High carbon steel wire rod and method for producing the same
By controlling the composition and production process of high-carbon steel wire rod, especially by adding Nb, the precipitation of network cementite is suppressed, thus solving the plasticity problem of high-carbon steel wire rod during the cooling process and improving its mechanical properties and resistance to hydrogen embrittlement.
Patent Information
- Application Number
- CN202311786832.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-22
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-22
AI Technical Summary
High-carbon steel wire rods are prone to developing a network of cementite structure when cooled on air-cooled roller conveyors, which affects plasticity. Furthermore, increasing the cooling rate will increase production costs and equipment burden.
By controlling the composition of high-carbon steel wire rod, especially by adding Nb, the eutectoid carbon content can be increased by utilizing Nb's drag effect on C, thereby inhibiting the precipitation of network cementite. Furthermore, by controlling the rolling and cooling processes, the risk of network cementite can be reduced.
It effectively reduces the risk of network cementite structure, ensures the plasticity and mechanical properties of high carbon steel wire rod, and improves resistance to hydrogen embrittlement and reduction of area.
Smart Images

Figure CN117867382B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of steel preparation technology. In particular, it relates to a high-carbon steel wire rod and its production method. Background Technology
[0002] High-carbon steel wire rod is generally used to manufacture prestressed steel wire, steel strand, and mining anchor cables. Its products are widely used in highways, railways, and mining. High-carbon steel wire rod is typically large in size, and during air-cooled roller cooling, insufficient cooling rate in the core area can easily lead to the formation of a network of cementite, thus affecting the wire rod's plasticity. However, excessively increasing the cooling rate can overburden the equipment and significantly increase production costs. Summary of the Invention
[0003] In view of this, embodiments of the present invention provide a high-carbon steel wire rod and a method for producing the same, which can reduce the risk of the formation of a network cementite structure and ensure the shaping of the high-carbon steel wire rod.
[0004] To achieve the above objectives, the embodiments of the present invention adopt the following technical solutions:
[0005] In a first aspect, embodiments of the present invention provide a high-carbon steel wire rod, comprising the following components in parts by weight: C: 0.80–0.83%; Si: 0.10–0.40%; Mn: 0.60–0.90%; Cr: 0.20–0.40%; V: 0.04–0.07%; Nb: 0.004–0.010%; P ≤ 0.03%; S ≤ 0.03%; Fe: 96–98%.
[0006] According to a specific implementation of an embodiment of the present invention, the high-carbon steel wire rod comprises the following components in parts by weight: C: 0.81-0.83%; Si: 0.20-0.30%; Mn: 0.70-0.80%; Cr: 0.25-0.35%; V: 0.04-0.05%; Nb: 0.004-0.008%; P: 0.02-0.03%; S: 0.02-0.03%; Fe: 97-98%.
[0007] According to a specific implementation of an embodiment of the present invention, the high-carbon steel wire rod comprises the following components in parts by weight: C: 0.83%; Si: 0.29%; Mn: 0.77%; Cr: 0.33%; V: 0.07%; Nb: 0.007%; P: 0.03%; S: 0.03%; Fe: 97.643%.
[0008] Secondly, embodiments of the present invention provide a method for producing high-carbon steel wire rod, comprising: smelting high-carbon steel wire rod raw materials to obtain raw material smelting liquid; adding a predetermined weight portion of ferroniobium to the raw material smelting liquid to obtain high-carbon steel wire rod smelting liquid; refining the high-carbon steel wire rod smelting liquid to obtain high-carbon steel wire rod refined liquid; transferring the high-carbon steel wire rod refined liquid to a continuous casting machine for continuous casting to obtain a billet; feeding the billet into a heating furnace for heating; using a high-pressure water device to descaling the billet; rolling and wire drawing the descaled billet to obtain coiled high-speed wire rod; and transferring the coiled high-speed wire rod to an air-cooled roller conveyor for controlled cooling to obtain high-carbon steel wire rod.
[0009] According to a specific implementation of an embodiment of the present invention, the continuous casting of the high-carbon steel wire rod refining liquid includes: controlling the casting speed to be 1.2 to 1.5 m / min, and continuously casting the high-carbon steel wire rod refining liquid.
[0010] According to a specific implementation of an embodiment of the present invention, the billet is fed into a heating furnace for heating, comprising: feeding the billet into a preheating section of the heating furnace for preheating, wherein the preheating temperature of the preheating section is 800℃~900℃; and after preheating the billet, feeding the billet into a homogenizing section of the heating furnace for heating, wherein the homogenizing temperature of the homogenizing section is 1100℃~1200℃.
[0011] According to a specific implementation of an embodiment of the present invention, a dephosphorized billet is rolled to obtain high-speed wire rod, comprising: sequentially transferring the dephosphorized billet to a roughing mill and an intermediate mill for rolling to obtain a bar; wherein the temperature of the dephosphorized billet is controlled at 1000℃~1120℃; and transferring the bar to a finishing mill for rolling to obtain high-speed wire rod; wherein the temperature of the bar is controlled at 860℃~910℃.
[0012] According to a specific implementation of an embodiment of the present invention, after obtaining the high-speed wire, the method further includes: transferring the high-speed wire to a spinning machine for spinning to obtain a coiled high-speed wire; wherein the temperature of the coiled high-speed wire is controlled at 920℃~950℃.
[0013] The high-carbon steel wire rod and its production method provided in this invention include the following components by weight: C: 0.80-0.83%; Si: 0.10-0.40%; Mn: 0.60-0.90%; Cr: 0.20-0.40%; V: 0.04-0.07%; Nb: 0.004-0.010%; P≤0.03%; S≤0.03%; Fe: 96-98%. This allows for the increase of eutectoid carbon content in the steel through the dragging effect of Nb on C, inhibiting the precipitation of network cementite, thereby reducing the risk of network cementite structure and ensuring the plasticity of the high-carbon steel wire rod. Attached Figure Description
[0014] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0015] Figure 1 This is a metallographic structure diagram of the high-carbon steel wire rod of Example 1 of the present invention under an optical microscope;
[0016] Figure 2 This is a metallographic structure image of the high-carbon steel wire rod in Example 2 of the present invention under an optical microscope;
[0017] Figure 3 This is a metallographic structure image of the high-carbon steel wire rod of Example 3 of the present invention under an optical microscope;
[0018] Figure 4 This is a metallographic image of the high-carbon steel wire rod in Example 4 of the present invention under an optical microscope;
[0019] Figure 5 This is a metallographic structure image of the high-carbon steel wire rod in Example 5 of the present invention under an optical microscope;
[0020] Figure 6 This is a metallographic structure image of the high-carbon steel wire rod of Example 6 of the present invention under an optical microscope;
[0021] Figure 7 This is a metallographic structure image of the high-carbon steel wire rod of Example 7 of the present invention under an optical microscope;
[0022] Figure 8 This is a metallographic structure diagram of the high-carbon steel wire rod in Example 8 of the present invention under an optical microscope;
[0023] Figure 9 This is a metallographic structure diagram of the high-carbon steel wire rod of Example 9 of the present invention under an optical microscope;
[0024] Figure 10 The image shows the metallographic structure of the high-carbon steel wire rod of this invention under an optical microscope.
[0025] Figure 11 This is a metallographic structure image of the high-carbon steel wire rod of Example 1 of the present invention under a scanning electron microscope;
[0026] Figure 12 This is a metallographic image of the high-carbon steel wire rod in Example 2 of the present invention under a scanning electron microscope;
[0027] Figure 13 This is a metallographic image of the high-carbon steel wire rod of Example 3 of the present invention under a scanning electron microscope;
[0028] Figure 14 This is a metallographic image of the high-carbon steel wire rod in Example 4 of the present invention, obtained using a scanning electron microscope.
[0029] Figure 15 This is a metallographic image of the high-carbon steel wire rod in Example 5 of the present invention, obtained using a scanning electron microscope.
[0030] Figure 16 This is a metallographic image of the high-carbon steel wire rod in Example 6 of the present invention, obtained using a scanning electron microscope.
[0031] Figure 17 This is a metallographic image of the high-carbon steel wire rod in Example 7 of the present invention, obtained using a scanning electron microscope.
[0032] Figure 18 This is a metallographic image of the high-carbon steel wire rod in Example 8 of the present invention, obtained using a scanning electron microscope.
[0033] Figure 19 This is a metallographic image of the high-carbon steel wire rod in Example 9 of the present invention under a scanning electron microscope;
[0034] Figure 20 The image shows the metallographic structure of the high-carbon steel wire rod of this invention under a scanning electron microscope. Detailed Implementation
[0035] The embodiments of the present invention will now be described in detail with reference to the accompanying drawings.
[0036] It should be understood that the described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0037] The present invention provides a high-carbon steel wire rod and its production method, which can reduce the risk of network cementite structure and ensure the shaping of high-carbon steel wire rod.
[0038] The method for producing high-carbon steel wire rod according to an embodiment of the present invention includes: smelting high-carbon steel wire rod raw materials to obtain raw material smelting liquid; adding a predetermined weight portion of ferroniobium to the raw material smelting liquid to obtain high-carbon steel wire rod smelting liquid; refining the high-carbon steel wire rod smelting liquid to obtain high-carbon steel wire rod refined liquid; transferring the high-carbon steel wire rod refined liquid to a continuous casting machine for continuous casting to obtain a billet; feeding the billet into a heating furnace for heating; using a high-pressure water device to descaling the billet; rolling and wire drawing the descaled billet to obtain coiled high-speed wire rod; and transferring the coiled high-speed wire rod to an air-cooled roller conveyor for controlled cooling to obtain high-carbon steel wire rod.
[0039] Adding a predetermined amount of ferroniobium to the raw material smelting liquid can give the high-carbon steel wire rod smelting liquid a predetermined amount of Nb. For example, the ferroniobium added to the raw material smelting liquid can be ferroniobium powder.
[0040] The phosphorus used in the descaling process of billets forms a dense layer of iron oxide scale on the surface of the billets. For example, a high-pressure water jet cleaner or water jet can be installed around a section of the production line. As the billets pass through this section, the impact force of the high-pressure water jet cuts and removes the iron oxide scale. This section of the production line can be located at room temperature.
[0041] The specifications for obtaining high-carbon steel wire rod are 13-15mm.
[0042] The high-carbon steel wire rod provided by the embodiments of the present invention can increase the eutectoid carbon content of the steel by adding Nb element to the raw material molten liquid, thereby inhibiting the precipitation of network cementite and reducing the risk of network cementite structure, and ensuring the shaping of high-carbon steel wire rod by utilizing the drag effect of Nb element on C element.
[0043] In one embodiment, the continuous casting of the high-carbon steel wire rod refining liquid includes: controlling the casting speed to be 1.2 to 1.5 m / min, and continuously casting the high-carbon steel wire rod refining liquid.
[0044] Here, the drawing speed (pulling speed) refers to the speed at which the billet is drawn from the continuous casting machine. In this embodiment of the invention, by controlling the drawing speed to 1.2–1.5 m / min, both production efficiency and the quality of the obtained billet are ensured.
[0045] In one embodiment, the billet is fed into a heating furnace for heating, including: feeding the billet into a preheating section of the heating furnace for preheating at a temperature of 800°C to 900°C; and after preheating, feeding the billet into a soaking section of the heating furnace for heating at a soaking temperature of 1100°C to 1200°C. By controlling the temperatures of the preheating and soaking sections, the risk of segregation of the billet in the heating furnace can be reduced, thereby suppressing the precipitation of network cementite.
[0046] In one embodiment, a high-speed wire rod is obtained by rolling a descaled billet, comprising: sequentially transferring the descaled billet to a roughing mill and an intermediate mill for rolling to obtain a bar; wherein the temperature of the descaled billet is controlled at 1000℃~1120℃; and transferring the bar to a finishing mill for rolling to obtain the high-speed wire rod; wherein the temperature of the bar is controlled at 860℃~910℃. Thus, by controlling the rolling temperature of the billet and the bar, austenitization can be performed on the billet, while simultaneously reducing the deformation resistance of the billet and refining the grain size.
[0047] For example, a water tank can be installed before the roughing mill, and the temperature of the billet delivered to the roughing mill can be controlled by controlling the amount of water sprayed from the water tank. A water tank can also be installed before the finishing mill, and the temperature of the bar delivered to the finishing mill can be controlled by controlling the amount of water sprayed from the water tank.
[0048] In one embodiment, after obtaining the high-speed wire, the method further includes: transferring the high-speed wire to a spinning machine for spinning to obtain a coiled high-speed wire; wherein the temperature of the coiled high-speed wire is controlled at 920°C to 950°C.
[0049] In this way, by increasing the temperature of the coiled high-speed wire ejected from the spinning machine, the cooling rate (also known as the cooling speed) of the ejected coiled high-speed wire can be increased, thereby suppressing the formation of network cementite during the phase transformation process of the ejected coiled high-speed wire.
[0050] The high-carbon steel wire rod provided in this embodiment of the invention comprises the following components in parts by weight: C: 0.80-0.83%; Si: 0.10-0.40%; Mn: 0.60-0.90%; Cr: 0.20-0.40%; V: 0.04-0.07%; Nb: 0.004-0.010%; P≤0.03%; S≤0.03%; Fe: 96-98%.
[0051] Carbon (C) is an effective element for improving the strength of high-carbon steel wire rod. When the C content is less than 1%, the C content is positively correlated with the tensile strength of high-carbon steel wire rod. In one embodiment, increasing the C content in high-carbon steel wire rod by 0.1% increases its tensile strength by 30–40 MPa.
[0052] However, increasing the carbon content in high-carbon steel wire rod can also lead to its development towards hypereutectoid steel, reducing the mechanical properties of the high-carbon steel wire rod. In one embodiment, the carbon content in the high-carbon steel wire rod is 1%. During the cooling process in the production of high-carbon steel wire rod, the supercooled austenite precipitates proeutectoid network secondary cementite during the cooling transformation. Therefore, in this embodiment, the carbon content is 0.80–0.83%.
[0053] Silicon (Si) can enhance the hardenability and tensile strength of high-carbon steel wire rod. When the Si content is less than 0.5%, the Si content is positively correlated with the tensile strength of high-carbon steel wire rod. In one embodiment, increasing the Si content in the high-carbon steel wire rod by 0.1% increases its tensile strength by 8 MPa.
[0054] However, an increase in the Si content in high-carbon steel wire rod will also reduce its torsional properties, thereby reducing the forming rate during cold forming. Therefore, in this embodiment, the Si content is 0.10–0.40%.
[0055] Manganese (Mn) can enhance the tensile strength of high-carbon steel wire rod. When the Mn content is less than 1.2%, the internal Mn content is positively correlated with the tensile strength of high-carbon steel wire rod. In one embodiment, increasing the Mn content in high-carbon steel wire rod by 0.1% increases its tensile strength by 10 MPa.
[0056] However, an increase in the Mn content in high-carbon steel wire rod can also lead to segregation within the wire rod, resulting in the formation of martensite and reducing its mechanical properties. Therefore, in this embodiment, the Mn content is 0.60–0.90%.
[0057] The Cr (chromium) in high-carbon steel wire rod can replace some of the Fe element in the cementite, transforming the cementite in the high-carbon steel wire rod into iron-chromium composite cementite (Fe,Cr)3C, thereby enhancing the tensile strength of the high-carbon steel wire rod and also helping to improve the reduction of area of the high-carbon steel wire rod.
[0058] However, an increase in the Cr content in high-carbon steel wire rod can also lead to delamination fracture and reduce its mechanical properties. Therefore, in this embodiment, the Cr content is 0.20–0.40%.
[0059] Vanadium (V) in high-carbon steel wire rod can enhance its tensile strength. V and carbon can form vanadium carbide (VC), which is a very fine-sized carbide that can precipitate in cementite lamellars, strengthening the cementite lamellars and thus improving the tensile strength of the wire rod.
[0060] However, excessively high V content in high-carbon steel wire rods reduces their torsional properties and, after large deformation during cold working, causes the Fe3C cementite lamellars to fracture, thus reducing the plasticity of the high-carbon steel wire rods. Therefore, in this embodiment, the V content is 0.04–0.07%.
[0061] The segregation of carbon elements at grain boundaries leads to a network cementite structure. The high-carbon steel wire rod provided in this embodiment can suppress the segregation of carbon elements at grain boundaries by the dragging effect of Nb elements, thereby suppressing the precipitation of network cementite, reducing the risk of network cementite structure, and ensuring the plasticity of the high-carbon steel wire rod.
[0062] Furthermore, due to the drag effect of Nb on C, if a network cementite is to be formed in high-carbon steel wire rod, the C content in the high-carbon steel wire rod needs to be increased, which can increase the eutectoid carbon content in the high-carbon steel wire rod.
[0063] In this embodiment of the invention, when the Nb content added to the high carbon steel wire rod is below 0.010%, the Nb content is positively correlated with the undercooling degree of pearlite formation.
[0064] The diffusion rate of carbon is negatively correlated with the undercooling degree of pearlite formation. As the Nb content in high-carbon steel wire rod increases, the diffusion rate of carbon decreases, resulting in a greater undercooling degree for pearlite formation. This reduces the pearlite phase transformation temperature and refines the interlamellar spacing of pearlite in high-carbon steel. Furthermore, Nb can improve the resistance of high-carbon steel wire rod to hydrogen-induced delayed fracture.
[0065] However, excessive Nb content can increase the degree of segregation inside the high-carbon steel wire rod billet, and lowering the pearlite phase transformation temperature can easily lead to the formation of martensite in the high-carbon steel wire rod during production due to the excessively low phase transformation temperature. Therefore, in this embodiment, the Nb content is 0.004–0.010%.
[0066] Furthermore, by controlling the Nb content to be 0.004–0.010%, the production cost of high-carbon steel wire rod can be reduced.
[0067] In one embodiment, the components of the high-carbon steel wire rod, in addition to C, Si, Mn, Cr, V, Nb, P (phosphorus), and S (sulfur), consist of Fe (iron) and unavoidable impurities.
[0068] In one embodiment, the high-carbon steel wire rod comprises the following components in parts by weight: C: 0.81–0.83%; Si: 0.20–0.30%; Mn: 0.70–0.80%; Cr: 0.25–0.35%; V: 0.04–0.05%; Nb: 0.004–0.008%; P: 0.02–0.03%; S: 0.02–0.03%; Fe: 97–98%.
[0069] In one embodiment, the high-carbon steel wire rod has a specification of 13-15 mm. The specification of the high-carbon steel wire rod refers to the diameter of the round steel bar placed in a disc shape.
[0070] The high-carbon steel wire rods in the above embodiments can be obtained by using the high-carbon steel wire rod production method described in any of the above embodiments, based on their composition.
[0071] The high-carbon steel wire rod provided by the embodiments of the present invention has enhanced resistance to hydrogen embrittlement, reduction of area and mechanical properties, as detailed in the following examples and comparative examples.
[0072] Table 1. Composition design of Examples 1-6 and Comparative Example 1
[0073]
[0074] The Nb content in the comparative example is a residual element from the production of high-carbon steel wire rod.
[0075] For example, the high-carbon steel wire rods of the embodiments and comparative examples can be processed by wire cutting to obtain corresponding 10mm high metallographic samples. After grinding and polishing the surface of each metallographic sample, they are etched with 4% nitric acid alcohol reagent to obtain the metallographic samples to be analyzed.
[0076] After obtaining the metallographic samples to be analyzed, refer to Figures 1 to 10 As shown, each metallographic sample to be analyzed can be observed using an optical microscope (OM) to grade its network cementite and simultaneously calculate the sorbitization rate of each sample. (See attached image.) Figures 11 to 20 As shown, the pearlite lamellar structure of each metallographic sample was observed using scanning electron microscopy (SEM), and the pearlite lamellar spacing of each sample was obtained. Specific results are shown in Table 2.
[0077] Table 2. Metallographic examination and analysis results of Examples 1-9 and Comparative Example 1
[0078] Network cementite grade (level) Soxhletization rate (%) Pearlite lamellar spacing (μm) Example 1 1 93 0.19 Example 2 0 95 0.17 Example 3 0 96 0.17 Example 4 1 97 0.18 Example 5 1 97 0.16 Example 6 0 97 0.16 Example 7 2 94 0.21 Example 8 0 95 0.18 Example 9 0 95 0.19 Comparative Example 4 90 0.23
[0079] As shown in Table 2, the network cementite level of the high-carbon steel wire rod obtained by the embodiments of the present invention is significantly reduced, and the pearlite lamellae are also significantly refined, providing a good foundation for subsequent drawing.
[0080] A hydraulic universal testing machine can be used to perform tensile tests on the high-carbon steel wire rods obtained in each embodiment and comparative example, and the tensile strength, yield strength and reduction of area of each high-carbon steel wire rod can be recorded. The specific results are shown in Table 3.
[0081] Table 3 shows the mechanical property test results of Examples 1-9 and Comparative Example 1.
[0082] Tensile strength (MPa) Yield strength (MPa) Reduction of area (%) Example 1 1302.5 821.7 36.4 Example 2 1305.9 838.2 34.4 Example 3 1309.1 866.0 35.8 Example 4 1324.8 854.6 34.5 Example 5 1328.2 856.9 35.7 Example 6 1329.0 841.8 34.6 Example 7 1343.9 849.8 34.3 Example 8 1337.3 851.7 35.9 Example 9 1350.8 867.9 34.8 Comparative Example 1255.3 817.4 31.3
[0083] As shown in Table 3, the tensile strength and reduction of area of the high-carbon steel wire rod obtained by the embodiments of the present invention are significantly improved, which can enhance the mechanical properties of the high-carbon steel wire rod. For example, the tensile strength of the high-carbon steel wire rod in Example 9 is 1350.8 and the reduction of area is 34.8%.
[0084] The apparent hydrogen diffusion coefficient of the high-carbon steel wire rods obtained in each example and comparative example can be determined by electrochemical hydrogen charging.
[0085] In one embodiment, the electrolyte in the hydrogen charging tank is a mixed solution of 0.2 mol / L NaOH + 0.25 g / L Ag₂O₃, and the electrolyte in the hydrogen diffusion tank is 0.2 mol / L NaOH. Using a constant potential mode of an electrochemical measuring instrument, the current increases with time until it no longer changes, and the apparent diffusion coefficient of hydrogen is calculated. Specific results are shown in Table 4.
[0086] Table 4. Apparent hydrogen diffusion coefficients of Examples 1-9 and Comparative Example 1
[0087] Apparent diffusion coefficient of hydrogen (cm2·s-1) Example 1 1302.5 Example 2 1305.9 Example 3 1309.1 Example 4 1324.8 Example 5 1328.2 Example 6 1329.0 Example 7 1343.9 Example 8 1337.3 Example 9 1350.8 Comparative Example 1255.3
[0088] Table 4 shows that adding Nb to high-carbon steel wire rod significantly reduces the apparent hydrogen diffusion coefficient. A higher apparent hydrogen diffusion coefficient is positively correlated with resistance to hydrogen-induced delayed fracture; therefore, adding Nb to high-carbon steel wire rod can improve its resistance to hydrogen-induced delayed fracture.
[0089] The high-carbon steel wire rod and its production method provided by the embodiments of the present invention, by adding Nb, on the one hand, can increase the eutectoid carbon content of the steel, and Nb has a dragging effect on C, thereby inhibiting the precipitation of network cementite and improving the hydrogen embrittlement resistance of the drawn high-carbon steel wire rod. On the other hand, Nb can reduce the phase transformation temperature of pearlite and refine the interlamellar spacing of pearlite, thereby increasing the section reduction rate of the high-carbon steel wire rod, and thus improving the overall mechanical properties of the high-carbon steel wire rod.
[0090] It should be noted that, in this document, relational terms such as "first" and "etc." are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0091] The various embodiments in this specification are described in a related manner. The same or similar parts between the various embodiments can be referred to each other. Each embodiment focuses on describing the differences from other embodiments.
[0092] In particular, the device embodiment is basically similar to the method embodiment, so the description is relatively simple. For relevant details, please refer to the description of the method embodiment.
[0093] For ease of description, the above apparatus is described by dividing it into various functional units / modules. Of course, in implementing this invention, the functions of each unit / module can be implemented in one or more software and / or hardware.
[0094] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A high-carbon steel wire rod, characterized in that, It is composed of the following components in parts by weight: C: 0.81~0.83%; Si: 0.20~0.30%; Mn: 0.70~0.80%; Cr: 0.25~0.35%; V: 0.04~0.05%; Nb: 0.004~0.008%; P: 0.02~0.03%; S: 0.02~0.03%; Fe: 97~98%; A method for producing high-carbon steel wire rod includes: smelting high-carbon steel wire rod raw materials to obtain raw material molten liquid; adding a predetermined weight proportion of ferroniobium to the raw material molten liquid to obtain high-carbon steel wire rod molten liquid; refining the high-carbon steel wire rod molten liquid to obtain high-carbon steel wire rod refined liquid; transferring the high-carbon steel wire rod refined liquid to a continuous casting machine for continuous casting to obtain a billet; feeding the billet into a heating furnace for heating; descaling the billet using a high-pressure water device; rolling and wire drawing the descaled billet to obtain coiled high-speed wire rod; and transferring the coiled high-speed wire rod to an air-cooled roller conveyor for controlled cooling to obtain high-carbon steel wire rod. The billet is fed into a heating furnace for heating, including: feeding the billet into a preheating section of the heating furnace for preheating, wherein the preheating temperature of the preheating section is 800℃~900℃; and after preheating the billet, feeding the billet into a homogenizing section of the heating furnace for heating, wherein the homogenizing temperature of the homogenizing section is 1100℃~1200℃. After obtaining the high-speed wire, the method further includes: transferring the high-speed wire to a spinning machine for spinning to obtain a coiled high-speed wire; wherein the temperature of the coiled high-speed wire is controlled at 920℃~950℃.
2. A method for producing high-carbon steel wire rod according to claim 1, characterized in that, include: The high-carbon steel wire rod raw material is smelted to obtain raw material molten liquid; A predetermined amount of ferroniobium is added to the raw material smelting liquid to obtain a high-carbon steel wire rod smelting liquid; The high-carbon steel wire rod smelting liquid is refined to obtain high-carbon steel wire rod refined liquid; The high-carbon steel wire rod refining liquid is transferred to a continuous casting machine for continuous casting to obtain a billet; The billet is fed into a heating furnace and heated. The billet was dephosphorized using a high-pressure water device. The dephosphorized billet is rolled and wire-spun to obtain coiled high-speed wire. The coiled high-speed wire is transferred to an air-cooled roller conveyor for controlled cooling to obtain high-carbon steel wire rod. The billet is fed into a heating furnace for heating, including: feeding the billet into a preheating section of the heating furnace for preheating, wherein the preheating temperature of the preheating section is 800℃~900℃; and after preheating the billet, feeding the billet into a homogenizing section of the heating furnace for heating, wherein the homogenizing temperature of the homogenizing section is 1100℃~1200℃. After obtaining the high-speed wire, the method further includes: transferring the high-speed wire to a spinning machine for spinning to obtain a coiled high-speed wire; wherein the temperature of the coiled high-speed wire is controlled at 920℃~950℃.
3. The method for producing high-carbon steel wire rod according to claim 2, characterized in that, The continuous casting of the high-carbon steel wire rod refining liquid includes: The casting speed is controlled at 1.2~1.5m / min, and the high-carbon steel wire rod refining liquid is continuously cast.
4. The method for producing high-carbon steel wire rod according to claim 2, characterized in that, The descaled billet is rolled to obtain high-speed wire rod, including: The dephosphorized billet is sequentially passed to the roughing mill and the intermediate mill for rolling to obtain bars; the temperature of the dephosphorized billet is controlled at 1000℃~1120℃. The bar is transferred to the finishing mill for rolling to obtain high-speed wire rod; wherein the temperature of the bar is controlled at 860℃~910℃.
Citation Information
Patent Citations
High carbon steel wire rod and preparation method thereof
CN101649416A
Coil rod used for 1670MPa level bridge cable zinc-coated wire and preparation method of coil rod
CN102181786A