Ni-doped anti-carbon deposition SOFC anode material, and preparation method and application thereof

CN117878338BActive Publication Date: 2026-11-20CHANGCHUN UNIV OF SCI & TECH +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311657791.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-06
Publication Date
2026-11-20
Estimated Expiration
2043-12-06

AI Technical Summary

Technical Problem

经过前人大量的实验数据证明,钙钛矿型阳极材料具有优异的抗积碳性能,其中SrMoO3基材料本身具有很好的导电性能且目前对该材料的研究探索相对较少

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117878338B_ABST
    Figure CN117878338B_ABST
Patent Text Reader

Abstract

The application discloses a kind of Ni doped anti-carbon SOFC anode material and its preparation method and application.The material of the application is with Sr 2+ Containing nitrate, containing Mo 6+ Nitrate, containing Ni 2+ Nitrate as raw material, is prepared by sol-gel method.The chemical formula of the material of the application is SrMo 1‑x Ni x O 3‑δ (0<x≤0.2).The compatibility of the material of the application and buffer layer material Ce 0.8 Sm 0.2 O 1.9 Good, with the solid oxide fuel cell made of the material of the application has good electrochemical performance in hydrogen atmosphere, has good structural stability in methane atmosphere.The material of the application is simple to prepare, and has good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solid oxide fuel cells, and relates to a Ni-doped carbon deposition resistant SOFC anode material, its preparation method and application. Background Art

[0002] Energy crisis and environmental pollution are two major obstacles that the healthy and rapid development of human society can never avoid. With the development of human society to the present, the two major problems of fossil resource depletion and exhaust pollution generated by fossil resource combustion have become increasingly prominent, and the development of clean, environmentally friendly and sustainable low-carbon energy technologies has attracted much attention. Compared with nuclear energy, an energy technology with great potential risks, solid oxide fuel cells (SOFCs) are much more stable and safe. They can directly convert the chemical energy in fuel into electric energy in one step, avoiding the energy loss caused by multiple conversions. The energy conversion process is not limited by the Carnot cycle, and has a very high energy conversion efficiency, thus attracting much attention in the field of new energy material development in recent years.

[0003] As an important component of SOFCs, the anode material has a great impact on the overall performance of the cell. When the traditional anode (Ni / YSZ) operates for a long time in alkane fuels such as CH4, carbon deposition is prone to occur on its surface, which will greatly reduce the output performance of the cell. Therefore, it is of great significance to develop solid oxide fuel cell anode materials with carbon deposition resistance and high performance. A large amount of previous experimental data has proved that perovskite-type anode materials have excellent carbon deposition resistance, among which SrMoO3-based materials themselves have good electrical conductivity and there are relatively few researches and explorations on such materials at present. The material of the present invention has a stable single perovskite structure under both methane and hydrogen atmospheres. The solid oxide fuel cell prepared from the material of the present invention has good performance under hydrogen, and can resist carbon deposition to a certain extent. Contents of the Invention

[0004] One of the objectives of the present invention is to provide a Ni-doped carbon deposition resistant SOFC anode material.

[0005] The second objective of the present invention is to provide the preparation method and application of the above Ni-doped carbon deposition resistant SOFC anode material.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: a Ni-doped carbon deposition resistant SOFC anode material, the chemical formula of the material is SrMo 1-x Ni x O 3-δ (0<x≤0.2), where δ in the formula is a value that ensures the electrical neutrality of the material.

[0007] The present invention also provides the preparation method of the above Ni-doped carbon deposition resistant SOFC anode material, which specifically includes the following steps: (1) According to the chemical formula SrMo 1-x Ni x O 3-δ (0<x≤0.2), the nitrates containing Sr 2+ , the nitrates containing Mo 6+ , and the nitrates containing Ni 2+ are respectively weighed according to the stoichiometric ratio of the corresponding metal elements; (2) The medicines weighed in step (1) are sequentially placed into a beaker, dissolved with deionized water, then a certain proportion of citric acid is weighed and added into the beaker, fully dissolved with deionized water to obtain a clear solution, ammonia water is added to adjust the pH of the solution to neutral, after stirring for a short time the solution becomes turbid, and an appropriate amount of nitric acid is added until the solution is clear. Subsequently, the solution is placed on a heating and stirring table to evaporate the solvent to dryness, and finally combustion occurs, and the obtained powder is collected; (3) The powder obtained in step (2) is fully ground in a mortar, the powder is collected into a crucible, the crucible is placed in a muffle furnace, and calcined at 600 to 800° C. for 10 to 12 hours in an air atmosphere; (4) The powder calcined in step (3) is fully ground in a mortar, and then an appropriate amount is taken and placed into a mold to be pressed into a sheet; (5) The sheet pressed in step (4) is placed into a high-temperature furnace, and calcined at 1050 to 1150° C. for 9 to 11 hours in an air atmosphere; (6) The calcined sheet from step (5) is taken out, cooled and placed into a test furnace, and calcined at 800 to 900° C. for 3 to 4 hours in a hydrogen atmosphere; (7) The calcined sheet from step (6) is placed in a mortar to be ground, absolute ethanol is added for full grinding, and after drying, SrMo 1-x Ni x O 3-δ (0<x≤0.2) solid oxide fuel cell anode electrode powder is obtained;

[0008] Preferably, the nitrate containing Sr 2+ used in step (1) is Sr(NO3)2, the nitrate containing Mo 6+ is H 24 Mo7N6O 24 ·4H2O, and the nitrate containing Ni 2+ is Ni(NO3)2·6H2O.

[0009] Preferably, the amount of citric acid weighed in step (2) is such that the ratio of citric acid to metal ions is 1.5:1;

[0010] Preferably, the specific method for tableting used in step (4) is to place an appropriate amount of powder into a mold with a diameter of 13 mm, and press it into a sheet under a pressure of 2 MPa.

[0011] The present invention further provides a solid oxide fuel cell fabricated using the Ni-doped carbon deposition resistant SOFC anode material, which is characterized by specifically comprising the following steps: (1) Weigh an appropriate amount of the SrMo prepared as described above 1-x Ni x O 3-δ (0<x≤0.2) solid oxide fuel cell anode electrode powder in a mortar, add a certain amount of binder, and grind uniformly to prepare an anode electrode slurry; (2) Weigh an appropriate amount of SmBaCo2O 5+δ cathode powder in a mortar, add a certain amount of binder, and grind uniformly to prepare a cathode electrode slurry; (3) Then weigh an appropriate amount of Ce 0.8 Sm 0.2 O 1.9 buffer layer powder in a mortar, add a certain amount of binder, and grind uniformly to prepare a buffer layer slurry; (4) Uniformly coat the buffer layer slurry prepared in step (3) on one side of the electrolyte sheet La by a screen printing method 0.9 Sr 0.1 Ga 0.8 Mg 0.2 O 2.85 , and place it on a baking oven to dry for 8 to 10 minutes; (5) Place the dried electrolyte sheet obtained above in a high-temperature tube furnace, and calcine it for 1 to 3 hours at 900 to 1000°C under N2 atmosphere to obtain a pre-material for fabricating a full cell; (6) Uniformly coat the electrode slurries prepared in steps (1) and (2) on both sides of the pre-material electrolyte La 0.9 Sr 0.1 Ga 0.8 Mg 0.2 O 2.85 and the buffer layer Ce 0.8 Sm 0.2 O 1.9 respectively, and dry to obtain a full cell sheet; (7) Place the dried full cell sheet obtained in step (6) in a high-temperature tube furnace, and calcine it for 1 to 3 hours at 900 to 1000°C under N2 atmosphere to obtain a solid oxide fuel cell using the SrMo 1-x Ni x O 3-δ (0<x≤0.2) material as the anode material.

[0012] Preferably, the SrMo used in step (1) 1-x Ni x O 3-δ(0<x≤0.2) The mass ratio of the anode powder to the binder is 1:1.5; the binder used is prepared by mixing terpineol and ethyl cellulose at a mass ratio of 9:1.

[0013] Preferably, in step (2), the electrolyte sheet La 0.9 Sr 0.1 Ga 0.8 Mg 0.2 O 2.85 has a thickness of 0.3 mm.

[0014] The present invention provides a Ni-doped carbon deposition resistant SOFC anode material, its preparation method and application. In terms of chemical composition, the chemical formula of the anode material is SrMo 1-x Ni x O 3-δ (0<x≤0.2), which has a single perovskite structure. The compatibility test results show that this anode material has good chemical compatibility with the buffer layer material Ce 0.8 Sm 0.2 O 1.9 and has a stable single perovskite structure under hydrogen. The SrMoO3-based perovskite material itself has very high electrical conductivity and good catalytic activity for hydrogen, but this material will be oxidized to the insulator SrMoO in air 4-δ , thus exhibiting low catalytic activity for methane. Studies have found that B-site doping can improve the catalytic activity of the material. In the present invention, Ni is used to partially substitute Mo at the B-site of the SrMoO 3-δ perovskite material, which significantly improves the electrochemical performance of the SrMoO3-based anode material, and the solid oxide fuel cell prepared from this doped material exhibits good carbon deposition resistance.

[0015] The example results show that, for the Ni-doped carbon deposition resistant SOFC anode material provided by the present invention, characterized by XRD, neither the intermediate synthesized in air nor the final product synthesized under hydrogen has impurity peaks, and they exhibit a stable tetragonal phase structure and a cubic phase structure respectively; the solid oxide fuel cell prepared with the preferred anode material provided by the present invention has a maximum output power of 851 mW cm at 850°C under H2 atmosphere -2 , and a maximum output power of 193 mW cm at 900°C under CH4 atmosphere -2 , which shows that this material has excellent electrochemical performance and good carbon deposition resistance. Brief Description of the Drawings

[0016] Figure 1 is the XRD pattern of the intermediate SrMo synthesized in air 0.95 Ni 0.05 O 4-δ .

[0017] Figure 2 SrMo monoperovskite after hydrogen reduction 0.95 Ni 0.05 O 3-δ XRD pattern.

[0018] Figure 3 To use the material SrMo of the present invention 0.95 Ni 0.05 O 3-δ Power density diagram of a full cell fabricated using the anode material in an H2 atmosphere.

[0019] Figure 4 To use the material SrMo of the present invention 0.95 Ni 0.05 O 3-δ Power density diagram of a full cell fabricated using the anode material in a CH4 atmosphere. Detailed Implementation

[0020] The present invention will be further described in detail below with reference to the accompanying drawings and specific implementation steps, but the present invention is not limited to the following examples.

[0021] This invention provides a method for preparing a Ni-doped anti-carbon-deposition SOFC anode material, specifically including the following steps: (1) Add Sr(NO3)2 and H 24 Mo7N6O 24 Weigh the raw materials ·4H2O and Ni(NO3)2·6H2O in a molar ratio of 1:0.14:0.05; (2) Place the weighed drugs obtained in step (1) into beakers in sequence, dissolve them with deionized water, then weigh citric acid according to the ratio of metal ions to citric acid 1:1.5 and add it to the beakers. Dissolve it completely with deionized water to obtain a clear solution. Adjust the pH to 7 with ammonia water. After stirring for 5 minutes, the solution becomes turbid. Then add 10 mL of nitric acid until the solution becomes clear. Then place the solution on a heating and stirring table to evaporate the solvent. Finally, it burns and the powder obtained is collected. (3) After grinding the powder obtained in step (2) in a mortar, collect the powder into a crucible, put the crucible into a muffle furnace, and calcine it at 600°C for 12 hours in an air atmosphere. (4) After grinding the powder calcined in step (3) in a mortar, weigh 0.3g of the powder and put it into a mold with a diameter of 13mm. Press it into a sheet with a pressure of 2MPa. (5) Place the pressed sheet from step (4) into a high-temperature furnace and calcine it at 1050°C for 10 hours in an air atmosphere; (6) Take out the calcined piece from step (5), cool it and put it into the test furnace, calcining it at 850°C for 4 hours in a hydrogen atmosphere; (7) The calcined slices from step (6) were placed in a mortar and ground, anhydrous ethanol was added and ground thoroughly, and then dried under a heat lamp to obtain SrMo. 0.95 Ni 0.05 O 3-δ Solid oxide fuel cell anode electrode powder;

[0022] A solid oxide fuel cell prepared using a Ni-doped, carbon-resistant SOFC anode material is characterized by comprising the following steps: (1) Weigh an appropriate amount of the SrMo obtained above. 0.95 Ni 0.05 O 3-δ Solid oxide fuel cell anode electrode powder is placed in a mortar, and a certain amount of binder is added (the mass ratio of anode powder to binder is 1:1.5; the binder is prepared by mixing terpineol and ethyl cellulose in a mass ratio of 9:1) and ground evenly to form an anode electrode slurry. (2) Weigh out an appropriate amount of SmBaCo2O 5+δ Cathode powder is placed in a mortar, a certain amount of binder is added, and the mixture is ground evenly to prepare a cathode electrode slurry (SmBaCo2O). 5+δ The cathode powder was prepared by solid-state method and sintered at 1150℃ for 10 hours. (3) Weigh out an appropriate amount of Ce 0.8 Sm 0.2 O 1.9 The buffer layer powder is placed in a mortar, a certain amount of binder is added and it is ground evenly to make a buffer layer slurry (the buffer layer material is prepared by sol-gel method and sintered at 800℃ for 2 hours). (4) The buffer layer slurry obtained in step (3) above is uniformly coated onto the 0.3mm electrolyte sheet La using screen printing. 0.9 Sr 0.1 Ga 0.8 Mg 0.2 O 2.85 One side is placed on an oven to dry for 8 minutes (the electrolyte sheet is sintered at 1400℃ for 10 hours using a dry pressing method to form a dense LSGM electrolyte sheet); (5) The dried electrolyte sheet was placed in a high-temperature tube furnace and calcined at 950°C for 2 hours under N2 atmosphere to obtain the pre-material for making a full battery. (6) The electrode slurry obtained in steps (1) and (2) is uniformly coated onto the electrolyte La, the precursor material, respectively. 0.9 Sr 0.1 Ga 0.8 Mg 0.2 O 2.85 and buffer layer Ce 0.8 Sm 0.2 O1.9 Both sides are dried to obtain full battery cells; (7) The dried full cell from step (6) is placed in a high-temperature tube furnace and calcined at 950°C for 2 hours under N2 atmosphere to obtain SrMo 0.95 Ni 0.05 O 3-δ Solid oxide fuel cells with the anode material as the anode material; (8) After collecting current with silver wire, the single cell obtained in step (7) is sealed to one end of a ceramic tube with silver paste, with the cathode facing outwards, and fixed in a muffle furnace. The cathode and anode of the single cell are connected to the electrochemical workstation through silver wire. Fuel gas is introduced into the anode of the solid oxide fuel cell through the ceramic tube, and the cathode of the solid oxide fuel cell is placed in the outside air atmosphere. Direct current is generated and output to the outside through the loss of electrons at the cathode and the gain of electrons at the anode at high temperature, thereby realizing the conversion of chemical energy into electrical energy.

[0023] The SrMo prepared according to this invention was analyzed by X-ray diffraction. 0.95 Ni 0.05 O 3-δ Phase analysis of the anode material powder was performed for comparison. Figure 1 and Figure 2 This indicates that the material of the present invention has a simple structure and no obvious impurity peaks during the synthesis process. Given that the material of the present invention is synthesized under pure hydrogen gas, meaning that the material of the present invention has a stable cubic perovskite phase under hydrogen gas, this indicates that SrMo... 0.95 Ni 0.05 O 3-δ The material is structurally stable under hydrogen atmosphere.

[0024] Regarding the material SrMo of the present invention 0.95 Ni 0.05 O 3-δ Electrochemical performance tests were conducted on a solid oxide fuel cell full cell fabricated using the anode material. The power density test results for the cell under H2 and CH4 conditions are as follows: Figure 3 , Figure 4 As shown, Figure 3 The maximum output power of the material of the present invention at 850°C in an H2 atmosphere is shown to be 851 mW cm⁻¹. -2 The maximum output power at 900℃ in a CH4 atmosphere is 193mW cm⁻¹. -2 This demonstrates that the material of this invention has excellent electrochemical properties and good resistance to carbon deposition.

[0025] The above description is only a preferred experimental example of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention shall be covered by the present invention.

Claims

1. A method for preparing a Ni-doped anti-carbon-deposition SOFC anode material, characterized in that, Specifically, the following steps are included: (1) According to the chemical formula SrMo 1-x Ni x O 3-δ The stoichiometric ratios of the corresponding metal elements in Sr are weighed separately. 2+ Nitrates, containing Mo 6+ H 24 Mo7N6O 24 ·4H2O, containing Ni 2+ nitrates, 0 <x≤0.2; (2) Place the weighed medicines obtained in step (1) into beakers in sequence, dissolve them with deionized water, then weigh a certain proportion of citric acid and add it to the beakers. Dissolve it fully with deionized water to obtain a clear solution. Add ammonia to adjust the pH of the solution to neutral. After stirring for a while, the solution becomes turbid. Add an appropriate amount of nitric acid until the solution is clear. Then place the solution on a heating and stirring table to evaporate the solvent. Finally, it burns and the powder obtained is collected. (3) After grinding the powder obtained in step (2) in a mortar, collect the powder into a crucible, place the crucible in a muffle furnace, and calcine it at 600~800℃ for 10~12 hours in an air atmosphere; (4) After grinding the powder calcined in step (3) in a mortar, take an appropriate amount and press it into a mold to form a sheet; (5) Place the pressed sheet from step (4) into a high-temperature furnace and calcine it at 1050~1150℃ for 9~11 hours in an air atmosphere; (6) Take out the calcined sheet from step (5), cool it and put it into the test furnace, and calcin it at 800~900℃ for 3~4 hours in a hydrogen atmosphere; (7) The calcined slices from step (6) were placed in a mortar and ground, anhydrous ethanol was added and ground thoroughly, and then dried to obtain SrMo. 1-x Ni x O 3-δ Solid oxide fuel cell anode electrode powder.

2. The method for preparing a Ni-doped anti-carbon-deposition SOFC anode material according to claim 1, characterized in that, The Sr-containing material used in step (1) 2+ The nitrate is Sr(NO3)2, which contains Ni. 2+ The nitrate is Ni(NO3)2·6H2O.

3. The method for preparing a Ni-doped anti-carbon-deposition SOFC anode material according to claim 1, characterized in that, The amount of citric acid taken in step (2) is 1.5:1 in ratio of citric acid to metal ions.

4. The method for preparing a Ni-doped anti-carbon-deposition SOFC anode material according to claim 1, characterized in that, The specific method of tableting used in step (4) is to put an appropriate amount of powder into a mold with a diameter of 13mm and press it into tablets with a pressure of 2MPa.

5. A solid oxide fuel cell fabricated using Ni-doped, carbon-resistant SOFC anode material, characterized in that, Specifically, the following steps are included: (1) Weigh an appropriate amount of SrMo prepared by the method described in claim 1 1-x Ni x O 3-δ Solid oxide fuel cell anode electrode powder is placed in a mortar, a certain amount of binder is added, and the mixture is ground evenly to form an anode electrode slurry; (2) Weigh out an appropriate amount of SmBaCo2O 5+δ Cathode powder is placed in a mortar, a certain amount of binder is added, and the mixture is ground evenly to form a cathode electrode slurry; (3) Weigh out an appropriate amount of Ce 0.8 Sm 0.2 O 1.9 The buffer layer powder is placed in a mortar, a certain amount of binder is added, and the mixture is ground evenly to make a buffer layer slurry. (4) The buffer layer slurry obtained in step (3) above is uniformly coated onto the electrolyte sheet La using screen printing. 0.9 Sr 0.1 Ga 0.8 Mg 0.2 O 2.85 Place one side of the oven on the side and dry for 8-10 minutes; (5) Place the dried electrolyte sheet in a high-temperature tube furnace and calcine it at 900~1000℃ for 1~3 hours under N2 atmosphere to obtain the pre-material for making a full battery; (6) The electrode slurry obtained in steps (1) and (2) is uniformly coated onto the electrolyte La, the precursor material, respectively. 0.9 Sr 0.1 Ga 0.8 Mg 0.2 O 2.85 and buffer layer Ce 0.8 Sm 0.2 O 1.9 Both sides are dried to obtain full battery cells; (7) Place the dried full cell from step (6) in a high-temperature tube furnace and calcine it at 900~1000°C for 1~3 hours under N2 atmosphere to obtain SrMo 1-x Ni x O 3-δ Solid oxide fuel cells with the anode material as the anode material.

6. A solid oxide fuel cell prepared with Ni-doped, carbon-resistant SOFC anode material according to claim 5, characterized in that, The SrMo used in step (1) 1-x Ni x O 3-δ The mass ratio of anode powder to binder is 1:1.5; the binder is prepared by mixing terpineol and ethyl cellulose in a mass ratio of 9:

1.

7. A solid oxide fuel cell prepared with Ni-doped, carbon-resistant SOFC anode material according to claim 5, characterized in that, The electrolyte tablet La used in step (3) 0.9 Sr 0.1 Ga 0.8 Mg 0.2 O 2.85 The thickness is 0.3mm.

Citation Information

Patent Citations

  • Preparation method for perovskite powder material for cathode of electrolytic tank of solid oxide

    CN101789501A

  • Fuel cell anode material with double-layered perovskite structure and preparation method

    CN108281677A