kg / t steel. After adding, shake the furnace 5~10 times. When the converter tapping temperature is 1680~1700℃, add iron-carbon balls into the converter. The amount of iron-carbon balls added is 1~3 kg / t steel. Select boiling tapping or killed tapping according to the type of steel. After tapping, add lime from the cover pot into the ladle. The amount of lime added from the cover pot is 2~3 kg / t steel.
[0014] The iron-carbon spheres will be made with the following mass percentages: C: 5%~15%, S: ≤0.13%, TFe: 50%~60%, FeO: 30%~40%, MFe: ≤1%, P: ≤0.03%, and the diameter of the iron-carbon spheres will range from 20 to 60 mm.
[0015] Magnesite will be produced using the following mass percentages: CaO: ≤2%, SiO₂ 2: ≤5%, MgO: ≥40%, magnesite diameter range is 5~80mm.
[0016] The following embodiments are implemented based on the technical solution of the present invention, providing detailed implementation methods and specific operation processes. However, the scope of protection of the present invention is not limited to the following embodiments. Unless otherwise specified, the methods used in the following embodiments are conventional methods.
[0017]
Example 1
[0018]
Example 2
[0019]
Example 3
[0020] The compositions of magnesite and iron-carbon spheres are shown in Tables 1 and 2.
[0021] Table 1 Magnesite composition (wt, %) of the examples
[0022] Table 2. Composition of iron-carbon spheres in the examples (wt, %)
[0023] This invention is used for dephosphorization under high-temperature over-oxidation conditions in the later stage of converter. At the end of the converter's high-temperature over-oxidation, it often means phosphorus reversion in the molten steel. By adding magnesite and iron-carbon balls and then shaking the furnace, not only is the physical temperature drop of the two materials utilized, but the high carbon content of the iron-carbon balls reacts with iron oxide to form CO gas, which continuously removes heat, ultimately achieving dephosphorization while also reducing the temperature. This provides an important reference for rescuing phosphorus-reverting steel grades and steel grades with low phosphorus requirements. Using iron-carbon balls and magnesite supplied by the steel plant together improves the success rate of dephosphorization under difficult dephosphorization conditions. The use of iron-carbon balls can not only increase the yield of metallic iron, but also play a role in cooling and providing (FeO), while the temperature-reducing effect of magnesite is significant. When used in conjunction with iron-carbon balls, the thermodynamic and kinetic conditions of dephosphorization can be fully utilized to achieve the purpose of dephosphorization under unfavorable high-temperature conditions.
Claims
1. A dephosphorization method under high-temperature peroxidation conditions at the end of a converter process, characterized in that, Specifically, it includes the following: When the converter tapping temperature is 1700~1720℃, magnesite and iron-carbon balls are added to the converter. The amount of magnesite added is 9~11kg / t steel, and the amount of iron-carbon balls added is 14~16kg / t steel. After adding, the furnace is shaken 5~10 times. When the converter tapping temperature is 1680~1700℃ (excluding 1700℃), magnesite and iron-carbon balls are added to the converter. The amount of magnesite added is 6~8 kg / t steel, and the amount of iron-carbon balls added is 9~11 kg / t steel. After adding, the furnace is shaken 5~10 times. Temperature was measured again. When the converter tapping temperature was 1680~1700℃, iron-carbon balls were added to the converter. The amount of iron-carbon balls added was 1~3 kg / t steel. Depending on the type of steel, boiling tapping or killed tapping was selected. After tapping, lime from a covered pot was added to the ladle. The amount of lime from the covered pot was 2~3 kg / t steel. The iron-carbon spheres have the following mass percentages: C: 5%~15%, S: ≤0.13%, TFe: 50%~60%, FeO: 30%~40%, MFe: ≤1%, P: ≤0.03%, and the diameter of the iron-carbon spheres ranges from 20 to 60 mm.
2. The dephosphorization method under high-temperature peroxidation conditions at the end of a converter process according to claim 1, characterized in that, The magnesite described herein is as follows (by mass percentage): CaO: ≤2%, SiO₂: ≤2%. 2: ≤5%, MgO: ≥40%, magnesite diameter range is 5~80mm.
Citation Information
Patent Citations
Smelting method of ultralow manganese steel
CN108998614A
Method of controlling green environment-friendly smelting of converter
CN109913612A
Iron-carbon sphere temperature regulating agent for converter smelting and preparation method of iron-carbon sphere temperature regulating agent