A heat treatment method for improving the impact performance of the core of a large-section low-alloy steel forge piece

By employing a heat treatment process of normalizing, quenching, and tempering, combined with the heat preservation control of the load block and thermocouple, the problem of poor core impact performance of large-section low-alloy steel forgings was solved, achieving low-cost and high-efficiency performance improvement.

CN117867222BActive Publication Date: 2026-11-20WUXI TURBINE BLADE
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311752158.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-19
Publication Date
2026-11-20
Estimated Expiration
2043-12-19

AI Technical Summary

Technical Problem

Large-section low-alloy steel forgings have poor core impact resistance, and existing heat treatment methods suffer from high cost, long cycle, and unstable performance.

Method used

The heat treatment process of normalizing, quenching and tempering is adopted, and the holding time is controlled by load blocks and thermocouples to ensure the uniformity and performance consistency of the forgings. The process includes forging, annealing, machining, quenching and tempering.

Benefits of technology

It improves the core impact performance of large-section low-alloy steel forgings, reduces the difference in tensile strength between the core and the surface, lowers production costs, and is suitable for low-cost mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004616141840000141
    Figure BDA0004616141840000141
  • Figure BDA0004616141840000151
    Figure BDA0004616141840000151
  • Figure BDA0004616141840000152
    Figure BDA0004616141840000152
Patent Text Reader

Abstract

The application provides a heat treatment method for improving the impact performance of a core part of a large-section low-alloy steel forge piece, and the heat treatment method comprises the following steps: (1) forging a low-alloy steel forge piece, and then sequentially performing annealing treatment and mechanical processing to obtain a primary forge piece; (2) mixing a negative load block with the primary forge piece obtained in step (1), and then sequentially performing quenching treatment and tempering treatment. The application provides a heat treatment process method of directly adopting "normalizing + quenching + tempering", and the process method can obtain a forge piece with a core-surface tensile strength difference within 40 MPa and high core impact performance, and has great practical value for low-cost and batch production of large-section low-alloy steel forge pieces.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of materials science and technology, and relates to a heat treatment method for low alloy structural steel forgings, and more particularly to a heat treatment method for improving the core impact performance of large cross-section low alloy steel forgings. Background Technology

[0002] The rapid development of wind power, nuclear power, and aerospace industries has spurred the development of large forgings, especially cost-effective low-alloy steel forgings. These forgings have effective thicknesses ranging from 100mm to 500mm, and even exceeding 600mm. Large forgings and related industries (including rings with diameters over 500mm and thick-walled seamless steel pipes) represent the highest level of forging, presenting significant challenges. Production is typically characterized by small batches, multiple varieties, and multiple production runs. Due to the small quantity of each variety, there is no complete, mature, and readily applicable production process. In most cases, producing each forging or part involves a process trial and innovation. Furthermore, the poor hardenability of low-alloy steel forgings often results in poor core impact toughness, failing to meet standard requirements. To improve core impact toughness, some strength is sacrificed through repeated heat treatment, but a common problem is that core impact toughness fails to improve significantly while surface strength decreases markedly, ultimately leading to the scrapping of the forging.

[0003] CN 113462956A discloses a large-section, high-hardenability, high-strength medium-manganese forged steel and its preparation method. The method disclosed is to improve the hardenability of large-section forgings by optimizing the alloy composition and content. However, for nuclear power and aerospace products with strict quality control requirements, the control of alloy composition and content is very strict, and it is difficult to adjust the alloy composition in actual production.

[0004] CN 104164548A discloses a heat treatment process for thick cross-section low-carbon low-alloy steel castings and forgings. Specifically, it discloses adding an annealing process and an intermediate heat treatment process between traditional quenching and tempering, thereby improving the core toughness by adjusting the content and size of the core microstructure in the thick cross-section. This process can improve core toughness, but the technical standards for large forgings used in nuclear power and aerospace have clear requirements for heat treatment procedures. Under the technical standard of quenching and tempering, quality control does not allow the addition of other heat treatment processes. On the other hand, the process provided by this patent requires two additional heat treatment processes, resulting in a longer production cycle and higher process costs. For low-alloy large forgings with low-cost advantages, this significantly increases production costs. Finally, the method provided by this patent also has a detail that is not specified at the operational level: the heating rate of the heat treatment furnace and the quantity of forgings loaded into the furnace are not specified. The lack of specification for these two factors leads to significant differences in the holding time after the forgings reach the actual required temperature in the furnace, resulting in large performance differences between batches and other quality risks. In particular, there is a risk of large differences in core and surface strength due to long surface holding time and short core holding time. Summary of the Invention

[0005] To address the shortcomings of existing technologies regarding the poor core impact performance of large-section low-alloy steel forgings, the present invention aims to provide a heat treatment method for improving the core impact performance of large-section low-alloy steel forgings. The method provided by the present invention can obtain forgings with a core-to-surface tensile strength difference within 40 MPa and high core impact performance, which has significant practical value for low-cost, mass production of large-section low-alloy steel forgings.

[0006] To achieve this objective, the present invention adopts the following technical solution:

[0007] This invention provides a heat treatment method for improving the core impact performance of large-section low-alloy steel forgings, the heat treatment method comprising the following steps:

[0008] (1) The low alloy steel forging is forged, and then annealed and machined in sequence to obtain a primary forging;

[0009] (2) Mix the load block and the first forging obtained in step (1), and then perform quenching and tempering treatment in sequence.

[0010] This invention provides a heat treatment process that directly employs "normalizing + quenching + tempering". This process can produce forgings with a core-to-surface tensile strength difference of less than 40 MPa and high core impact performance. It has significant practical value for low-cost, mass production of large-section low-alloy steel forgings.

[0011] As a preferred technical solution of the present invention, the low alloy steel forging in step (1) includes Cr-Mo series steel with an alloy element content of no more than 5wt%.

[0012] Preferably, the C content in the Cr-Mo series steel is 0.2 to 0.4 wt%, for example, it can be 0.2 wt%, 0.24 wt%, 0.28 wt%, 0.32 wt%, 0.36 wt%, or 0.4 wt%, but is not limited to the listed values; other unlisted values ​​within the range are also applicable. The Ni content is ≤0.5 wt%, for example, it can be 0.5 wt%, 0.4 wt%, 0.3 wt%, 0.2 wt%, or 0.1 wt%, but is not limited to the listed values; other unlisted values ​​within the range are also applicable.

[0013] It is worth noting that the alloying elements in the Cr-Mo steel preparation method of the present invention include Mn, Ni, V and Al, and their content does not exceed 5wt%, for example, it can be 0.5wt%, 0.4wt%, 0.3wt%, 0.2wt% or 0.1wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0014] As a preferred technical solution of the present invention, the forging temperature in step (1) is 1090 to 1110°C, for example, it can be 1090°C, 1092°C, 1094°C, 1096°C, 1098°C, 1100°C or 1110°C, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0015] Preferably, the deformation amount of the forging in step (1) is 30% to 70%, for example, it can be 30%, 40%, 50%, 60% or 70%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0016] The present invention uses forging to ensure that the low alloy forging has a finer initial grain size.

[0017] As a preferred technical solution of the present invention, the annealing temperature in step (1) is 690 to 750°C, for example, it can be 690°C, 694°C, 698°C, 702°C, 706°C, 710°C, 720°C, 730°C, 740°C or 750°C, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0018] Preferably, the holding time for the annealing treatment in step (1) is ≥40 min, for example, it can be 40 min, 44 min, 48 min, 52 min, 56 min or 60 min, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0019] Preferably, the holding time for the annealing treatment in step (1) is the effective thickness of the low alloy steel forging × (2~3) min / mm, for example, it can be the effective thickness of the low alloy steel forging × 2 min / mm, the effective thickness of the low alloy steel forging × 2.4 min / mm, the effective thickness of the low alloy steel forging × 2.8 min / mm or the effective thickness of the low alloy steel forging × 3 min / mm, but it is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0020] The annealing treatment described in this invention aims to eliminate forging stress and prepare for machining before quenching. However, excessively high annealing temperatures can lead to coarse grains or the re-generation of internal stress due to excessive supercooling during cooling after heating. Conversely, excessively low temperatures can result in poor stress relief or inadequate microstructure adjustment, failing to provide sufficient microstructure preparation for quenching. Furthermore, excessively short holding times can lead to insufficient annealing, retaining forging stress and increasing the risk of cracking during machining.

[0021] Preferably, the effective thickness of the forging in step (1) is ≤400mm, for example, it can be 400mm, 390mm, 380mm, 370mm, 360mm, 350mm, 340mm, 330mm or 320mm, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0022] Preferably, the fillet radius at the corner of the forging in step (1) is ≥5mm, for example, it can be 5mm, 6mm, 7mm, 8mm, 9mm or 10mm, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0023] This invention uses machining to reduce the effective thickness of a single forging to within 400mm and to round the sharp edges and corners of the forging to a radius of not less than R5mm to prevent cracking during quenching and cooling. If the effective thickness of the single forging is too large, it will lead to a significant difference between the core and surface of the material during quenching, making it difficult to significantly improve the core impact of the final product.

[0024] As a preferred technical solution of the present invention, the effective thickness of the load block and the primary forging in step (2) is the same.

[0025] Preferably, the load block is provided with blind holes for mounting thermocouples.

[0026] Preferably, the thermocouple includes a type K thermocouple or a type N thermocouple; the depth of the blind hole is half the effective thickness of the forging.

[0027] Preferably, the extension line of the thermocouple is connected to a display instrument for calculating the holding time of quenching and tempering treatments.

[0028] Preferably, the load block comprises low alloy steel.

[0029] Preferably, the low alloy steel includes any one of 45 steel, 35 steel, or 30 steel.

[0030] It is worth noting that by using the load coupler of the load block to control the holding time of quenching and tempering, this invention can ensure the rigor of the holding time during heat treatment and solve the problem of large differences in core and surface strength of low alloy forgings due to poor hardenability.

[0031] As a preferred technical solution of the present invention, the quenching process in step (2) adopts a stepped heating process, which includes sequential quenching at a first temperature, quenching at a second temperature, and water cooling.

[0032] Preferably, the quenching temperature of the first temperature is 840 to 860°C, for example, it can be 840°C, 844°C, 848°C, 852°C, 856°C or 860°C, but is not limited to the listed values. Other values ​​not listed within the range are also applicable.

[0033] Preferably, the holding time for quenching at the first temperature is ≥30 min, for example, it can be 30 min, 32 min, 34 min, 36 min, 38 min or 40 min, but is not limited to the listed values. Other values ​​not listed within the range are also applicable.

[0034] Preferably, the holding time for quenching at the first temperature is the effective thickness of the forging in one pass × (1~1.5) min / mm, for example, it can be the effective thickness of the forging in one pass × 1 min / mm, the effective thickness of the forging in one pass × 1.2 min / mm, the effective thickness of the forging in one pass × 1.4 min / mm or the effective thickness of the forging in one pass × 1.5 min / mm, but it is not limited to the listed values. Other values ​​not listed within the range are also applicable.

[0035] As a preferred embodiment of the present invention, the second quenching temperature is 100-120°C above AC3 of the forging material, for example, it can be 100°C, 104°C, 108°C, 112°C, 116°C or 120°C, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0036] Preferably, the holding time for the second temperature quenching is 60 to 90 minutes when the thermocouple temperature of the load block reaches 100°C above AC3 of the forging material. For example, it can be 60 minutes, 65 minutes, 70 minutes, 75 minutes, 80 minutes, 85 minutes or 90 minutes, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0037] It is worth noting that AC3 in this invention refers to the temperature at which the microstructure of the low alloy steel forging described in this invention is completely transformed into austenite.

[0038] The purpose of the quenching treatment described in this invention is to achieve a homogenized microstructure and a martensitic transformation in the forging.

[0039] As a preferred technical solution of the present invention, the tempering process in step (2) includes a first tempering, a first air cooling, a second tempering and a second air cooling performed sequentially.

[0040] As a preferred embodiment of the present invention, the temperature of the first tempering is 110-130°C below AC1 of the forging material, for example, it can be 110°C, 114°C, 118°C, 122°C, 126°C or 130°C, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0041] Preferably, the holding time for the first tempering is 720 to 750 minutes when the thermocouple temperature of the load block reaches 130°C below AC1 of the forging material. For example, it can be 720 minutes, 725 minutes, 730 minutes, 735 minutes, 740 minutes, 745 minutes, or 750 minutes, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0042] Preferably, the primary tempering is performed by entering the furnace at the designated temperature.

[0043] Preferably, the secondary tempering temperature is 100-120°C below AC1 of the forging material, for example, it can be 100°C, 104°C, 108°C, 112°C, 116°C or 120°C, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0044] Preferably, the holding time for the secondary tempering is 720 to 750 minutes when the thermocouple temperature of the load block reaches 120°C below AC1 of the forging material. For example, it can be 720 minutes, 725 minutes, 730 minutes, 735 minutes, 740 minutes, 745 minutes, or 750 minutes, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0045] It is worth noting that AC1 in this invention refers to the temperature at which the microstructure of the low alloy steel forging of this invention changes from pearlite to austenite.

[0046] Preferably, the secondary tempering is performed by entering the furnace at the designated temperature.

[0047] The purpose of the tempering treatment described in this invention is to ensure the precipitation of strengthening agents in the forging and to regulate and reduce the differences in strength and impact toughness caused by the difference in hardening effect between the core and surface of the forging.

[0048] It is worth noting that the temperature of the secondary tempering described in this invention is higher than that of the primary tempering, which can improve the impact performance while ensuring the strength of the forging.

[0049] As a preferred embodiment of the present invention, the heat treatment method for improving the core impact performance of large-section low-alloy steel forgings provided by the present invention includes the following steps:

[0050] (1) The low alloy steel forging is forged, and then annealed and machined in sequence to obtain a primary forging;

[0051] The low-alloy steel forgings include Cr-Mo series steel with an alloy element content of no more than 5 wt%; the Cr-Mo series steel has a C content of 0.2 to 0.4 wt% and a Ni content of ≤0.5 wt%.

[0052] The forging temperature is 1090–1110℃, and the deformation is 30–70%.

[0053] The annealing temperature is 690-710℃, and the holding time is the effective thickness of the low alloy steel forging × (2-3) min / mm.

[0054] The effective thickness of the forging is ≤400mm, and the fillet radius at the edges is ≥5mm;

[0055] (2) Mix the load block and the first forging obtained in step (1), and then perform quenching and tempering treatment in sequence;

[0056] The effective thickness of the load block and the primary forging is the same; the load block is provided with blind holes for setting thermocouples; the extension line of the thermocouple is connected to a display instrument for calculating the holding time of quenching and tempering treatments.

[0057] The quenching process includes sequential first-temperature quenching, second-temperature quenching, and water cooling; the first-temperature quenching temperature is 840-860℃, and the holding time is the effective thickness of the forging × (1-1.5) min / mm; the second-temperature quenching temperature is 100-120℃ above AC3 of the forging material, and the holding time is 60-90 min when the thermocouple temperature of the load block reaches 100℃ above AC3 of the forging material.

[0058] The tempering process includes a first tempering, a first air cooling, a second tempering, and a second air cooling performed sequentially. The first tempering is performed by entering the furnace at a temperature below the AC1 of the forging material, which is 110–130°C. The holding time is 720–750 min when the thermocouple temperature of the load block reaches 130°C below the AC1 of the forging material. The second tempering is performed by entering the furnace at a temperature below the AC1 of the forging material, which is 100–120°C. The holding time is 720–750 min when the thermocouple temperature of the load block reaches 120°C below the AC1 of the forging material.

[0059] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. The purpose and beneficial effects of the present invention can be better achieved and realized through the following preferred technical solutions.

[0060] Compared with the prior art, the present invention has the following beneficial effects:

[0061] (1) The heat treatment method provided by the present invention adopts a lower tempering temperature and uses a load thermocouple to control the holding time, which can achieve a core-to-surface tensile strength difference of large cross-section low alloy steel forging within 40MPa (solving the problem of large core-to-surface strength difference caused by poor hardenability of this type of alloy forging), and the room temperature impact performance of the core is significantly improved.

[0062] (2) The present invention adopts the process of tempering by entering the furnace at the temperature, which can solve the problem that the actual performance of the forgings is greatly different due to the difference in holding time caused by the change in the amount of heat treatment furnace loading and the change in the heating rate.

[0063] (3) The heat treatment method provided by the present invention has a higher temperature for the first tempering than that for the second tempering, which can improve the impact performance while ensuring the strength of the forging. Detailed Implementation

[0064] To facilitate understanding of the present invention, the following embodiments are provided. Those skilled in the art should understand that these embodiments are merely illustrative and should not be construed as limiting the scope of the invention.

[0065] Example 1

[0066] This embodiment provides a heat treatment method for improving the core impact performance of large-section low-alloy steel forgings, the heat treatment method comprising the following steps:

[0067] (1) A low alloy steel forging with an effective thickness of 500 mm is forged, and then annealed and machined in sequence to obtain a primary forging;

[0068] The low-alloy steel forgings include Cr-Mo series steel with an alloy element content of 4 wt%; the Cr-Mo series steel has a C content of 0.3 wt% and a Ni content of 0.4 wt%.

[0069] The forging temperature is 1100℃ and the deformation is 50%.

[0070] The annealing temperature is 700℃, and the holding time is the effective thickness of the low alloy steel forging × 2.5 min / mm;

[0071] The effective thickness of the forging is 350 mm, and the fillet radius at the corners is 8 mm.

[0072] (2) Mix the load block and the first forging obtained in step (1), and then perform quenching and tempering treatment in sequence;

[0073] The effective thickness of the load block and the primary forging is the same; the load block is provided with blind holes for setting thermocouples; the extension line of the thermocouple is connected to a display instrument for calculating the holding time of quenching and tempering treatments.

[0074] The quenching process includes sequential first-temperature quenching, second-temperature quenching, and water cooling; the first-temperature quenching temperature is 850℃, and the holding time is the effective thickness of the forging × 1min / mm; the second-temperature quenching temperature is 110℃ above AC3 of the forging material, and the holding time is 60min when the thermocouple temperature of the load block reaches 100℃ above AC3 of the forging material.

[0075] The tempering process includes a first tempering, a first air cooling, a second tempering, and a second air cooling performed sequentially. The first tempering is performed by entering the furnace at a temperature below AC1 of the forging material, with a holding time of 720 minutes after the thermocouple temperature of the load block reaches 130°C below AC1 of the forging material. The second tempering is performed by entering the furnace at a temperature below AC1 of the forging material, with a temperature below AC1 of the forging material, with a holding time of 720 minutes after the thermocouple temperature of the load block reaches 120°C below AC1 of the forging material.

[0076] Example 2

[0077] This embodiment provides a heat treatment method for improving the core impact performance of large-section low-alloy steel forgings, the heat treatment method comprising the following steps:

[0078] (1) A low alloy steel forging with an effective thickness of 600 mm is forged, and then annealed and machined in sequence to obtain a primary forging;

[0079] The low-alloy steel forgings include Cr-Mo series steel with an alloy element content of 3 wt%; the Cr-Mo series steel has a C content of 0.2 wt% and a Ni content of 0.4 wt%.

[0080] The forging temperature is 1090℃, and the deformation is 30%.

[0081] The annealing temperature is 690℃, and the holding time is the effective thickness of the low alloy steel forging × 3min / mm;

[0082] The effective thickness of the forging is 400 mm, and the fillet radius at the edges is 5 mm.

[0083] (2) Mix the load block and the first forging obtained in step (1), and then perform quenching and tempering treatment in sequence;

[0084] The effective thickness of the load block and the primary forging is the same; the load block is provided with blind holes for setting thermocouples; the extension line of the thermocouple is connected to a display instrument for calculating the holding time of quenching and tempering treatments.

[0085] The quenching process includes sequential first-temperature quenching, second-temperature quenching, and water cooling; the first-temperature quenching temperature is 840℃, and the holding time is the effective thickness of the forging × 1.5 min / mm; the second-temperature quenching temperature is 100℃ above AC3 of the forging material, and the holding time is 90 min when the thermocouple temperature of the load block reaches 100℃ above AC3 of the forging material.

[0086] The tempering process includes a first tempering, a first air cooling, a second tempering, and a second air cooling performed sequentially. The first tempering is performed by entering the furnace at a temperature below the AC1 of the forging material, with a temperature of 110°C below the AC1 of the forging material and a holding time of 730 minutes when the thermocouple temperature of the load block reaches 130°C below the AC1 of the forging material. The second tempering is performed by entering the furnace at a temperature below the AC1 of the forging material, with a temperature of 100°C below the AC1 of the forging material and a holding time of 730 minutes when the thermocouple temperature of the load block reaches 120°C below the AC1 of the forging material.

[0087] Example 3

[0088] This embodiment provides a heat treatment method for improving the core impact performance of large-section low-alloy steel forgings, the heat treatment method comprising the following steps:

[0089] (1) A low alloy steel forging with an effective thickness of 700 mm is forged, and then annealed and machined in sequence to obtain a primary forging;

[0090] The low-alloy steel forgings include Cr-Mo series steel with an alloy element content of 5 wt%; the Cr-Mo series steel contains 0.4 wt% C and 0.5 wt% Ni.

[0091] The forging temperature is 1110℃, and the deformation is 70%.

[0092] The annealing temperature is 710℃, and the holding time is the effective thickness of the low alloy steel forging × 2 min / mm;

[0093] The effective thickness of the forging is 300 mm, and the fillet radius at the edges is 5 mm.

[0094] (2) Mix the load block and the first forging obtained in step (1), and then perform quenching and tempering treatment in sequence;

[0095] The effective thickness of the load block and the primary forging is the same; the load block is provided with blind holes for setting thermocouples; the extension line of the thermocouple is connected to a display instrument for calculating the holding time of quenching and tempering treatments.

[0096] The quenching process includes sequential first-temperature quenching, second-temperature quenching, and water cooling; the first-temperature quenching temperature is 860℃, and the holding time is the effective thickness of the forging × 1.1 min / mm; the second-temperature quenching temperature is 120℃ above AC3 of the forging material, and the holding time is 70 min when the thermocouple temperature of the load block reaches 100℃ above AC3 of the forging material.

[0097] The tempering process includes a first tempering, a first air cooling, a second tempering, and a second air cooling performed sequentially. The first tempering is performed by entering the furnace at a temperature below the AC1 of the forging material, with a temperature of 130°C below the AC1 of the forging material and a holding time of 750 minutes after the thermocouple temperature of the load block reaches 130°C below the AC1 of the forging material. The second tempering is performed by entering the furnace at a temperature below the AC1 of the forging material, with a temperature of 120°C below the AC1 of the forging material and a holding time of 750 minutes after the thermocouple temperature of the load block reaches 120°C below the AC1 of the forging material.

[0098] Example 4

[0099] This embodiment provides a heat treatment method to improve the core impact performance of large-section low-alloy steel forgings. The only difference between this heat treatment method and that of Embodiment 1 is:

[0100] In this embodiment, the effective thickness of the primary forging in step (1) is modified to 450 mm.

[0101] Example 5

[0102] This embodiment provides a heat treatment method to improve the core impact performance of large-section low-alloy steel forgings. The only difference between this heat treatment method and that of Embodiment 1 is:

[0103] In this embodiment, the annealing temperature in step (1) is modified to 650℃, and the holding time is the effective thickness of the low alloy steel forging × 2.5 min / mm.

[0104] Example 6

[0105] This embodiment provides a heat treatment method to improve the core impact performance of large-section low-alloy steel forgings. The only difference between this heat treatment method and that of Embodiment 1 is:

[0106] In this embodiment, the annealing temperature in step (1) is modified to 750℃, and the holding time is the effective thickness of the low alloy steel forging × 2.5 min / mm.

[0107] Example 7

[0108] This embodiment provides a heat treatment method to improve the core impact performance of large-section low-alloy steel forgings. The only difference between this heat treatment method and that of Embodiment 1 is:

[0109] This embodiment omits the tempering process described in step (2).

[0110] Example 8

[0111] This embodiment provides a heat treatment method to improve the core impact performance of large-section low-alloy steel forgings. The only difference between this heat treatment method and that of Embodiment 1 is:

[0112] This embodiment omits the secondary tempering process described in step (2).

[0113] Example 9

[0114] This embodiment provides a heat treatment method to improve the core impact performance of large-section low-alloy steel forgings. The only difference between this heat treatment method and that of Embodiment 1 is:

[0115] This embodiment omits the mixing process of the load block.

[0116] Comparative Example 1

[0117] This comparative example provides a heat treatment method for improving the core impact performance of large-section low-alloy steel forgings. The heat treatment method includes sequential annealing, quenching, and tempering. The effective thickness of the forging is 350 mm after quenching.

[0118] The annealing treatment is performed at a temperature of 650℃ for a time equal to the effective thickness × 2.0 min / mm; the quenching treatment is performed at a temperature of AC3 + 40℃ for a time equal to the effective thickness × 1.5 min / mm, and the cooling method is water cooling; the tempering treatment is performed at a temperature of AC1 - 60℃ for a time equal to the effective thickness × 2.5 min / mm.

[0119] Performance testing:

[0120] Mechanical properties of the outer edge and core of the forgings obtained after heat treatment in the above embodiments and comparative examples were tested, and the results are shown in Table 1 and Table 2, respectively.

[0121] The mechanical property testing includes room temperature tensile testing and room temperature impact testing.

[0122] Table 1

[0123]

[0124]

[0125] Table 2

[0126]

[0127] In summary, the heat treatment method provided by this invention can obtain forgings with a core-to-surface tensile strength difference of less than 40 MPa and high core impact performance, which has significant practical value for low-cost, mass production of large-section low-alloy steel forgings.

[0128] The applicant declares that the detailed process equipment and process flow of the present invention are illustrated through the above embodiments, but the present invention is not limited to the above detailed process equipment and process flow, that is, it does not mean that the present invention must rely on the above detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0129] The applicant declares that the detailed process flow of this invention is illustrated by the above embodiments, but this invention is not limited to the above detailed process flow, that is, it does not mean that this invention must rely on the above detailed process flow to be implemented. Those skilled in the art should understand that any improvements to this invention, equivalent substitutions of raw materials for the product of this invention, addition of auxiliary components, and selection of specific methods, etc., all fall within the protection scope and disclosure scope of this invention.

Claims

1. A heat treatment method for improving the core impact performance of large-section low-alloy steel forgings, characterized in that, The heat treatment method includes the following steps: (1) The low alloy steel forging is forged, and then annealed and machined in sequence to obtain a primary forging; the annealing temperature is 690~750℃; the holding time of the annealing is the effective thickness of the low alloy steel forging × (2~3) min / mm; the effective thickness of the primary forging is ≤400mm; the fillet radius at the corner of the primary forging is ≥5mm; (2) The load block and the primary forging obtained in step (1) are mixed and then quenched and tempered in sequence; the effective thickness of the load block and the primary forging are the same; The tempering process includes a first tempering, a first air cooling, a second tempering, and a second air cooling performed sequentially. The temperature of the first tempering is 110~130℃ below AC1 of the forging material; the holding time of the first tempering is 720~750min when the thermocouple temperature of the load block reaches 130℃ below AC1 of the forging material. The temperature of the secondary tempering is 100-120°C below AC1 of the forging material; the holding time of the secondary tempering is 720-750 minutes when the thermocouple temperature of the load block reaches 120°C below AC1 of the forging material.

2. The heat treatment method according to claim 1, characterized in that, The low-alloy steel forgings in step (1) include Cr-Mo series steel with an alloy element content of no more than 5 wt%.

3. The heat treatment method according to claim 2, characterized in that, The Cr-Mo series steel has a C content of 0.2~0.4wt% and a Ni content of ≤0.5wt%.

4. The heat treatment method according to claim 1, characterized in that, The forging temperature in step (1) is 1090~1110℃.

5. The heat treatment method according to claim 4, characterized in that, The deformation amount of the forging in step (1) is 30~70%.

6. The heat treatment method according to claim 1, characterized in that, The holding time for the annealing treatment in step (1) is ≥40 min.

7. The heat treatment method according to claim 1, characterized in that, The load block is provided with blind holes for mounting thermocouples.

8. The heat treatment method according to claim 7, characterized in that, The extension line of the thermocouple is connected to a display instrument for calculating the holding time of quenching and tempering treatments.

9. The heat treatment method according to claim 1, characterized in that, The load block is made of low alloy steel.

10. The heat treatment method according to claim 9, characterized in that, The low-alloy steel includes any one of 45 steel, 35 steel, or 30 steel.

11. The heat treatment method according to claim 1, characterized in that, The quenching process in step (2) adopts a stepped heating process, which includes quenching at a first temperature, quenching at a second temperature, and water cooling in sequence.

12. The heat treatment method according to claim 11, characterized in that, The first quenching temperature is 840~860℃.

13. The heat treatment method according to claim 12, characterized in that, The holding time for quenching at the first temperature is ≥30 min.

14. The heat treatment method according to claim 13, characterized in that, The holding time for quenching at the first temperature is the effective thickness of the forging in one pass × (1-1.5) min / mm.

15. The heat treatment method according to claim 11, characterized in that, The second quenching temperature is 100~120℃ above AC3 of the forging material.

16. The heat treatment method according to claim 15, characterized in that, The holding time for the second temperature quenching is 60-90 minutes when the thermocouple temperature of the load block reaches 100°C above AC3 of the forging material.

17. The heat treatment method according to claim 1, characterized in that, The first tempering process uses the method of entering the furnace at the specified temperature.

18. The heat treatment method according to claim 1, characterized in that, The secondary tempering adopts the method of entering the furnace at the specified temperature.

19. The heat treatment method according to claim 1, characterized in that, The heat treatment method includes the following steps: (1) The low alloy steel forging is forged, and then annealed and machined in sequence to obtain a primary forging; The low-alloy steel forgings include Cr-Mo series steel with an alloy element content not exceeding 5 wt%; the Cr-Mo series steel has a C content of 0.2~0.4 wt% and a Ni content ≤0.5 wt%. The forging temperature is 1090~1110℃, and the deformation is 30~70%; The annealing temperature is 690~750℃, and the holding time is the effective thickness of the low alloy steel forging × (2~3) min / mm; The effective thickness of the forging is ≤400mm, and the fillet radius at the edges is ≥5mm; (2) Mix the load block and the first forging obtained in step (1), and then perform quenching and tempering treatment in sequence; The effective thickness of the load block and the primary forging is the same; the load block is provided with blind holes for setting thermocouples; the extension line of the thermocouple is connected to a display instrument for calculating the holding time of quenching and tempering treatments. The quenching process includes sequential first-temperature quenching, second-temperature quenching, and water cooling; the first-temperature quenching temperature is 840~860℃, and the holding time is the effective thickness of the forging × (1-1.5) min / mm; the second-temperature quenching temperature is 100~120℃ above AC3 of the forging material, and the holding time is 60~90 min when the thermocouple temperature of the load block reaches 100℃ above AC3 of the forging material. The tempering process includes a first tempering, a first air cooling, a second tempering, and a second air cooling performed sequentially. The first tempering is performed by entering the furnace at a temperature below the AC1 of the forging material, which is 110~130℃. The holding time is 720~750 minutes after the thermocouple temperature of the load block reaches 130℃ below the AC1 of the forging material. The second tempering is performed by entering the furnace at a temperature below the AC1 of the forging material, which is 100~120℃ below the AC1 of the forging material. The holding time is 720~750 minutes after the thermocouple temperature of the load block reaches 120℃ below the AC1 of the forging material.

Citation Information

Patent Citations

  • Heat treatment process of heavy section low-carbon and low-alloy steel castings and forgings

    CN104164548A

  • Large-section high-hardenability high-strength medium-manganese forged steel and preparation method thereof

    CN113462956A

  • Method for eliminating black spot structures in large low alloy steel forgings

    CN115216605A

  • Method for improving toughness of high-temperature-resistant low-carbon medium-low alloy steel

    CN117107167A