A method for improving microstructure uniformity of 2618 aluminum alloy free forging
By performing high-temperature annealing and calculating deformation before forging 2618 aluminum alloy forgings, and by controlling the heat treatment parameters, the problems of coarse grains and uneven microstructure in 2618 aluminum alloy forgings were solved, thus improving product quality and performance.
Patent Information
- Application Number
- CN202311756621.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-20
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-20
AI Technical Summary
2618 aluminum alloy free forgings often exhibit problems such as coarse grains and uneven microstructure after heat treatment, which are difficult to solve effectively with existing technologies, resulting in unqualified products that cannot be reworked.
By performing high-temperature annealing before forging, and combining the calculation of deformation amount and forging process heat treatment parameters such as quenching and artificial aging temperature, the microstructure is refined and homogenized.
This effectively solved the problems of coarse grains and uneven microstructure in 2618 aluminum alloy forgings, improving the overall performance and market competitiveness of the products.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of hot working of aluminum alloys, and relates to a method for improving the uniformity of microstructure of 2618 aluminum alloy free forgings. Background Technology
[0002] 2618 aluminum alloy belongs to the Al-Cu-Mg-Fe-Ni alloy system and can be strengthened by heat treatment. Due to its high heat resistance and good cold and hot working properties, this alloy is widely used in the aerospace industry. Typically, 2618 aluminum alloy forgings are produced through free forging. After heat treatment, they often exhibit coarse grains and poor uniformity in their low-magnification microstructure. Once this occurs, it cannot be improved through heat treatment rework or other methods and must be scrapped. Research indicates that this phenomenon is related to improper forging process design for 2618 alloy. It is essential to rationally set the forging heating temperature, perform appropriate high-temperature annealing of the bar stock before forging, and strictly control the deformation amount to prevent the formation of uneven microstructure in the forgings. Summary of the Invention
[0003] The purpose of this invention is to provide a method for improving the uniformity of the microstructure of 2618 aluminum alloy free forgings, so as to solve the problems of coarse grains and uneven microstructure caused by the raw materials themselves or the amount of deformation in 2618 aluminum alloy free forgings.
[0004] Technical solution:
[0005] This invention provides a method for improving the microstructure uniformity of 2618 aluminum alloy free forgings, comprising:
[0006] Determine the high-temperature annealing temperature and time before forging the bar based on the bar diameter;
[0007] The number of forging processes for the main bar forging steps is determined based on the amount of bar deformation.
[0008] The bar stock was subjected to high-temperature annealing according to the determined high-temperature annealing heating temperature and time before forging.
[0009] According to the forging process, the high-temperature annealed bar stock is forged to obtain the required forgings;
[0010] The forging is heat-treated according to its effective thickness.
[0011] Furthermore, based on the diameter of the bar stock, the high-temperature annealing heating temperature and time before forging are determined, including:
[0012] For bars with a diameter > 150 mm, the heating temperature is determined to be 470-500℃, and the holding time is 1.5 minutes / 1 mm for the smaller of the length and diameter.
[0013] For bars with a diameter ≤150mm, the heating temperature is set at 440~470℃, and the holding time is 2 minutes / 1 mm for the smaller of the length and diameter.
[0014] Furthermore, the number of forging processes for the main bar stock is determined based on the bar stock deformation, including:
[0015] The deformation ε of the bar is calculated using the deformation calculation formula:
[0016] ε=△L / L before
[0017] △L = L_back - L_front;
[0018] The dimensions before L are the dimensions before forging, the dimensions after L are the dimensions after forging, and △L is the difference in dimensions before and after forging.
[0019] The number of forging cycles is determined based on the bar deformation amount ε and the deformation range per forging cycle. Among these, the deformation amount per forging cycle is controlled to avoid the coarse grain range of 5-15% and ≥75%, and the maximum deformation amount of hammer forging is ≤60%, while the maximum deformation amount of press forging is <75%.
[0020] Furthermore, the method also includes:
[0021] The bar stock after high-temperature annealing is heated before forging at a temperature of 440–460℃.
[0022] When the diameter of the bar after high-temperature annealing is greater than 150 mm, the holding time shall be 1.5 minutes per millimeter, whichever is smaller between the length and the diameter.
[0023] When the diameter of the bar after high-temperature annealing is ≤150 mm, the holding time is 2 minutes / 1 mm, whichever is smaller between the length and the diameter.
[0024] The conventional forging method is adopted, the final forging temperature is ≥380℃, and the forging is air-cooled after being supported.
[0025] Furthermore, during the forging process, the hammering should be light, with each hammering causing no more than 5% deformation, and the hammering should be slow, with a frequency of less than 2 times per second.
[0026] Furthermore, heat treatment includes quenching and artificial aging.
[0027] For forgings with an effective thickness > 150 mm, the quenching temperature is 530-550℃, the holding time is 2 minutes / 1 mm, and then the forging is cooled to room temperature with boiling water.
[0028] For forgings with an effective thickness ≤150mm, the heating temperature is 520~540℃, the holding time is 3 minutes / 1 mm, and then the parts are cooled to room temperature with boiling water.
[0029] Furthermore, the artificial aging temperature is 190–199℃, and the temperature is maintained for 0.5–2 hours, followed by natural air cooling to room temperature.
[0030] Beneficial effects:
[0031] Typically, 2618 aluminum alloy forgings, such as free forgings, produced according to the forging process, often exhibit defects such as coarse grains and poor uniformity in the low-magnification microstructure after heat treatment. Adding high-temperature annealing before forging, combined with calculated deformation during the forging process, and controlling the quenching and artificial aging temperatures during heat treatment, can effectively solve problems such as coarse grains and uneven microstructure in 2618 aluminum alloy forgings, significantly improving the overall performance and market competitiveness of the product. Detailed Implementation
[0032] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention.
[0033] First, through comparative studies, we found that billets that have undergone high-temperature annealing before forging, when subjected to the same forging heating temperature and the same deformation steps, exhibit a high degree of recrystallization, good equiaxedness, and fine and uniform deformed structure.
[0034] Secondly, the degree of dynamic recrystallization can be improved by calculating and controlling the degree of deformation. However, when the degree or amount of deformation in the final forging is determined and cannot be adjusted, additional forging passes must be added before the final forging. This can promote dynamic recrystallization of the billet and refine and homogenize the microstructure. During billet forging, the degree or amount of deformation can be appropriately increased, and the heating temperature can be selected within a wide temperature range of 440℃ to 460℃.
[0035] Finally, by controlling the quenching and artificial aging temperature and heating time in the post-forging heat treatment process, problems such as coarse grains and uneven structure can be prevented to the greatest extent possible during the heat treatment process.
[0036] This invention addresses the problems of coarse grains and uneven microstructure in 2618 aluminum alloy forgings by adding high-temperature annealing before forging, combining it with the calculation of deformation during the forging process, and controlling the heat treatment solution temperature.
[0037] This invention provides a method for improving the microstructure uniformity of 2618 aluminum alloy free forgings, comprising:
[0038] Determine the high-temperature annealing temperature and time before forging the bar based on the bar diameter;
[0039] The number of forging processes for the main bar forging steps is determined based on the amount of bar deformation.
[0040] The bar stock was subjected to high-temperature annealing according to the determined high-temperature annealing heating temperature and time before forging.
[0041] According to the forging process, the high-temperature annealed bar stock is forged to obtain the required forgings;
[0042] The forging is heat-treated according to its effective thickness.
[0043] For bars with a diameter >150mm, the heating temperature is 470-500℃, and the holding time is 1.5 minutes / 1 mm for the smaller of the length and diameter.
[0044] For bars with a diameter ≤150mm, the heating temperature is 440~470℃, and the holding time is 2 minutes / 1 mm for the smaller of the length and diameter. This can obtain a relatively uniform microstructure.
[0045] The deformation of the bar stock is calculated to determine the number of forging processes. The calculated deformation is calculated using the formula ε=△L / L.
[0046] △L = L_back - L_front
[0047] Control the deformation amount per forging to avoid the coarse grain range of 5-15% and ≥75%, and the maximum deformation amount of hammer forging should be ≤60%, and the maximum deformation amount of press forging should be <75%.
[0048] After high-temperature annealing, the bars are heated before forging at a temperature of 440–460℃. For diameters > 150 mm, the holding time is 1.5 minutes per millimeter of the smaller of the length and diameter; for diameters ≤ 150 mm, the holding time is 2 minutes per millimeter of the smaller of the length and diameter.
[0049] The conventional forging method is adopted, the final forging temperature is ≥380℃, and the forging is air-cooled after being supported.
[0050] During the forging process, the hammering should be light, and the deformation should not exceed 5% with each hammering. The hammering should be slow and the frequency should be less than 2 times / 1 second.
[0051] The final forging is subjected to heat treatment, specifically including quenching and artificial aging.
[0052] For forgings with an effective thickness > 150 mm, the quenching temperature is 530-550℃, the holding time is 2 minutes / 1 mm, and then the forging is cooled to room temperature with boiling water.
[0053] For forgings with an effective thickness ≤150mm, the heating temperature is 520~540℃, the holding time is 3 minutes / 1mm, and then the parts are cooled to room temperature with boiling water.
[0054] The artificial aging temperature is 190-199℃, and the temperature is maintained for 0.5-2 hours, followed by natural air cooling to room temperature.
[0055] By using high-temperature annealing before forging, combined with calculating the total deformation amount and determining the forging deformation heat treatment, and the post-forging quenching + artificial aging heat treatment process, the problems of coarse grains and uneven structure caused by uneven grain distribution in 2618 aluminum alloy forgings can be effectively solved.
[0056] Example 1:
[0057] Bar blanking dimensions: φ210×155mm, produced using a 2T free forging hammer.
[0058] Step 1: High-temperature annealing before forging: 480-490℃, holding coefficient: 1.5 minutes / 1 mm.
[0059] Step 2: Calculate the deformation amount according to the formula to determine the number of forging processes:
[0060] First forging: φ210×155 axially elongated and squared to 148×148×245. Pre-forging heating temperature is 440~460℃, holding coefficient is 1.5 minutes / 1 mm. During forging, hammering is gentle, with each hammer blow causing no more than 5% deformation, and a frequency of less than 2 times / 1 second. Final forging temperature ≥380℃, followed by air cooling.
[0061] Second forging: A 148×148×245mm axially elongated forging square is shaped to 120×120×373mm. The pre-forging heating temperature is 440~460℃, with a holding time of 2 minutes / 1mm. During forging, hammering is gentle, with each hammer blow causing no more than 5% deformation, and a frequency of less than 2 blows / 1 second. The final forging temperature is ≥380℃, and the forging is followed by air cooling.
[0062] Step 3: Perform heat treatment on the forged parts. Quenching temperature 530℃, holding time 360 minutes, cooling to room temperature with boiling water; artificial aging temperature 199℃, holding time 45 minutes, air cooling.
[0063] By adding high-temperature annealing before forging, combined with the calculation of deformation in the forging process, and controlling the quenching and artificial aging temperature of heat treatment, the problems of coarse grains and uneven structure of 2618 aluminum alloy forgings can be effectively solved, which can significantly improve the overall performance and market competitiveness of the product.
[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in the present invention, and these modifications or substitutions should be covered within the protection scope of the present invention.
Claims
1. A method for improving the microstructure uniformity of 2618 aluminum alloy free forgings, characterized in that, include: Determine the high-temperature annealing temperature and time before forging the bar based on the bar diameter; The number of forging processes for the main bar forging steps is determined based on the amount of bar deformation. The bar stock was subjected to high-temperature annealing according to the determined high-temperature annealing heating temperature and time before forging. According to the forging process, the high-temperature annealed bar stock is forged to obtain the required forgings; The forging is heat-treated according to its effective thickness; Based on the diameter of the bar stock, determine the high-temperature annealing heating temperature and time before forging, including: For bars with a diameter > 150 mm, the heating temperature is determined to be 470-500℃, and the holding time is 1.5 minutes / 1 mm for the smaller of the length and diameter. For bars with a diameter ≤150mm, the heating temperature is determined to be 440~470℃, and the holding time is 2 minutes / 1 mm for the smaller of the length and diameter. The number of forging processes for the main bar stock is determined based on the bar stock deformation, including: The deformation ε of the bar is calculated using the deformation calculation formula: ε=△L / L before △L = L_back - L_front; The dimensions before L are the dimensions before forging, the dimensions after L are the dimensions after forging, and △L is the difference in dimensions before and after forging. The number of heat treatments in the process is determined based on the deformation amount ε of the bar and the range of deformation per heat treatment. Among them, the deformation amount per heat treatment is controlled to avoid the coarse grain range of 5-15% and ≥75%, and the maximum deformation amount of hammer forging is ≤60%, and the maximum deformation amount of press is <75%. The method further includes: The bar stock after high-temperature annealing is heated before forging at a temperature of 440–460℃. When the diameter of the bar after high-temperature annealing is greater than 150 mm, the holding time shall be 1.5 minutes per millimeter, whichever is smaller between the length and the diameter. When the diameter of the bar after high-temperature annealing is ≤150 mm, the holding time is 2 minutes / 1 mm, whichever is smaller between the length and the diameter. The conventional forging method is adopted, the final forging temperature is ≥380℃, and the forging is air-cooled after support; During forging, hammering should be light, with each hammer blow causing no more than 5% of the deformation. Hammering should be slow, with a frequency of less than 2 times per second. Heat treatment includes quenching and artificial aging; For forgings with an effective thickness > 150 mm, the quenching temperature is 530-550℃, the holding time is 2 minutes / 1 mm, and then the forging is cooled to room temperature with boiling water. For forgings with an effective thickness ≤150mm, the heating temperature is 520~540℃, the holding time is 3 minutes / 1 mm, and then the forging is cooled to room temperature with boiling water. The artificial aging temperature is 190-199℃, and the temperature is maintained for 0.5-2 hours, followed by natural air cooling to room temperature.
Citation Information
Patent Citations
Novel forging process for skateboard support based on aluminum alloy with high strength and toughness
CN112846058A
Preparation method of high-alloying difficult-to-deform high-temperature alloy GH4151 disc forging
CN115722628A