A short process for preparing a high-strength copper-nickel-silicon alloy
By employing a short-process preparation method, including hot rolling, aging treatment, and deep cryogenic rolling, the complexity of producing Cu-Ni-Si alloy sheets and strips has been solved, enabling the preparation of high-strength and highly conductive copper-nickel-silicon alloys suitable for electronic applications such as lead frames.
Patent Information
- Application Number
- CN202410049473.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-12
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-01-12
AI Technical Summary
The existing Cu-Ni-Si alloy sheet and strip processing involves complex production processes, long workflows, unstable product quality, and difficulty in achieving both high strength and excellent conductivity, thus failing to meet the miniaturization and integration requirements in the lead frame field.
A short-process preparation method is adopted, including hot rolling after solution treatment, first aging treatment, deep cryogenic rolling and second aging treatment. By refining the grains, precipitating nanophases and generating deformable twins, the strength and conductivity of the material are improved.
While shortening the process flow, it significantly improves the strength and conductivity of copper-nickel-silicon alloys, meeting the high-performance requirements of electronic fields such as lead frames, and reducing material instability.
Smart Images

Figure CN117867425B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of copper alloy materials technology, and in particular to a short-process preparation method for high-strength copper-nickel-silicon alloys. Background Technology
[0002] As integrated circuits develop towards large-scale and ultra-large-scale applications, the lead frame materials used in integrated circuits are also developing towards finer lead pitches and more multi-pin designs. The integration density of semiconductor devices is also increasing, creating an urgent need for lead frame materials. Cu-Ni-Si alloys, due to their excellent strength, good conductivity, low manufacturing difficulty, and good processability, have become the most commonly used alloy materials for lead frames.
[0003] C70250 copper alloy products possess high strength, good electrical conductivity, resistance to high-temperature softening, and thermal relaxation, making them widely used in electronic fields such as lead frames, elastic elements, miniature terminals, and connector materials. C70250 copper alloy ingots are composed of the following elements: Ni: 2.2 4.2%, Si: 0.25 1.25%, Mg: 0.05 The composition is 0.3% Cu, ≥96.5%, with the remainder being unavoidable impurities. However, traditional Cu-Ni-Si alloy sheet and strip processing suffers from complex production processes, long workflows, unstable product quality, high surface roughness, and uneven sheet shape. Furthermore, the strength and conductivity of the processed material are often compromised, making it difficult to simultaneously achieve industrialization and meet the requirements of equipment miniaturization and integration. This severely hinders the application of Cu-Ni-Si alloys in the lead frame field. Therefore, to obtain a Cu-Ni-Si alloy with both high strength and excellent conductivity through a short and stable processing method, a short-process preparation method for high-strength copper-nickel-silicon alloy is provided. Summary of the Invention
[0004] The technical problem to be solved by this invention is how to prepare copper-nickel-silicon alloys with both high strength and excellent conductivity using a short process. In view of the defects in the prior art, a short process preparation method for high-strength copper-nickel-silicon alloys is provided.
[0005] To address the aforementioned technical problems, this invention provides a short-process preparation method for high-strength copper-nickel-silicon alloys, comprising the following steps: (1) The as-cast C70250 copper alloy is solution treated and then hot-rolled to obtain a hot-rolled copper alloy; (2) The hot-rolled copper alloy is subjected to a first aging treatment, deep cold rolling and a second aging treatment in sequence to obtain the high-strength copper-nickel-silicon alloy.
[0006] Preferably, in step (1): The solution treatment is performed at a temperature of 800~1000℃ for 1~3 hours.
[0007] Preferably, in step (1): The hot rolling process employs multi-pass rolling, with a total deformation of 50-60% and a single-pass deformation of 15-25%; the initial rolling temperature of the hot rolling is 800-1000℃; and / or After each rolling pass, the process also includes holding the hot-rolled material at its initial rolling temperature.
[0008] Preferably, in step (1): The hot rolling process is carried out in three passes, with a total deformation of 60% and a single pass deformation of 20%.
[0009] Preferably, in step (2): The temperature for the first aging treatment is 450~500℃, and the treatment time is 1~2 hours.
[0010] Preferably, in step (2): The deep cold rolling process employs multi-pass rolling, with a total deformation of 40-50% and a single-pass deformation of 5-10%; the initial rolling temperature of the deep cold rolling process is -200 to -150℃.
[0011] Preferably, in step (2): The deep cold rolling process is carried out in four passes, with a total deformation of 40% and a single pass deformation of 10%.
[0012] Preferably, in step (2): The second aging treatment is performed at a temperature of 450~500℃ for a time of 30~90 minutes.
[0013] Preferably, in step (2): The first aging treatment was performed at a temperature of 450°C for 1 hour; the second aging treatment was performed at a temperature of 500°C for 30 minutes.
[0014] Preferably, in step (2): The cooling medium for cryogenic rolling is one or both of liquid nitrogen and liquid helium.
[0015] Compared with the prior art, the present invention has at least the following beneficial effects: This invention provides a short-process preparation method for high-strength copper-nickel-silicon alloys. Based on solution treatment, as-cast C70250 copper alloy is hot-rolled, followed by a first aging treatment, cryogenic rolling, and a second aging treatment, ultimately yielding a copper-nickel-silicon alloy with both high strength and excellent electrical conductivity. In this way, after solution treatment, hot rolling directly refines the grains to a size conducive to deformation twin formation and minimizing grain boundary effects. Then, the first aging treatment uniformly precipitates supersaturated solution atoms, forming nanophases to increase the content of deformation twins. Finally, cryogenic rolling generates deformation twins, and the second aging treatment further improves the material's mechanical strength and electrical conductivity. Compared to traditional processes, the electrical conductivity remains essentially unchanged, while the strength of the copper alloy is significantly improved, and the process flow is shortened. Thus, the advantage of this invention's preparation process is that it can produce high-performance alloy materials with less deformation and a shorter rolling process, reducing the instability of alloy materials caused by excessive rolling steps. Attached Figure Description
[0016] Figure 1 This is a flowchart of a short-process preparation method for a high-strength copper-nickel-silicon alloy provided in an embodiment of the present invention; Figure 2 This is a metallographic image of the as-cast C70250 copper alloy provided by the present invention; Figure 3 This is a scanning electron microscope energy dispersive spectroscopy (EDS) image of the as-cast C70250 copper alloy provided by the present invention; Figure 4 These are the IPF diagram and recrystallization microstructure diagram of the hot-rolled copper alloy provided in Embodiment 1 of the present invention; wherein, (a) is the IPF diagram and (b) is the recrystallization microstructure diagram; Figure 5 These are IPF diagrams and Σ3 twin boundary distribution diagrams of the cryogenically rolled copper alloy provided in Example 1 and the room-temperature rolled copper alloy provided in Comparative Example 2; wherein (a) and (b) are IPF diagrams, and (c) and (d) are Σ3 twin boundary distribution diagrams. Figure 6 These are the IPF and KAM diagrams of the high-strength copper-nickel-silicon alloy provided in Embodiment 1 of the present invention; wherein, (a) is the IPF diagram and (b) is the KAM diagram; Figure 7 These are stress-strain diagrams of the high-strength copper-nickel-silicon alloy provided in Example 1 of the present invention and the copper-nickel-silicon alloys provided in Comparative Examples 2 and 3. Figure 8 This is a graph showing the change in electrical conductivity of the high-strength copper-nickel-silicon alloy provided in Example 1 of the present invention and the copper-nickel-silicon alloys provided in Comparative Examples 2 and 3 during the second aging process. Detailed Implementation
[0017] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0018] like Figure 1 As shown in the embodiment of the present invention, a short-process preparation method for a high-strength copper-nickel-silicon alloy is provided, which includes the following steps: Step (1): The as-cast C70250 copper alloy is solution treated and then hot-rolled to obtain a hot-rolled copper alloy; Step (2): The hot-rolled copper alloy is subjected to a first aging treatment, deep cold rolling and a second aging treatment in sequence to obtain a high-strength copper-nickel-silicon alloy.
[0019] In this invention, based on solution treatment, the as-cast C70250 copper alloy is hot-rolled, followed by a first aging treatment, cryogenic rolling, and a second aging treatment, ultimately yielding a copper-nickel-silicon alloy with both high strength and excellent electrical conductivity. Thus, this invention directly refines the grain size to a level conducive to deformation twin formation and minimizing grain boundary influence through hot rolling after solution treatment. Then, the first aging treatment uniformly precipitates supersaturated solution atoms, resulting in the precipitation of the nano-phase Ni2Si to increase the content of deformation twins. Finally, cryogenic rolling generates deformation twins, and the second aging treatment further improves the material's mechanical strength and electrical conductivity. Compared to traditional processes, the electrical conductivity is almost unchanged, while the strength of the copper alloy is significantly improved, and the process flow is shortened.
[0020] In this invention, Ni and Si elements can form Ni2Si. The precipitation of the Ni2Si phase improves the strength of the material without reducing the conductivity of the copper alloy, thus enabling the material to achieve high strength and high conductivity. Si is precipitated from the copper alloy matrix as much as possible to improve the alloy's conductivity, and Ni is precipitated as much as possible as a phase to further improve the alloy's conductivity.
[0021] According to some preferred embodiments, in step (1), the solution treatment temperature is 800~1000℃ (for example, it can be 800℃, 820℃, 850℃, 880℃, 900℃, 920℃, 950℃, 980℃ or 1000℃), and the time is 1~3h (for example, it can be 1h, 1.5h, 2h, 2.5h or 3h).
[0022] In this invention, the solution treatment temperature is limited to 800~1000℃ and the time is limited to 1~3h. This solution treatment can dissolve the coarse second phase of the as-cast C70250 copper alloy, preventing it from becoming a crack initiation and causing the alloy material to fracture during large deformation. On the other hand, it can also homogenize the solute elements, so as to avoid coarsening of the precipitate phase caused by solute enrichment during the aging process.
[0023] According to some preferred embodiments, in step (1), the hot rolling adopts multi-pass rolling, and the total deformation is 50-60% (for example, it can be 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59% or 60%), and the single-pass deformation is 15-25% (for example, it can be 15%, 16%, 18%, 20%, 21%, 22%, 24% or 25%); the initial rolling temperature of the hot rolling is 800-1000℃ (for example, it can be 800℃, 820℃, 850℃, 880℃, 900℃, 920℃, 950℃, 980℃ or 1000℃).
[0024] According to some preferred embodiments, in step (1), after each rolling pass, a heat holding period is performed at the initial rolling temperature of the hot roll. Preferably, the heat holding time is 5 to 10 minutes.
[0025] In this invention, after each hot rolling pass, the hot-rolled alloy is returned to the furnace for heat preservation to eliminate the hot-rolled texture. Heat preservation ensures that the initial grains are not too small, while making the solid solution atoms more uniform. At the same time, restoring the hot rolling temperature to the initial rolling temperature is beneficial for re-hot rolling.
[0026] According to some preferred embodiments, in step (1), the hot rolling is carried out in three passes, with a total deformation of 60% and a single pass deformation of 20%.
[0027] In this invention, hot rolling is performed directly after solution treatment to break up the coarse grains of the as-cast C70250 copper alloy, eliminate casting defects, and refine the grains to a suitable size that facilitates the formation of deformation twins and minimizes the influence of grain boundaries. Simultaneously, the multi-pass rolling process is more conducive to the formation of stable deformation twins in subsequent manufacturing processes, thereby further improving the strength of the copper-nickel-silicon alloy.
[0028] In this invention, experiments have confirmed that if the total deformation of hot rolling is less than 50%, the low deformation amount cannot produce sufficiently fine grains; if the total deformation of hot rolling is greater than 60%, the grain size is difficult to control, heat loss is high, and rolling costs will increase. Meanwhile, if the deformation per pass is less than 15%, the low energy storage is not conducive to the formation of fine recrystallized grains; if the deformation per pass is greater than 25%, the equipment requirements are high, and grain growth is likely to occur during the heat preservation process.
[0029] According to some preferred embodiments, in step (2), the temperature of the first aging treatment is 450~500℃ (for example, it can be 450℃, 455℃, 460℃, 465℃, 470℃, 475℃, 480℃, 485℃, 490℃, 495℃ or 500℃), and the treatment time is 1~2h (for example, it can be 1h, 1.2h, 1.5h, 1.6h, 1.8h or 2h).
[0030] In this invention, a first aging treatment initially and uniformly precipitates saturated solid solution atoms, forming a nanophase to improve electrical conductivity and facilitate subsequent dislocation pinning and deformation twin formation. Experiments have shown that if the aging temperature of the first treatment is too low, the amount of second phase precipitated will be insufficient, resulting in lower electrical conductivity of the final processed copper alloy. Conversely, if the aging temperature is too high, it will affect the size of the precipitated second phase, making it coarse and uneven, thus affecting the content of deformation twins and leading to poor mechanical strength in the final prepared copper alloy.
[0031] According to some preferred embodiments, in step (2), the cryogenic rolling adopts multi-pass rolling, with a total deformation of 40-50% (for example, it can be 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49% or 50%), and a single-pass deformation of 5-10% (for example, it can be 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5% or 10%); the starting rolling temperature of the cryogenic rolling is -200~-150℃ (for example, it can be -200℃, -190℃, -180℃, -170℃, -160℃ or -150℃).
[0032] In this invention, experiments have confirmed that if the total deformation of cryogenic rolling is less than 40%, the deformation is too low, resulting in low strength of the final copper-nickel-silicon alloy. If the total deformation of cryogenic rolling is greater than 50%, self-annealing is likely to occur during the rolling process, affecting the aging effect. Furthermore, if the deformation per pass is less than 5%, deformation twins are less likely to form; if the deformation per pass is greater than 10%, self-annealing will occur, causing the stored energy during deformation to be released, leading to a reduction in precipitated phases during subsequent aging, and consequently, lower electrical conductivity and mechanical strength.
[0033] According to some preferred embodiments, in step (2): Deep cold rolling adopts four-pass rolling, with a total deformation of 40% and a single-pass deformation of 10%.
[0034] According to some preferred embodiments, in step (2), the temperature of the second aging treatment is 450~500℃ (for example, it can be 450℃, 455℃, 460℃, 465℃, 470℃, 475℃, 480℃, 485℃, 490℃, 495℃ or 500℃), and the treatment time is 30~90min (for example, it can be 30min, 40min, 45min, 50min, 60min, 70min, 80min or 90min).
[0035] In this invention, experiments have shown that if the aging temperature of the second aging treatment is too low, it will affect the amount of the second phase precipitated, resulting in a lower electrical conductivity of the final processed copper alloy; if the aging temperature is too high, the precipitated second phase will be uneven, affecting the content of deformed twins, resulting in poor mechanical strength of the final prepared copper alloy.
[0036] According to some preferred embodiments, in step (2), the cooling medium for cryogenic rolling is one or both of liquid nitrogen and liquid helium.
[0037] This invention does not impose any particular restrictions on the equipment used for cryogenic rolling.
[0038] To more clearly illustrate the technical solution and advantages of the present invention, a short-process preparation method for a high-strength copper-nickel-silicon alloy is described in detail below through several embodiments.
[0039] The composition of the as-cast C70250 copper alloy used in the following examples and comparative examples is as follows: Ni: 2.6%, Si: 0.5%, Mg: 0.2%, Cu: ≥96.5%, with the remainder being unavoidable impurities; room temperature is 25°C.
[0040] Example 1 (1) After the as-cast C70250 copper alloy with a thickness of 20mm was solution treated at 900℃ for 1h, it was directly hot rolled to obtain hot-rolled copper alloy. Hot rolling process: A total of 3 hot rolling passes are performed, with a reduction of 4 mm in each pass, i.e., a single pass deformation of 20%. After each pass, the alloy is returned to the furnace and held for 5 minutes to restore the initial rolling temperature of 900℃. After a total of 3 reductions (total deformation of 60%), the alloy is held at 900℃ for 10 minutes to eliminate the hot rolling texture, resulting in a hot-rolled copper alloy with a thickness of 8 mm. (2) After the hot-rolled copper alloy is cooled to room temperature by water, it is aged at 450°C for 1 hour to obtain a pre-rolled copper alloy; the pre-rolled copper alloy is placed in liquid nitrogen for cooling. After cooling for 20 minutes, the copper alloy can be reduced to the temperature of liquid nitrogen. Then, after deep cryogenic rolling, it is aged at 500°C for 30 minutes to obtain a high-strength copper-nickel-silicon alloy. Cryogenic rolling process: A total of 4 rolling passes are performed, with a reduction of 0.8 mm per pass, which is a deformation of 10%. After each rolling, the material is placed back into liquid nitrogen for 5 minutes to cool. This process is repeated four times, resulting in a total deformation of 40%, and a high-strength copper-nickel-silicon alloy with a thickness of 4.8 mm is obtained.
[0041] Example 2 Example 2 is basically the same as Example 1, except that: (1) After the as-cast C70250 copper alloy with a thickness of 20mm was solution treated at 800℃ for 3h, it was directly hot rolled to obtain hot-rolled copper alloy. Hot rolling process: A total of 4 passes of hot rolling are performed, with a reduction of 3 mm in each pass, i.e., a single pass deformation of 15%. After each pass, the alloy is returned to the furnace and held for 5 minutes to restore the initial rolling temperature to 800℃. After a total of 4 reductions (total deformation of 60%), the alloy is held at 800℃ for 10 minutes to eliminate the hot rolling texture, resulting in a hot-rolled copper alloy with a thickness of 8 mm.
[0042] Example 3 Example 3 is basically the same as Example 1, except that: (1) After the as-cast C70250 copper alloy with a thickness of 20mm was solution treated at 900℃ for 1h, it was directly hot rolled to obtain hot-rolled copper alloy. Hot rolling process: A total of 2 passes of hot rolling are performed, with a reduction of 5 mm in each pass, i.e., a single pass deformation of 25%. After each pass, the alloy is returned to the furnace and held for 5 minutes to restore the initial rolling temperature of 900℃. After a total reduction of 50% (two passes), the alloy is held at 900℃ for 10 minutes to eliminate the hot rolling texture, resulting in a hot-rolled copper alloy with a thickness of 10 mm.
[0043] Example 4 Example 4 is basically the same as Example 1, except that the temperature of the first aging treatment before cryogenic rolling is 500°C and the time is 1 hour.
[0044] Example 5 Example 5 is basically the same as Example 1, except that the cryogenic rolling process in step (2) is different: Cryogenic rolling process: A total of 5 rolling passes are performed, with a reduction of 0.8 mm per pass, which is a deformation of 10%. After each rolling, the material is placed back into liquid nitrogen for 5 minutes to cool. This process is repeated five times, resulting in a total deformation of 50%, and a high-strength copper-nickel-silicon alloy with a thickness of 4 mm is obtained.
[0045] Example 6 Example 6 is basically the same as Example 1, except that the aging treatment after cryogenic rolling in step (2) is carried out at 450°C for 90 minutes.
[0046] Example 7 Example 7 is basically the same as Example 1, except that the cryogenic rolling process in step (2) is different: Cryogenic rolling process: A total of 6 rolling passes are performed. In the first five passes, the thickness is reduced by 0.8 mm in each pass, which is 10% of the deformation. After each rolling, the material is cooled in liquid nitrogen for 5 minutes. This process is repeated five times. In the last pass, the thickness is reduced by 0.4 mm, which is 55% of the deformation, resulting in a high-strength copper-nickel-silicon alloy with a thickness of 3.6 mm.
[0047] Comparative Example 1 As-cast C70250 copper alloy.
[0048] Comparative Example 2 Comparative Example 2 is basically the same as Example 1, except that: (2) After the hot-rolled copper alloy is cooled to room temperature, it is aged at 450°C for 1 hour to obtain a pre-rolled copper alloy; the pre-rolled copper alloy is rolled at room temperature and then aged at 500°C for 30 minutes to obtain a high-strength copper-nickel-silicon alloy. Room temperature rolling process: A total of 4 rolling passes are performed at room temperature, with a reduction of 0.8 mm per pass, which is 10% of the deformation. This process is repeated four times, resulting in a total deformation of 40%, to obtain a high-strength copper-nickel-silicon alloy with a thickness of 4.8 mm.
[0049] Comparative Example 3 (1) After the as-cast C70250 copper alloy with a thickness of 20mm was solution treated at 900℃ for 1h, it was directly hot rolled to obtain hot-rolled copper alloy. Hot rolling process: A total of 3 hot rolling passes are performed, with a reduction of 4 mm in each pass, i.e., a single pass deformation of 20%. After each pass, the alloy is returned to the furnace and held for 5 minutes to restore the initial rolling temperature of 900℃. After a total of 3 reductions (total deformation of 60%), the alloy is held at 900℃ for 10 minutes to eliminate the hot rolling texture, resulting in a hot-rolled copper alloy with a thickness of 8 mm. (2) After the hot-rolled copper alloy is cooled to room temperature, it is rolled at room temperature and then aged at 450°C for 1 hour to obtain a high-strength copper-nickel-silicon alloy. Room temperature rolling process: A total of 22 rolling passes are performed, with the deformation amount of each pass being 10% of the previous pass, that is, the total deformation amount is 90.15%, and finally a high-strength copper-nickel-silicon alloy with a thickness of 0.79mm is obtained.
[0050] Comparative Example 4 Comparative Example 4 is basically the same as Example 1, except that step (2) was not aged before cryogenic rolling; (2) After the hot-rolled copper alloy is cooled to room temperature by water, it is placed in liquid nitrogen for cooling. After cooling for 20 minutes, the copper alloy can be reduced to the temperature of liquid nitrogen. Then, after deep cryogenic rolling, it is aged at 500℃ for 30 minutes to obtain a high-strength copper-nickel-silicon alloy. Cryogenic rolling process: A total of 4 rolling passes are performed, with a reduction of 0.8 mm per pass, which is a deformation of 10%. After each rolling, the material is placed back into liquid nitrogen for 5 minutes to cool. This process is repeated four times, resulting in a total deformation of 40%, and a high-strength copper-nickel-silicon alloy with a thickness of 4.8 mm is obtained.
[0051] Comparative Example 5 Comparative Example 5 is basically the same as Example 1, except that: (2) After the hot-rolled copper alloy is cooled to room temperature by water, it is aged at 450°C for 1 hour to obtain a pre-rolled copper alloy; the pre-rolled copper alloy is placed in liquid nitrogen for cooling. After cooling for 20 minutes, the copper alloy can be reduced to the temperature of liquid nitrogen. Then, after deep cryogenic rolling, it is aged at 500°C for 30 minutes to obtain a high-strength copper-nickel-silicon alloy. Cryogenic rolling process: A total of 2 rolling passes are performed, with a reduction of 1.6 mm per pass, which is a deformation of 20%. After each rolling, the material is placed back into liquid nitrogen for 5 minutes to cool. This process is repeated twice, resulting in a total deformation of 40%, and a high-strength copper-nickel-silicon alloy with a thickness of 4.8 mm is obtained.
[0052] Comparative Example 6 Comparative Example 6 is basically the same as Example 1, except that: step (2) did not undergo a second aging treatment after cryogenic rolling; (2) After the hot-rolled copper alloy is cooled to room temperature by water, it is aged at 450°C for 1 hour to obtain a pre-rolled copper alloy. The pre-rolled copper alloy is placed in liquid nitrogen for cooling. After cooling for 20 minutes, the copper alloy can be reduced to the temperature of liquid nitrogen. Then, it is subjected to deep cryogenic rolling to obtain a high-strength copper-nickel-silicon alloy. Cryogenic rolling process: A total of 2 rolling passes are performed, with a reduction of 1.6 mm per pass, which is a deformation of 20%. After each rolling, the material is placed back into liquid nitrogen for 5 minutes to cool. This process is repeated twice, resulting in a total deformation of 40%, and a high-strength copper-nickel-silicon alloy with a thickness of 4.8 mm is obtained.
[0053] Comparative Example 7 Comparative Example 7 is basically the same as Example 1, except that: (1) After the as-cast C70250 copper alloy with a thickness of 20mm was solution treated at 900℃ for 1h, it was directly hot rolled to obtain hot-rolled copper alloy. Hot rolling process: A total of 4 passes of hot rolling are performed, with a reduction of 4 mm in each pass, that is, a single pass deformation of 80%. After each pass, the alloy is returned to the furnace and held for 5 minutes to restore the initial rolling temperature of 900℃. After a total of 4 reductions (total deformation of 80%), the alloy is held at 900℃ for 10 minutes to eliminate the hot rolling texture, resulting in a hot-rolled copper alloy with a thickness of 6 mm.
[0054] The copper-nickel-silicon alloy products obtained from the above embodiments and comparative examples were tested for hardness, ultimate tensile strength and elongation. The test results are shown in Table 1.
[0055] Specifically, the hardness of the copper-nickel-silicon alloy product was tested using a Vickers hardness tester with a sample size of 10×10×2mm; the tensile properties of the copper-nickel-silicon alloy product were tested using an electronic universal tensile tester with a gauge length of 8×2×1mm and a tensile speed of 0.2mm / min; and the conductivity of the copper-nickel-silicon alloy product at room temperature was tested using a Sigma 2008B eddy current conductivity tester with a sample size of 10×10×2mm.
[0056] Table 1
[0057] Metallographic structure and scanning electron microscopy (SEM) energy dispersive spectroscopy (EDS) analysis were performed on the as-cast C70250 copper alloy used in the embodiments and comparative examples of this invention. Figure 2 The metallographic image shown indicates that the as-cast C70250 copper alloy exhibits distinct millimeter-scale coarse equiaxed grains, with a grain size of approximately 2 mm; as shown... Figure 3 The EDS diagram shown indicates that the as-cast C70250 copper alloy contains numerous as-cast defects such as porosity, and also contains a large amount of micron-sized second phases formed by Ni and Si enrichment.
[0058] The hot-rolled copper alloy obtained in step (1) of Example 1 was observed using backscattered electron diffraction (EBSD) to examine the grain morphology after hot rolling and the microstructure of the alloy after preliminary deformation, as shown below. Figure 4 The EBSD inverse pole diagram and recrystallization microstructure are shown. Among them, [the following is a description of the structure / structure]. Figure 4 It is known that the microstructure of the hot-rolled copper alloy with a hot-rolled deformation of 60% after solution treatment is mainly composed of approximately equiaxed grains, and also contains some annealing twins. The average grain size is 95.61 μm. No obvious impurities and defects were observed in the hot-rolled copper alloy prepared by the preparation method used in this invention. The recrystallized microstructure is conducive to the accumulation of energy storage during subsequent deformation and has the potential to generate deformation twins.
[0059] The preliminary rolled copper alloys obtained in step (2) of Example 1 and Comparative Example 2 were characterized to obtain the following results: Figure 5 The IPF diagrams and Σ3 twin boundary distribution diagrams of copper alloys after cryogenic rolling and room temperature rolling are shown. Figure 5 It can be seen that when the total deformation is 40%, the grains compress and elongate along the rolling direction. From a macroscopic perspective, the grain compression phenomenon in copper alloys during room temperature rolling and cryogenic rolling is quite similar. However, cryogenic rolling deformation produces a large number of lamellar deformation twins due to the activation of twins, while room temperature rolling deformation produces more deformation bands. Since grain boundaries hinder dislocations, the appearance of twin boundaries can improve the strength of the alloy material.
[0060] Figure 6 The microstructure of the high-strength copper-nickel-silicon alloy material obtained in Example 1 after aging treatment-cryogenic rolling-aging treatment shows that it is similar to... Figure 5 In contrast, the alloy material after the second aging treatment still retains the original deformed grain morphology, and the deformed twins generated by deep cryogenic rolling still exist stably, thus playing a key role in improving strength.
[0061] Figure 7 Table 1 shows the stress-strain diagrams of C70250 copper alloy under different rolling processes, with specific values as shown in Table 1. Comparative Examples 2 and 3 show that, under room temperature rolling, greater deformation results in better work hardening and precipitation strengthening due to higher stored energy. The alloy material aged at 90% deformation peak value has higher strength than the alloy material aged at 40% deformation peak value. Furthermore, the alloy material with obvious deformation twins in Example 1 showed significantly improved mechanical properties compared to the alloy material rolled at room temperature. After the second aging treatment, the high-strength copper-nickel-silicon alloy obtained in Example 1 showed a 24.96% increase in tensile strength compared to the copper-silicon-nickel alloy obtained in Comparative Example 3, reaching 866 MPa. Simultaneously, the elongation reached 12.1%, showing a significant advantage over Comparative Examples 2 and 3.
[0062] It should be noted that, for Comparative Example 3, if the alloy is aged at 500°C for 1 hour after room temperature rolling, softening will occur; while the alloy material obtained after room temperature rolling and aging at 450°C for 1 hour has the best performance.
[0063] Figure 8 This refers to the electrical conductivity of C70250 copper alloy during the second aging process under different rolling processes. Figure 8 It can be seen that the conductivity of the copper alloy materials prepared in Comparative Example 2 and Example 1 is 34.5% IACS and 36.3% IACS, respectively. The conductivity of the copper alloy material prepared by cryogenic rolling is better than that of the copper alloy material rolled at room temperature, which illustrates the balancing effect of deformation twins on mechanical and electrical properties. Therefore, the high-strength copper-nickel-silicon alloy prepared by this invention achieves a synergistic improvement in mechanical and electrical properties. The presence of deformation twins significantly enhances the mechanical properties, meeting the increasing strength requirements.
[0064] In this invention, as summarized above, the generated deformed twins modulate the resistivity of copper-nickel-silicon alloys through microscopic grain boundary structural characteristics. Because the atomic arrangement in the grain boundary region differs significantly from that within the grain, this structural change leads to periodic fluctuations in the atomic potential at the grain boundary, affecting the electron transport path. Electrons are scattered as they pass through these potential walls, increasing the resistivity of the alloy material. However, twin boundaries typically maintain a high degree of coherence with adjacent matrix grains, with almost no structural defects such as dislocations. This results in a resistivity of twin boundaries that is far lower than that of ordinary grain boundaries, down to an order of magnitude. Simultaneously, twin boundaries act as effective barriers to dislocation movement, promoting grain size reduction. This grain refinement process significantly improves the strength of the alloy material. Furthermore, the presence of deformed twins enhances the work hardening ability of the alloy material, improves the uniformity during deformation, reduces local stress concentration during deformation, thus delaying necking and further improving the uniform elongation of the alloy material. Therefore, deformed twin boundaries not only reduce resistivity but also significantly enhance the mechanical properties of the alloy material.
[0065] It should be noted that, in Figure 7 and Figure 8 In this context, RTR represents room temperature rolling in Comparative Examples 2 and 3, CR represents cryogenic rolling in Example 1, and A represents the first aging treatment.
[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A short-process preparation method for a high-strength copper-nickel-silicon alloy, characterized in that, The method includes the following steps: (1) The as-cast C70250 copper alloy is solution treated and then hot rolled to obtain a hot-rolled copper alloy; the solution treatment temperature is 800~1000℃ and the time is 1~3h; the hot rolling adopts multi-pass rolling, the total deformation is 50~60%, and the single-pass deformation is 15~25%; the initial rolling temperature of the hot rolling is 800~1000℃; (2) The hot-rolled copper alloy is subjected to a first aging treatment, a deep cryogenic rolling process, and a second aging treatment in sequence to obtain the high-strength copper-nickel-silicon alloy. The temperature of the first aging treatment is 450~500℃ and the treatment time is 1~2 h. The deep cryogenic rolling process adopts multi-pass rolling with a total deformation of 40~50% and a single-pass deformation of 5~10%. The starting rolling temperature of the deep cryogenic rolling process is -200℃ to -150℃. The temperature of the second aging treatment is 450~500℃ and the treatment time is 30~90 min.
2. The preparation method according to claim 1, characterized in that, In step (1): After each rolling pass, the process also includes holding the hot-rolled material at its initial rolling temperature.
3. The preparation method according to claim 1, characterized in that, In step (1): The hot rolling process is carried out in three passes, with a total deformation of 60% and a single pass deformation of 20%.
4. The preparation method according to claim 1, characterized in that, In step (2): The deep cold rolling process is carried out in four passes, with a total deformation of 40% and a single pass deformation of 10%.
5. The preparation method according to claim 1, characterized in that, In step (2): The first aging treatment was performed at a temperature of 450°C for 1 hour; the second aging treatment was performed at a temperature of 500°C for 30 minutes.
6. The preparation method according to any one of claims 1 to 5, characterized in that, In step (2): The cooling medium for cryogenic rolling is one or both of liquid nitrogen and liquid helium.
Citation Information
Patent Citations
Production technology for high-strength and high-conductivity copper-nickel-silicon alloy
CN107794406A