C / ti coating, c / ti oxidized coating, method for producing the same, bipolar plate provided with the c / ti coating and / or the c / ti oxidized coating, hydrogen fuel cell provided with the bipolar plate
By preparing a C/Ti coating on a metal bipolar plate, including a Ti layer, a C-Ti composite layer, and an aC surface layer, the corrosion problem of the metal bipolar plate in an acidic environment was solved, and the performance and stability of the fuel cell were improved.
Patent Information
- Application Number
- CN202410088099.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-22
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-01-22
AI Technical Summary
Metal bipolar plates are prone to corrosion in the acidic environment of proton exchange membrane fuel cells, leading to catalyst poisoning and decreased conductivity, which affects battery performance and stability.
A C/Ti coating structure is adopted, including a Ti layer, a C-Ti composite layer and an aC surface layer. A coating with excellent corrosion resistance and conductivity is formed by magnetron sputtering and electrochemical oxidation treatment. The specific steps include magnetron sputtering deposition and constant potential polarization treatment.
This improved the corrosion resistance and electrical conductivity of the metal bipolar plates, thereby enhancing the overall performance and stability of the fuel cell.
Smart Images

Figure CN117878347B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of bipolar plate coating technology, and more particularly to a C / Ti coating, a C / Ti oxide coating and a method for preparing the same, a bipolar plate having a C / Ti coating and / or a C / Ti oxide coating, and a hydrogen fuel cell having a bipolar plate. Background Technology
[0002] Proton exchange membrane fuel cells (PEMFCs) have attracted widespread attention in the field of mobility due to their high energy density and environmentally friendly characteristics, and are considered an important direction for future development. In PEMFCs, bipolar plates (BPs) are key components, playing a crucial role in connecting the battery cells and transferring current. Metal bipolar plates are considered the main direction for future development due to their advantages of lightweight and low cost.
[0003] However, metal bipolar plates are susceptible to corrosion in the acidic environment of PEMFCs, which can lead to catalyst poisoning and decreased conductivity, thus affecting battery performance and lifespan. Therefore, designing and fabricating coatings with high corrosion resistance and high conductivity for metal bipolar plates has become an inevitable choice to promote their application.
[0004] Currently, amorphous carbon (aC) with metal coatings is considered one of the most promising types of metal bipolar plate coatings. This coating combines the conductivity of metals with the excellent chemical stability of aC, resulting in good overall performance. However, challenges such as over-passivation dissolution at high potentials and corrosion detachment of the aC layer limit the stability of the coating in the high potential range.
[0005] Therefore, there is an urgent need to optimize the coating to further improve its stability in the high potential range, thereby achieving high efficiency performance of the metal bipolar plate coating. Summary of the Invention
[0006] (The technical problem the invention aims to solve)
[0007] This invention aims to address the problem of corrosion of traditional metal bipolar plates in acidic environments, particularly in proton exchange membrane fuel cells. In existing technologies, corrosion of metal bipolar plates can lead to catalyst poisoning and decreased conductivity, affecting the performance and stability of the fuel cell.
[0008] (The solution adopted to solve the above technical problems)
[0009] In a first aspect, this application provides a C / Ti coating adhered to the surface of a substrate to form a bipolar plate, comprising: a Ti layer; a C-Ti composite layer adhered to at least a portion of the surface of the Ti layer; and an aC surface layer adhered to at least a portion of the surface of the C-Ti composite layer. In the C-Ti composite layer, the atomic ratio of C to Ti is 2:1 to 6:5; the aC surface layer is predominantly composed of C / C sp2 bonds, and the peak area of C / C sp2 bonds after XPS fitting accounts for 55%-60%.
[0010] Preferably, the thickness of the Ti layer and the C-Ti composite layer is 20-80 nm, and the thickness of the aC surface layer is 20-60 nm.
[0011] Preferably, the thickness of the Ti layer and the C-Ti composite layer is 70 nm, and the thickness of the aC surface layer is 45 nm.
[0012] In a second aspect, this application provides a bipolar plate comprising a substrate and at least one C / Ti coating as described in the first aspect, attached to at least a portion of the surface of the substrate.
[0013] Thirdly, this application provides a C / Ti oxide coating that is attached to the surface of a substrate to form a bipolar plate, comprising the C / Ti coating described in the first aspect and an oxide layer attached to at least a portion of the surface of the C / Ti coating.
[0014] Fourthly, this application provides a bipolar plate comprising a substrate and at least one C / Ti oxide coating as described in the third aspect, attached to at least a portion of the surface of the substrate.
[0015] Fifthly, this application provides a hydrogen fuel cell comprising the bipolar plate described in the second aspect.
[0016] In a sixth aspect, this application provides a hydrogen fuel cell comprising the bipolar plate described in the fourth aspect.
[0017] In a seventh aspect, this application provides a method for preparing a C / Ti coating according to the first aspect, wherein the method includes the following steps: i) selecting a substrate, ensuring its surface is clean, and fixing it in a vacuum chamber; ii) using a Ti target as the target material, releasing the material on the Ti target by magnetron sputtering and depositing it on at least a portion of the surface of the substrate to form a Ti layer; iii) using a graphite target and a Ti target as target materials, releasing the material on the graphite target and the Ti target by magnetron sputtering and depositing it on at least a portion of the surface of the Ti layer to form a C-Ti composite layer; iv) turning off the Ti target, using only the graphite target as the target material, releasing the material on the graphite target by magnetron sputtering and depositing it on at least a portion of the surface of the C-Ti composite layer to form an aC surface layer.
[0018] Preferably, in step ii), the Ti target current is set to 80A, the bias voltage is set to 350V, the duty cycle is 40%, and the deposition time is 30min.
[0019] Preferably, in step iii), the Ti target current is set to 60A, the graphite target current is set to 40A, and the deposition time is 30min.
[0020] Preferably, in step iv), the graphite target current is set to 60A and the deposition time is 20min.
[0021] Eighthly, this application provides a method for preparing a C / Ti oxide coating according to the third aspect, wherein the method is carried out in an electrochemical workstation with a three-electrode system, and the method includes the following steps: a) placing a bipolar plate with a C / Ti coating and a three-electrode connected to the electrochemical workstation into a corrosion electrolysis cell for corrosion testing; b) obtaining the potentiodynamic polarization curve of the C / Ti coating surface and determining the anodic region and the corresponding potential therefrom; c) placing the anodic region of the C / Ti coating surface at different potentials for constant potential polarization treatment to form an oxide layer on at least a portion of the surface of the C / Ti coating, thereby preparing the C / Ti oxide coating.
[0022] Preferably, the different potentials are 0.4Vocp, 0.5Vocp, 0.6Vocp and 0.7Vocp.
[0023] Preferably, the constant potential polarization time is 3 hours.
[0024] Preferably, the substrate is made of SS316L.
[0025] Preferably, the thickness of the oxide layer is 5-15 nm.
[0026] Preferably, the oxygen content of the oxide layer has an atomic percentage of 10%-25%.
[0027] (Beneficial effects)
[0028] This application improves the corrosion resistance of the metal bipolar plate and increases the conductivity of the electrode surface by introducing a C / Ti oxide coating with high corrosion resistance and conductivity, thereby enhancing the overall performance and stability of the fuel cell. Attached Figure Description
[0029] Figure 1 This is a cross-sectional schematic diagram of a bipolar plate according to the first embodiment of this application;
[0030] Figure 2These are electron diffraction images of a C / Ti / SS sample prepared according to the first embodiment of this application, wherein (a) is a FIB-TEM cross-sectional image of C / Ti / SS, (b)-(d) are local high-resolution HRTEM and SAED images of C / Ti / SS, and (e)-(f) are element-mapping EDS images and line scan curves of the C / Ti / SS cross-section;
[0031] Figure 3 These are XPS depth etching images of a C / Ti / SS sample prepared according to the first embodiment of this application, wherein (a) is the elemental distribution in the depth direction of C / Ti / SS, (b) is the fine depth etching spectrum of C1s, (c1)-(c4) and (d1)-(d4) are the fine spectral analyses of Ti 2p3 / 2 at C1s and four characteristic etching time points, and (e) and (f) are the peak area percentages of each species in C1s;
[0032] Figure 4 The results of potentiodynamic polarization test and electrochemical impedance spectroscopy test of C / Ti / SS and SS316L prepared according to the first embodiment of this application are shown. Among them, (a) is the potentiodynamic polarization curve of C / Ti / SS, and (b) and (c) are the Nyquist plot and Bode plot of electrochemical impedance spectroscopy test, respectively.
[0033] Figure 5 This is a flowchart illustrating the preparation process of the C / Ti coating according to the first embodiment of this application;
[0034] Figure 6 This is a cross-sectional schematic diagram of a bipolar plate according to the second embodiment of this application;
[0035] Figure 7 This is a schematic diagram illustrating the evolution of a bipolar plate according to the second embodiment of this application;
[0036] Figure 8 This is a flowchart illustrating the preparation process of a C / Ti oxide coating according to the second embodiment of this application;
[0037] Figure 9 These are the constant potential test curves of the C / Ti / SS sample according to the second embodiment of this application, wherein (a) is the constant potential polarization curve and (b) is the charge accumulation curve in the constant potential polarization.
[0038] Figure 10 These are the potentiodynamic polarization test curves of C / Ti / SS samples according to the first and second embodiments of this application, wherein (a) and (b) are the potentiodynamic polarization curves of the original C / Ti / SS and the pre-polarized C / Ti / SS and the corresponding linear curves, respectively;
[0039] Figure 11These are the NEDC cyclic polarization test curves of the C / Ti / SS sample according to the second embodiment of this application;
[0040] Figure 12 The capacitor current response curves of C / Ti / SS according to the first and second embodiments of this application at points (a) I*, (b) II*, (c) III* and (d) IV* in the characteristic potential transition region of the NEDC-based dynamic potential cyclic polarization scheme.
[0041] Figure 13 The figures are Faraday current response curves of C / Ti / SS at points (a) I**, (b) II**, (c) III** and (d) IV** in the characteristic potential transition region of the NEDC-based dynamic potential cyclic polarization scheme according to the first and second embodiments of this application.
[0042] Figure 14 The images show the surface morphology and corresponding elemental mapping of C / Ti / SS under NEDC-based dynamic potential cyclic polarization according to the first and second embodiments of this application, wherein (a) is the original sample, (b) is the original sample after cyclic polarization, (c) is the PS-0.6Vocp sample after cyclic polarization, and (d) is the PS-0.7Vocp sample after cyclic polarization.
[0043] Figure 15 The image shows the C / Ti / SS elemental depth distribution in XPS based on NEDC dynamic potential cyclic polarization according to the first and second embodiments of this application. (a) is before and after pre-polarization of the sample, (b) is before and after cyclic polarization of the original sample, (c) is before and after cyclic polarization of the PS-0.6Vocp sample, and (d) is before and after cyclic polarization of the PS-0.7Vocp sample.
[0044] Figure 16 The fine spectral analysis of surface C1s features of C / Ti / SS based on NEDC dynamic potential cyclic polarization according to the first and second embodiments of this application is shown in (a) before and after cyclic polarization of the original sample, (b) before and after cyclic polarization of the PS-0.6Vocp sample, and (c) before and after cyclic polarization of the PS-0.7Vocp sample.
[0045] Figure 17 The peak area ratio of each species in the fine spectrum of C / Ti / SS after dynamic potential cyclic polarization based on NEDC according to the first and second embodiments of this application;
[0046] Figure 18 The above is a FIB-TEM characterization of a 0.7V prepolarized C / Ti / SS sample according to the second embodiment of this application, wherein (a) is a FIB-TEM cross-sectional image, (b) and (d) are cross-sectional element mapping EDS images and line scan curves, and (c) is a local high-resolution image.
[0047] Figure 19 The ICR changes of C / Ti / SS according to the first and second embodiments of this application after dynamic potential cyclic polarization based on NEDC are shown, wherein (a) is the ICR change under different pressures, and (b) is the ICR change at 140 N / cm. 2 ICR below;
[0048] Figure 20 The results are static contact angle test results of C / Ti / SS samples before and after cyclic dynamic polarization according to the first and second embodiments of this application. Among them, (a1), (b1), and (c1) are static contact angle images of the original C / Ti / SS surface, (a2), (b2), and (c2) are static contact angle images of the C / Ti / SS surface after polarization, and (d) is the corresponding bar chart.
[0049] Figure 21 These are schematic diagrams of the potential distribution of C / Ti / SS under dynamic potential cyclic polarization according to the first and second embodiments of this application, wherein (a) is a schematic diagram of the potential distribution of the original sample, (b) is a schematic diagram of the potential distribution of the sample after pre-polarization of 0.7Vocp, (c) is a schematic diagram of the corrosion process of C on the surface of the original sample, and (d1)-(d2) are schematic diagrams of the corrosion process of C on the surface of the sample after pre-polarization of 0.7Vocp.
[0050] Figure 22 This is a schematic diagram of the structural distribution of a hydrogen fuel cell according to the fourth embodiment of this application. Detailed Implementation
[0051] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0052] (First Implementation)
[0053] [Bipolar plate with C / Ti coating]
[0054] Figure 1 This is a cross-sectional schematic diagram of a bipolar plate according to the first embodiment of this application. (See diagram below.) Figure 1 As shown, the bipolar plate 3 in the first embodiment is composed of a substrate 2 and a C / Ti coating 1 attached to the surface of the substrate 2.
[0055] Substrate 2 refers to the main material that supports the coating, also known as the substrate or base plate. It has a specific shape and size and provides the surface for coating adhesion. In this paper, substrate 2 mainly refers to the material used to prepare the bipolar plate 3, and its properties and characteristics have a significant impact on the coating's adhesion, stability, and overall performance.
[0056] In some embodiments, the material of the substrate 2 is stainless steel, particularly preferably SS316L. SS316L is a specific alloy of stainless steel with excellent corrosion resistance and mechanical properties, and is a type of stainless steel commonly used in applications requiring high corrosion resistance and oxidation resistance.
[0057] Furthermore, the material of substrate 2 can also be other materials. For example, metals such as aluminum alloys and titanium alloys, as well as carbon fiber composites, are all choices with excellent performance under different environments and working conditions. Based on the specific application requirements, different materials of substrate 2 can be flexibly selected to achieve the best coating performance.
[0058] C / Ti coating 1 refers to the material covering the surface of substrate 2, which can be one layer or multiple layers. C / Ti coating 1 is designed to provide the performance characteristics required for bipolar plate 3, including but not limited to high corrosion resistance, excellent electrical conductivity, and stable chemical properties.
[0059] [C / Ti coating structure, composition characterization, preparation and performance testing]
[0060] like Figure 1 As shown, the C / Ti coating 1 consists of a Ti layer 11, a C-Ti composite layer 12, and an aC surface layer 13.
[0061] During the coating preparation process, Ti layer 11 is attached to the surface of substrate 2 as a base layer, C-Ti composite layer 12 is attached to the surface of Ti layer 11 as an intermediate layer, and aC surface layer 13 is attached to the surface of C-Ti composite layer 12 as a top layer. When Ti layer 11, C-Ti composite layer 12, and aC surface layer 13 are attached to the surfaces of their respective layers (substrate 2, Ti layer 11, and C-Ti composite layer 12), the attachment area can be selected to cover part or all of the surface of the corresponding layer.
[0062] In some embodiments, the thickness of the Ti layer 11 is 20-80 nm, the thickness of the C-Ti composite layer 12 is 20-80 nm, and the thickness of the aC surface layer 13 is 20-60 nm.
[0063] Selected area electron diffraction of C / Ti / SS samples
[0064] Figure 2These are electron diffraction images of a C / Ti / SS sample prepared according to the first embodiment of this application, wherein (a) is a FIB-TEM cross-sectional image of C / Ti / SS, (b)-(d) are local high-resolution HRTEM and SAED images of C / Ti / SS, and (e)-(f) are element-mapping EDS images and line scan curves of the C / Ti / SS cross-section.
[0065] It should be understood that the described C / Ti / SS refers to the bipolar plate 3 with C / Ti coating 1 disclosed above, where SS refers to stainless steel (SS316L).
[0066] Depend on Figure 2 The total thickness of the prepared C / Ti coating 1 (single layer) is approximately 185 nm, of which the thickness of the Ti layer 11 and the C-Ti composite layer 12 is approximately 70 nm, and the thickness of the aC surface layer 13 is approximately 45 nm.
[0067] In some embodiments, in the C-Ti composite layer 12, the C content slowly increases from 0% to 25%, while the Ti content slowly decreases from 90% to 65%, which alleviates the large compositional difference between the metal and amorphous carbon layers to some extent.
[0068] The microstructure of C / Ti coating 1 was further investigated using selected area electron diffraction (SEG). Figure 2 In (a), a region of the surface layer 13 of aC was selected for selective electron diffraction, and the results were obtained. Figure 2 (c) and Figure 2 (d) Selection of electron diffraction pattern. Observation. Figure 2 (c) and Figure 2 (d) The surface of aC layer 13 exhibits typical amorphous diffraction rings, showing its typical amorphous carbon structure. This amorphous characteristic provides the coating with excellent corrosion resistance and electrical conductivity.
[0069] Furthermore, in Figure 2 (b) In the figure, selective electron diffraction was performed on the region containing the C-Ti composite layer 12 and the Ti layer 11, yielding the results. Figure 2 (d) Selection of electron diffraction pattern. Figure 2 (d) shows multiple diffraction spots distributed in a ring pattern with different radii. By calibrating the radii of the diffraction rings, two distinct phases were identified: Ti with an HCP structure and TiC with an FCC structure. The diffraction rings, from the inside out, correspond to the (001) and (011) crystal planes of the Ti phase and the (002) and (022) crystal planes of the TiC phase, respectively. This indicates that a complex crystallographic structure of Ti and TiC nanocrystals has formed inside the C / Ti coating 1, providing a solid crystallographic basis for the coating's high electrical conductivity and superior mechanical properties.
[0070] XPS depth etching of C / Ti / SS samples
[0071] Figure 3 These are XPS depth etching images of a C / Ti / SS sample prepared according to the first embodiment of this application, wherein (a) is the elemental distribution along the depth direction of C / Ti / SS, (b) is the fine depth etching spectrum of C1s, and (c1)-(c4) and (d1)-(d4) are the C1s and Ti 2p at four characteristic etching time points. 3 / 2 Fine spectral analysis shows that (e) and (f) represent the peak area percentages of each species in C1s.
[0072] To further understand the composition of C / Ti coating 1, XPS deep etching was used to analyze the composition distribution of C / Ti / SS. The etching produced 30 sets of fine spectra and elemental distributions in the depth direction. Figure 3 (a) shows the peak intensity variation of each element along the depth direction. The overall trend is consistent with the TEM results, indicating that the etching includes the C-Ti composite layer 12 and the aC surface layer 13. It is worth noting that the O element increases in both the aC surface layer 13 and the C-Ti composite layer 12. The O richness in the aC surface layer 13 is due to the oxidation of the sample in the air, while the O in the C-Ti composite layer 12 is attributed to the easy oxidation of Ti during the coating deposition process. Figure 3 (b) shows the change of the fine spectrum of C with the increase of etching time. When the spectrum is in the C surface layer 13, the main peak of C is located at 284.3 eV, corresponding to the peak position of CC sp2. As it gradually enters the C-Ti composite layer 12, the C peak shifts towards the lower eV direction, and the main peak gradually evolves to 282.1 eV, corresponding to the peak position of TiC.
[0073] To clarify the variation trends of the components in the layer, peak fitting was performed on the fine spectra of C and Ti. The corresponding fitting parameters, including binding energy and full width at half maximum (FWHM), are shown in the table below:
[0074]
[0075] The C 1s narrow spectrum was divided into TiC (282.1 eV), TiC x The Ti 2p peaks consist of six components: Ti sp2 (283.0 eV), CC sp2 (284.3 eV), CC sp3 (285.3 eV), CO (287.7 eV), and C=O (289.1 eV). 3 / 2 It is then divided into Ti (454.9 eV), TiC (455.8 eV), and TiC x (457.1 eV), and TiO x (458.6eV) There are 4 component peaks. Figure 3(c) and (d) selected four sets of characteristic narrow spectra with etching times of 0 min, 48 min, 54 min and 78 min for display.
[0076] The proportion of each species is represented by the percentage of peak area after peak fitting, such as... Figure 3 As shown in (e) and (f), the C-Ti composite layer 13 is dominated by C-C sp2 bonding, with a peak area ratio of 55%-60%, which ensures the initial conductivity of C / Ti / SS. After 40 minutes, the C-Ti composite layer 12, TiC, and TiC gradually penetrate into it. x The proportion of bonding gradually increases, while the proportions of C-Csp2 and C-Csp3 bonding gradually decrease. From Figure 3 (f) shows that the proportion of Ti species gradually increases when Ti enters the C-Ti composite layer 12 from 40 min to 50 min. x The proportion gradually decreases, and Ti in the layer mainly exists in the form of metal or carbide.
[0077] In some embodiments, the atomic ratio of C to Ti in the C-Ti composite layer 12 is 2:1 to 6:5.
[0078] according to Figure 2 FIB-TEM and Figure 3 Characterization and analysis of XPS deep etching revealed that a C / Ti coating 1 was successfully fabricated on SS316L, comprising a bottom Ti layer 11, a middle C-Ti composite layer 12, and a top aC surface layer 13. The main component of the aC surface layer 13 is CC sp2; the C-Ti composite layer 12 is mainly composed of TiC and Ti nanocrystals. The C / Ti coating 1 forms a simple structure of metal layer-transition layer-aC layer, and a compositional transition of metal-metal carbide-CC sp2.
[0079] Electrochemical test comparison of C / Ti / SS sample and SS316L
[0080] Figure 4 The results of potentiodynamic polarization test and electrochemical impedance spectroscopy test of C / Ti / SS and SS316L prepared according to the first embodiment of this application are shown. Among them, (a) is the potentiodynamic polarization curve of C / Ti / SS, and (b) and (c) are the Nyquist plot and Bode plot of electrochemical impedance spectroscopy test, respectively.
[0081] like Figure 4As shown, C / Ti / SS exhibits a more positive corrosion potential, a lower corrosion current density, and a larger overpassivation potential compared to substrate 2 (SS316L). Notably, C / Ti / SS shows a significant activation peak in the region where it begins to enter the anodic region, a phenomenon also observed in previous Ti coatings, primarily attributed to the passivation of Ti within the coating. The highest current of the activation peak reaches 4.3 × 10⁻⁶. -7 A / cm 2 After the activation peak, the current rapidly decreased to 2.2 × 10⁻⁶. -8 A / cm 2 As the potential increases, the current shows a continuous increasing trend. After the potential reaches 1.18V, the current exceeds 10V. -6 A / cm 2 After the potential reached 1.2V, the current density decreased slightly and then increased again, indicating a secondary passivation phenomenon. It can be seen that due to the excellent corrosion resistance of Ti metal itself, the simple C / Ti / SS structure in this application, compared to the multilayer C / Cr / SS, only has a slightly higher current density in the anodic region, but it is still far below the DOE technical target (1×10⁻⁶). -6 A / cm 2 In the Nyquist plot (4(b)) of the electrochemical impedance spectroscopy, the capacitive arc radius of C / Ti / SS is significantly larger than that of SS316L, indicating better corrosion resistance. In the Bode plot (4(c)), the |Z| of C / Ti / SS... 0.01Hz It can reach 3.8×10 5 Ω·cm 2 The corresponding phase angle remains around 80° within the range of 1-0.01Hz, demonstrating excellent stability.
[0082] Preparation process of C / Ti coating
[0083] Figure 5 This is a flowchart illustrating the preparation process of a C / Ti coating according to the first embodiment of this application. This application employs magnetron sputtering technology to prepare the C / Ti coating, such as... Figure 5 As shown, the preparation process is achieved by steps i)-iv).
[0084] i) Select substrate 2, ensure its surface is clean, and fix it in a vacuum chamber.
[0085] In the preparation of the C / Ti coating 1, the first step is to select and clean the substrate 2 to ensure optimal adhesion and performance. The substrate 2 is a key component constituting the bipolar plate 3, and is typically made of materials such as stainless steel. Considering the corrosion resistance and mechanical properties of stainless steel, SS316L was preferred when selecting the substrate 2.
[0086] To ensure a strong bond between the C / Ti coating 1 and the substrate 2, the cleanliness of the substrate 2 surface must be ensured. Therefore, a thorough surface cleaning process is performed during the preparation process, including the use of solvents, acid washing or other surface treatment methods to remove any dirt, oxides or other substances on the surface that may affect the adhesion of the coating.
[0087] After cleaning, the substrate 2 is fixed in the vacuum chamber of the magnetron sputtering equipment. The preparation under vacuum conditions can prevent impurities in the air from entering, which helps to improve the purity and quality of the coating.
[0088] ii) Using a Ti target as the target material, the material on the Ti target is released by magnetron sputtering and deposited on at least a portion of the surface of the substrate to form a Ti layer 11.
[0089] When depositing Ti layer 11, the Ti target current was set to 80A, the bias voltage was set to 350V, the duty cycle was 40%, and the deposition time was 30min.
[0090] Specifically, the flow rate of Ti atoms released from the Ti target is controlled by adjusting the current to 80A. The bias voltage, applied to the substrate 2 during sputtering, guides the released Ti atoms to deposit on the surface of the substrate 2. The duty cycle refers to the proportion of the sputtering current's duty time; adjusting the duty cycle allows for precise control of the deposition rate and uniformity. The deposition time is the time it takes for the Ti layer 11 to form; controlling the sputtering time of the target adjusts the thickness of the Ti layer 11.
[0091] iii) Using graphite and Ti targets as target materials, the material on the graphite and Ti targets is released by magnetron sputtering and deposited on at least a portion of the surface of the Ti layer to form a C-Ti composite layer 12.
[0092] When depositing the C-Ti composite layer 12, both graphite and Ti targets are used as target materials to ensure that C elements are introduced into the coating to form a layer with a composite structure.
[0093] During the deposition of the C-Ti composite layer 12, the current of the Ti target was set to 60 A to control the flow rate of released Ti atoms. This current setting was intended to adjust the supply of Ti elements, ensuring sufficient Ti elements to interact with C elements in the C-Ti composite layer 12. Simultaneously, the current of the graphite target was set to 40 A to control the flow rate of released Ti atoms, ensuring the introduction of sufficient C source to react with Ti and form the C-Ti composite layer 12. Furthermore, the deposition time was set to 30 min to ensure sufficient time for C and Ti elements to deposit on the surface of the Ti layer 11.
[0094] iv) Turn off the Ti target and use only the graphite target as the target material. Release the material on the graphite target by magnetron sputtering and deposit it on at least a part of the surface of the C-Ti composite layer to form the aC surface layer 13.
[0095] During the deposition of the aC surface layer 13, the Ti target was turned off, and only the graphite target was used for magnetron sputtering deposition of the aC surface layer 13.
[0096] In step iv), the graphite target current is set to 60A and the deposition time is 20min.
[0097] During the deposition of the aC surface layer 13, the current of the graphite target was set to 60A to release sufficient C atom flux. By adjusting the current, sufficient amorphous carbon was introduced into the aC surface layer 13. Furthermore, the deposition time was controlled to 20 minutes to ensure the formation of a sufficient carbon layer in the aC surface layer 13 and to maintain good bonding with the C-Ti composite layer 12.
[0098] (Second Implementation)
[0099] [Bipolar plate with C / Ti oxide coating]
[0100] Figure 6 This is a cross-sectional schematic diagram of a bipolar plate according to the second embodiment of this application. Figure 7 This is a schematic diagram illustrating the evolution of a bipolar plate according to the second embodiment of this application. For example... Figure 6-7 As shown, the bipolar plate 3 involved in the second embodiment is composed of a substrate 2 and a C / Ti oxide coating 4 attached to the surface of the substrate 2.
[0101] In some embodiments, the material of the substrate 2 is stainless steel, particularly preferably SS316L. SS316L is a specific alloy of stainless steel with excellent corrosion resistance and mechanical properties, and is a type of stainless steel commonly used in applications requiring high corrosion resistance and oxidation resistance.
[0102] Furthermore, the material of substrate 2 can also be other materials. For example, metals such as aluminum alloys and titanium alloys, as well as carbon fiber composites, are all choices with excellent performance under different environments and working conditions. Based on the specific application requirements, different materials of substrate 2 can be flexibly selected to achieve the best coating performance.
[0103] The C / Ti oxide coating 4 refers to the material covering the surface of the substrate 2, which can be one layer or multiple layers. The C / Ti oxide coating 4 is designed to provide the performance characteristics required for the bipolar plate 3, including but not limited to high corrosion resistance, excellent electrical conductivity, and stable chemical properties.
[0104] [Structure, composition characterization, preparation and performance testing of C / Ti oxide coating]
[0105] like Figure 6-7 As shown, the C / Ti oxide coating 4 is composed of a C / Ti coating 1 and an oxide layer 14 attached to at least a portion of the surface of the C / Ti coating 1. The C / Ti coating 1 described herein is the C / Ti coating 1 having any structure / composition in the first embodiment, particularly the C / Ti coating 1 composed of a Ti layer 11, a C-Ti composite layer 12, and an aC surface layer 13.
[0106] The thickness of oxide layer 14 is 5-15 nm.
[0107] The oxygen content of oxide layer 14 is 10%-25% atomically.
[0108] Preparation process of C / Ti oxide coating
[0109] Figure 8 This is a flowchart illustrating the preparation process of the C / Ti oxide coating according to the second embodiment of this application. The preparation process of the C / Ti oxide coating of this application is carried out in an electrochemical workstation with a three-electrode system (counter electrode (CE), reference electrode (RE), and working electrode (WE)). Figure 8 As shown, the preparation process is achieved by steps a)-c).
[0110] a) The bipolar plate 3 with C / Ti coating 1 and the three electrodes connected to the electrochemical workstation were placed into the corrosion electrolysis cell for corrosion testing.
[0111] b) Obtain the potentiodynamic polarization curves of the C / Ti coating 1 surface and use them to determine the anodic region and the corresponding potential;
[0112] c) The anodic region on the surface of C / Ti coating 1 is placed at different potentials to perform constant potential polarization treatment, so as to form an oxide layer 14 on at least a part of the surface of C / Ti coating 1, thereby preparing C / Ti oxide coating 4.
[0113] It should be understood that Figure 8 The preparation process of the C / Ti oxide coating shown is actually a constant potential polarization test process, that is, a pre-polarization treatment process for the C / Ti coating involved in the first embodiment.
[0114] Potentiostatic testing of C / Ti / SS samples
[0115] Figure 9 These are the constant potential test curves of the C / Ti / SS sample according to the second embodiment of this application, wherein (a) is the constant potential polarization curve and (b) is the charge accumulation curve in the constant potential polarization.
[0116] In this embodiment, a constant potential treatment is performed at a relatively low potential to promote the coating surface to reach a steady state. Based on the potentiodynamic polarization curve, four different potentials of 0.4V are selected in the anodic region. ocp 0.5V ocp 0.6V ocp and 0.7V ocp A constant potential polarization was performed for 3 hours, with these potentials set relative to the open circuit potential (OCP). Figure 9 (a) shows the constant potential polarization curve. In the initial stage of polarization, the current drops rapidly within a short period of time, reaching 0.4V. ocp The current under polarization can reach 10 -8 A / cm 2 As the potential increases, the current density gradually increases, especially at potentials less than or equal to 0.6V. ocp The current showed a decreasing trend over three hours. At 0.7V ocp Below, because the polarization potential is in the overpassivation potential range, the current increases by 1.54 × 10⁻⁶ after 1 hour of constant potential polarization. -7 The slope increases slowly, eventually reaching a current density of 3.6 × 10⁻⁶. -7 A / cm 2 . Figure 9 (b) is the charge accumulation curve in constant potential polarization, which corresponds to the magnitude of the current density. As the polarization potential increases, the amount of transferred charge increases, and the slope of the charge curve is the largest at 0.7V.
[0117] Comparison of potentiodynamic polarization tests of C / Ti / SS samples
[0118] Figure 10 These are the potentiodynamic polarization test curves of C / Ti / SS samples according to the first and second embodiments of this application, wherein (a) and (b) are the potentiodynamic polarization curves of the original C / Ti / SS and the pre-polarized C / Ti / SS, and the corresponding linear curves, respectively.
[0119] It should be understood that the original C / Ti / SS described here refers to the C / Ti / SS before pre-polarization, that is, before the constant potential test, which is the C / Ti / SS involved in the first embodiment. Conversely, the pre-polarized C / Ti / SS refers to the C / Ti / SS after pre-polarization, that is, after the constant potential test, which is the C / Ti / SS involved in the second embodiment.
[0120] After performing pre-potential constant polarization treatment for 3 hours at four potentials selected based on the potentiodynamic polarization results of C / Ti coating 1, potentiodynamic polarization tests were conducted on the pre-polarized C / Ti / SS. The results are as follows: Figure 10As shown, the original C / Ti / SS exhibits a high activity peak between 0.6V and 0.7V in the anodic region, which disappears after pre-polarization, indicating that pre-polarization passivates the active Ti in the coating. Furthermore, only with pre-polarization at 0.4V... ocp Both the sample and the original specimen underwent repassivation when the potential exceeded 1.2V, and when the prepolarization potential was higher than 0.5V. ocp At that time, the passivation behavior disappears.
[0121] The table below summarizes representative parameters from the potentiodynamic polarization curves, such as E. corr i corr i 0.84V E >1μA wait.
[0122]
[0123] It can be seen that as the pre-polarization potential increases, E corr Gradually move forward, i corr Gradually decrease, until the prepolarization potential reaches 0.6V. ocp At that time, E corr Increasing the voltage from 0.582V in the original sample to 0.635V, i corr From 3.81×10 -8 A / cm 2 Reduced to 4.11 × 10 -9 A / cm 2 The value decreased by nearly an order of magnitude, indicating that the pre-polarization treatment effectively improved the corrosion resistance of the coating and reduced the corrosion rate. However, as the pre-polarization potential further increased to 0.7V... ocp At that time, E corr The negative shift is to 0.596V, i corr Increased to 7.17 × 10 -9 A / cm 2 This indicates that excessively high pre-polarization potential leads to a decrease in coating performance. Current density at 0.84V is also commonly used to evaluate bipolar plate performance; the i values of the five samples... 0.84 All less than 10 -6 A / cm 2 0.6V ocp The pre-polarized sample exhibited the lowest current density (2.13 × 10⁻⁶). -8 A / cm 2 ), compared to the original sample's i 0.84 The voltage is reduced by half, exhibiting excellent corrosion resistance. In terms of passivation performance, when the pre-polarization potential is higher than 0.5V... ocp Afterwards, E tp Significantly increased, 0.6V ocp Next E tp The highest voltage is 1.36V.
[0124] In summary, the experimental results show that pre-polarization treatment significantly improves the corrosion resistance of C / Ti / SS. As the pre-polarization potential increases, the current density in the anodic region decreases, and the overpassivation potential increases. The sample with a pre-polarization potential of 0.6 Vocp exhibits superior corrosion resistance. After the pre-polarization potential rises to 0.7 Vocp, the overpassivation potential shifts negatively, but it is still better than the original coating.
[0125] Capacitor current response under NEDC cyclic polarization
[0126] Figure 11 The curves are NEDC cyclic polarization test curves of the C / Ti / SS sample according to the second embodiment of this application.
[0127] In the NEDC dynamic potential cyclic polarization scheme, there are multiple consecutive potential transitions, generating two different currents during potential changes. The first current is the Faraday current, which is generated by the electrochemical reaction at the reaction interface and follows Faraday's law, meaning the amount of chemical reaction caused by the current is proportional to the amount of charge passing through. The second current is the capacitive current, which is related to the charge accumulation at the interface when the potential changes. The capacitive current generally decays exponentially over time, faster than the Faraday current. Previous studies have only focused on the Faraday process, i.e., only the current generated by the electrochemical reaction. However, in practical applications, the extremely high capacitive current generated by potential transitions is not negligible, and it reflects certain information about interfacial charge transfer and related reactions.
[0128] like Figure 11 As shown, in this embodiment, four characteristic regions in the NEDC dynamic potential cycle are selected: regions I and II represent the potential transition from 1.08V to 1.22V, region III represents the potential transition from 1.22V to 1.02V, and region IV represents the potential transition from 0.95V to 1.22V. In the generated current curve, capacitive current points I*, II*, III*, and IV*, and Faraday current points I**, II**, III**, and IV** are selected within each region. Figure 11 In this embodiment, based on the results of the potentiodynamic polarization curves, the peak potential E of the dynamic potential cyclic polarization scheme for all samples is selected. peak All values were 1.22V, corresponding to a full-load potential of 0.95V for each stack. Each set of cyclic polarization lasted 1200s, with 150 sets tested per test, for a total of 50 hours.
[0129] Figure 12 The figures are the capacitive current response curves of C / Ti / SS at points (a) I*, (b) II*, (c) III* and (d) IV* in the characteristic potential transition region of the NEDC-based dynamic potential cyclic polarization scheme according to the first and second embodiments of this application.
[0130] For the original C / Ti / SS and 0.6V ocp and 0.7V ocp The pre-polarized C / Ti / SS sample was subjected to dynamic potential cyclic polarization (E) based on NEDC. peak =1.22V), the capacitive current and Faraday current of four characteristic potential transition regions in each cycle were statistically analyzed. Figure 11 ). Figure 12 The capacitive current response of three samples in four characteristic potential transition regions is shown. Overall, pre-polarization treatment alters the capacitive current. For pre-polarization of 0.6V... ocp In the subsequent samples, the capacitive currents I* and II* increased with voltage transitions in regions I and II compared to the original sample. Furthermore, since the potential transitions in both regions were from 1.08V to 1.22V, the capacitive currents were similar. Figure 12 (a) and (b)).
[0131] Within region III, a negative capacitive current III* is generated due to the reverse transition of the potential. Figure 12 (c)), similar to regions I and II, 0.6V ocp The absolute value of the sample capacitance current increases significantly after pre-polarization. Within region IV ( Figure 12 (d) The capacitance current IV* is significantly increased compared to other characteristic points, reaching 0.6V. ocp The capacitive current after pre-polarization can reach up to 1.1 × 10⁻⁶. -5 A / cm 2 This is attributed to the increased potential transitions in this region.
[0132] Conversely, 0.7V ocp After pre-polarization, the capacitive current decreased in all samples, and the absolute value of the capacitive current (III*) also decreased in region III. Furthermore, the trend of capacitive current variation with cycling was altered in the pre-polarized C / Ti / SS samples compared to the original C / Ti / SS samples. The capacitive current of the original C / Ti / SS samples stabilized after 90 cycles, while the pre-polarized samples stabilized more slowly, continuously changing over 150 cycles. In summary, pre-polarization treatment altered the capacitive current generated during potential transitions and changed the charging and discharging process of the interfacial double layer. This may be due to changes in the surface properties of the coating after pre-polarization, leading to alterations in the double-layer capacitance.
[0133] Figure 13 The figures are Faraday current response curves of C / Ti / SS at points (a) I**, (b) II**, (c) III** and (d) IV** in the characteristic potential transition region of the NEDC-based dynamic potential cyclic polarization scheme according to the first and second embodiments of this application.
[0134] Specifically, Figure 13 The Faraday current responses of the three samples in four characteristic potential transition regions are shown. Overall, pre-polarization treatment significantly reduced the Faraday current and slowed down the surface reaction rate. The Faraday currents I**, II**, and IV** generated during the transition from low to high potential in the original samples exhibited similar phased trends. Before 12 cycles, the current showed a rapid decrease, indicating that the surface gradually stabilized and the electrochemical reaction rate decreased rapidly during this stage. Subsequently, the current began to rise between 12 and 36 cycles, with the electrochemical reaction accelerating as the cycles progressed. After 36 cycles, the current stabilized, with the currents at points I** and II** remaining stable at 0.30–0.40 μA / cm. 2 The IV** point, due to its large transition potential difference, remains stable at 0.55-0.75 μA / cm. 2 Overall, the coating exhibited a low reaction rate and good stability during cycling.
[0135] 0.6V ocp After pre-polarization, the current changes similarly to the original sample in the first 10 cycles, with I** and IV** continuously decreasing to 0.16 μA / cm. 2 and 0.30μA / cm 2 The current at the lowest point was reduced by nearly half compared to the original sample, and remained lower than that of the original sample for the first 125 cycles. However, after 10 cycles, the current began to rise and exceeded that of the original sample after 125 cycles, with the final cycle current slightly higher than that of the original sample. 0.7V ocp After pre-polarization, the Faraday current remained at a low level, continuously decreasing during the first 20 cycles, and in subsequent cycles, I** and IV** remained lower than the original sample, maintaining at 0.20 and 0.40 μA / cm, respectively. 2 It is noteworthy that in region III of the reverse transition, the Faraday current exhibits a negative reduction current at 0.6V. ocp and 0.7V ocp The absolute values of the current at point III** after pre-polarization were all greater than those of the original sample. In summary, the Faraday current density of the pre-polarized sample was significantly lower than that of the original sample, indicating that the pre-polarization treatment reduced the corrosion rate and decreased the potential drop of the double layer under steady-state conditions.
[0136] Corrosion behavior of C / Ti oxide coating under cyclic polarization
[0137] <Surface morphology changes>
[0138] Figure 14The images show the surface morphology and corresponding elemental mapping of C / Ti / SS under NEDC-based dynamic potential cyclic polarization according to the first and second embodiments of this application, wherein (a) is the original sample, (b) is the original sample after cyclic polarization, (c) is the PS-0.6Vocp sample after cyclic polarization, and (d) is the PS-0.7Vocp sample after cyclic polarization.
[0139] To analyze the effect of pre-polarization treatment on the surface corrosion pattern under dynamic potential cyclic polarization, the surface morphology, interface structure, and coating composition of the tested samples were characterized. The surface morphology of the original samples is shown below. Figure 14 As shown in (a), numerous scratches left from substrate polishing are clearly visible in the low-magnification image. In the high-magnification image, a large number of white particles are displayed, caused by… Figure 14 (a5) The elemental mapping diagram shows that the white particles are titanium particles, which are metal droplets generated during the coating preparation process. These droplets vary in size, with larger ones reaching a diameter of 5 μm and smaller ones being nanometer-sized. The enrichment of C on the Ti particles suggests that these particles were formed and embedded in the coating before the deposition of C. Figure 14 (b) shows the surface morphology of the original sample after dynamic potential cyclic polarization. Compared to the original sample, the surface abrasion marks are reduced, and numerous deep and small pits appear on the surface. In addition, such as... Figure 14 As shown in (b4), there are large corrosion pits with a diameter of about 3 μm on the surface. The center of the pit is depleted of C and Ti, while O and Fe are enriched. O is enriched in the white area at the edge of the pit. It is speculated that these large corrosion pits are developed from defects formed by the shedding of Ti particles from the surface of the original sample.
[0140] Figure 14 (c) is 0.6V ocp The surface morphology of the pre-polarized sample after dynamic potential cyclic polarization, and Figure 14 (b) Similarly, pitting corrosion appeared on the surface, and the wear marks on the substrate became shallower. In addition, as... Figure 14 As shown in (c2) and (c3), corrosion products enriched with C are present around the Ti particles on the surface. Furthermore, a large area of carbon corrosion products covers the surface. Figure 14 The presence of corrosion products (c4) and (c5) may be one reason why the coating surface is slowed down by the coverage of these corrosion products. When the pre-polarization potential rises to 0.7V... ocp After dynamic potential cyclic polarization, the surface bulk layer of the sample maintained its integrity. There was still enrichment of C corrosion products around the Ti particles, due to galvanic corrosion between the Ti particles and the surrounding coating, causing the coating surface around the Ti particles to act as an anode and be preferentially oxidized. In addition to the locally deep and small pitting, slightly larger and shallower corrosion pits also appeared on the surface, such as... Figure 14As shown in (d3), the corrosion pits are 1-2 μm in diameter, with low Ti and C content and high O and Fe content, indicating that the substrate is exposed and corrosion products are attached within the pits. In summary, both the original and pre-polarized samples exhibited predominantly localized pitting corrosion during dynamic potential cyclic polarization. The pre-polarized sample showed a higher content of C oxidation products on its surface, and the overall coating remained intact, demonstrating good stability.
[0141] <Evolution of Coating Structures>
[0142] Figure 15 The images show the C / Ti / SS elemental depth distribution in XPS based on NEDC dynamic potential cyclic polarization according to the first and second embodiments of this application. (a) shows the pre-polarized sample before and after polarization, (b) shows the original sample before and after cyclic polarization, (c) shows the PS-0.6Vocp sample before and after cyclic polarization, and (d) shows the PS-0.7Vocp sample before and after cyclic polarization.
[0143] XPS tests were performed on the original C / Ti / SS and pre-polarized C / Ti / SS samples before and after cyclic dynamic polarization to further analyze the effect of pre-polarization on the compositional structure evolution during coating cyclic polarization. Figure 15 (a) XPS image of elemental depth distribution of the sample before and after prepolarization, 0.6V ocp The elemental distribution of the coating changes very little after pre-polarization, and due to the extremely low corrosion current density during polarization, only slight thinning of the coating occurs. This is true when the pre-polarization potential is 0.7V. ocp The increased corrosion current density accelerates the dissolution of the coating surface, as shown in the figure, resulting in a noticeable thinning. Figure 15 (b) shows the elemental distribution of the original sample before and after cyclic dynamic polarization. The interface between the surface aC layer and the C-Ti composite layer is aligned to represent the coating thinning. The etching time required for the thinned portion of the coating after cyclic polarization is approximately 6 minutes. (Comparison with 0.6V) ocp The thinning of the samples before and after pre-polarization is clearly visible. Pre-polarization treatment slows down the dissolution of the coating during cyclic polarization, reducing the etching time of the thinned portion to 4 minutes (Figure 15(b)). When the pre-polarization potential rises to 0.7V... ocp Afterwards, the coating thickness did not change significantly before and after cyclic polarization. It is noteworthy that oxygen accumulation was present on the surface of the samples after pre-polarization at 0.6V. ocp The pre-polarized surface showed a slight increase in O content compared to the original surface, and after cyclic polarization, the O atom content on both surfaces exceeded 20%. 0.7V ocp After pre-polarization, the oxygen atom content exceeded 25%, and the content did not change significantly before and after cyclic polarization. This indicates that the surface oxygen accumulation generated during the pre-polarization process is the key to alleviating coating dissolution.
[0144] <Coating Composition Changes>
[0145] Figure 16 The fine spectral analysis of surface C1s features of C / Ti / SS based on NEDC dynamic potential cyclic polarization according to the first and second embodiments of this application is shown in (a) before and after cyclic polarization of the original sample, (b) before and after cyclic polarization of the PS-0.6Vocp sample, and (c) before and after cyclic polarization of the PS-0.7Vocp sample. Figure 17 It refers to the peak area ratio of each species in the fine spectrum of C / Ti / SS after dynamic potential cyclic polarization based on NEDC according to the first and second embodiments of this application. Figure 18 The above are FIB-TEM characterizations of a 0.7V prepolarized C / Ti / SS sample according to the second embodiment of this application, wherein (a) is a FIB-TEM cross-sectional image, (b) and (d) are cross-sectional element mapping EDS images and line scan curves, and (c) is a local high-resolution image.
[0146] To further clarify the mechanism of the pre-polarization process in alleviating coating dissolution, peak fitting was performed on the fine C spectra of the original C / Ti / SS and pre-polarized C / Ti / SS samples before and after cyclic dynamic polarization. The results are as follows: Figure 16 As shown, the peak area percentage of each species is summarized in... Figure 17 First, we focus on the effect of the pre-polarization process on the surface C bonding composition at 0.6V. ocp After pre-polarization, the proportion of C-Csp3 increased significantly, from 24.9% in the original sample to 34.5%. This is attributed to the reduction of weaker bonds and C-Csp2 during polarization. Simultaneously, the CO bond peak showed a slight increase, from 13.9% in the original sample to 16.7%. The pre-polarization potential was increased to 0.7V. ocp The corrosion of C became more pronounced afterward, with the proportion of CO bonds increasing significantly to 32.2%. Although CC sp2 decreased during the pre-polarization process, it is worth noting that due to the control of the pre-polarization potential, the corrosion of the C surface was not severe, and CC sp2 remained its main component. At the same time, the increase in the proportion of CC sp3 and CO bonds is beneficial to improving the corrosion resistance of the coating in the next stage.
[0147] To further clarify the impact of pre-polarization on the surface composition of the coating, the effect of 0.7V was investigated. ocp The prepolarized C / Ti / SS samples were characterized by FIB-TEM. Figure 18 As shown in (a), the pre-polarization did not affect the overall structure of the coating, and the surface layer of aC remained in an amorphous state. Figure 18(b) The elemental mapping image clearly shows that an oxygen-rich layer (oxide layer 14) with a thickness of approximately 15 nm was formed on the surface of the aC layer after pre-polarization, and the formation of this oxide layer was also confirmed by elemental line scan. Simultaneously, the O element content was also relatively high in the layer containing Ti, which is common in previous C / Ti coating depositions and is attributed to the oxidation of Ti during the deposition process. Combined with the current response and XPS analysis results under NEDC cyclic polarization, it can be concluded that the surface oxygen-rich layer generated by the pre-polarization treatment effectively alleviates further oxidation of the surface during cyclic dynamic polarization and reduces the corrosion rate, which is key to mitigating coating dissolution.
[0148] <Changes in coating conductivity>
[0149] Figure 19 The ICR changes of C / Ti / SS according to the first and second embodiments of this application after dynamic potential cyclic polarization based on NEDC are shown, wherein (a) is the ICR change under different pressures, and (b) is the ICR change at 140 N / cm. 2 The ICR below.
[0150] ICR tests were performed on the original C / Ti / SS and pre-polarized C / Ti / SS before and after NEDC-based dynamic potential cyclic polarization to evaluate the change in conductivity. The results are as follows: Figure 19 As shown, for all samples, as the pressure during measurement gradually increases, the contact area between the carbon paper and the sample increases, and the ICR value gradually decreases. The original C / Ti / SS sample exhibits excellent conductivity, with an ICR of less than 5 mΩ·cm at all pressures. 2 At 140 N / cm 2 Below this, the ICR decreases to 1.4 mΩ·cm 2 This is far below the DOE target value of 10 mΩ·cm. 2 This highlights the excellent conductivity of the coating. After pre-polarization, due to the increased proportion of CC sp3 and CO bonds and the decreased proportion of CC sp2 bonds on the surface, the ICR shows a significant increase, reaching 0.6V. ocp and 0.7V ocp 140 N / cm after pre-polarization 2 The ICR increased to 4.6 mΩ·cm. 2 and 5.1 mΩ·cm 2 It still meets the conductivity requirements of bipolar plates.
[0151] The ICR of the original sample rapidly decreased from 1.4 mΩ·cm after dynamic potential cyclic polarization. 2 Increased to 5.6 mΩ·cm 2 The growth exceeded three times. For example... Figure 19 As shown in (a), 0.7V ocpThe ICR of the pre-polarized sample after cyclic polarization was similar to that of the former, and the final ICR also increased to 5.6 mΩ·cm. 2 It only increased by 0.6 mΩ·cm 2 This indicates 0.7V ocp Pre-polarization slowed the corrosion rate and the increase in ICR without negatively affecting the conductivity of the sample during cyclic polarization. 0.6V ocp The pre-polarized sample exhibited more stable conductivity, with its ICR increasing only to 4.8 mΩ·cm after cyclic polarization. 2 Compared to the pre-polarized sample, the increase was only 0.2 mΩ·cm. 2 In summary, pre-polarization treatment slowed down the rapid increase of ICR after cyclic polarization, 0.6V. ocp The conductivity of the pre-polarized sample is more stable.
[0152] <Hydrophobicity Change>
[0153] Figure 20 The results are static contact angle test results of C / Ti / SS samples before and after cyclic dynamic polarization according to the first and second embodiments of this application. Among them, (a1), (b1), and (c1) are static contact angle images of the original C / Ti / SS surface, (a2), (b2), and (c2) are static contact angle images of the C / Ti / SS surface after polarization, and (d) is the corresponding bar chart.
[0154] Overall, the contact angles of the pre-polarized and cyclically polarized samples (C / Ti / SS) were higher than those of the original sample (C / Ti / SS). The contact angle of the original sample was 63° at 0.6V. ocp and 0.7V ocp The contact angles increased to 64° and 75° after pre-polarization, respectively, attributed to changes in surface morphology caused by corrosion. Following cyclic polarization, the contact angle further increased, from 63° to 79° for the original sample at 0.6V. ocp The pre-polarized sample rises to 79° at 0.7V. ocp The pre-polarized sample remained relatively stable at 76°. Since the composition of surface chemical bonds among the three samples did not differ significantly after cyclic polarization, the differences in contact angle were primarily due to surface morphology. This result indicates that the accumulation of surface corrosion products during polarization leads to an increase in the surface contact angle.
[0155] Mechanism of performance enhancement of C / Ti oxide coating
[0156] Figure 21These are schematic diagrams of the potential distribution of C / Ti / SS under dynamic potential cyclic polarization according to the first and second embodiments of this application. (a) is a schematic diagram of the potential distribution of the original sample, (b) is a schematic diagram of the potential distribution of the sample after pre-polarization of 0.7 Vocp, (c) is a schematic diagram of the corrosion process of C on the surface of the original sample, and (d1)-(d2) are schematic diagrams of the corrosion process of C on the surface of the sample after pre-polarization of 0.7 Vocp.
[0157] The mechanism by which controlled oxidation treatment enhances coating performance is analyzed from the following two aspects. First, at 0.7 Voc... p The oxide layer formed on the coating surface after pre-polarization is key to slowing down the corrosion rate. After the oxide layer appears, the Faraday current decreases significantly and remains stable during cycling. Based on fundamental electrochemical knowledge, this indicates that compared to the original sample, the Faraday current at 0.7 Voc... p Prepolarization reduces the ΔEdl of the sample, which is attributed to the increase in the potential drop ΔE in the oxide layer. Figure 21 (b) Secondly, the XPS results show that the surface CO bonding content increases significantly after pre-polarization, reaching 0.7 Voc. p This was particularly evident in pre-polarized samples. According to previous studies, the oxidation process of carbon generally involves two steps:
[0158] C + H₂O → CO ad +2N + +2e - (1-1)
[0159] CO ad +H₂O→CO₂+2H₂O + +2e - (1-2)
[0160] Carbon surface oxides CO ad It is considered a reaction intermediate in the corrosion process, at 0.207V. NHE The surface functional groups formed above (1-1), these carbon oxidation intermediates, are easily formed at lower overpotentials and are highly irreversible, requiring higher overpotentials for subsequent oxidation reactions (1-2). For pure carbon electrodes, the anodic potential limit for exponentially increasing corrosion rates occurs above 0.9V. Therefore, in the original sample, during cyclic dynamic polarization at high potentials, the surface C underwent continuous corrosion, remaining in an unstable state, resulting in a high coating corrosion rate and significant thickness reduction. Figure 21 (c)). Meanwhile, some unstable C on the surface of the pre-polarized sample is oxidized according to the reaction ( Figure 21(b) reduces the defect density on the surface of the coating itself, and the stable oxide layer formed requires a higher overpotential to undergo further reaction, thereby reducing the corrosion current density and slowing down the dissolution of the coating.
[0161] In summary, the enhanced corrosion resistance of the C / Ti oxide coating is mainly attributed to the reduction in ΔE caused by the formation of the surface oxide layer. dl Furthermore, the intermediates formed by carbon oxidation increase the overpotential required for further corrosion of the surface, reduce the corrosion sites on the coating surface, and thus reduce the corrosion rate.
[0162] Effect of C / Ti oxide coating
[0163] This application prepares a single-layer C / Ti coating on SS316L and performs controlled oxidation treatment on it with different pre-polarization potentials. The effects of the pre-polarization treatment on the structural composition, corrosion resistance, conductivity and current response in NEDC cyclic dynamic potential polarization are studied, and the following conclusions can be drawn.
[0164] (1) A C / Ti coating was successfully prepared on SS316L, consisting of a Ti layer at the bottom, a C-Ti composite layer in the middle, and an aC surface layer. The main component of the aC surface layer is CC sp2; the C-Ti composite layer is mainly composed of TiC and Ti nanocrystals. A simple compositional transition of Ti-TiC-aC is formed within the C / Ti coating.
[0165] (2) Pre-polarization treatment significantly improved the corrosion resistance of C / Ti / SS. As the pre-polarization potential increased from 0.4V... ocp Rise to 0.6V ocp E corr Increase, i corr Decrease, Et p Gradually increase. The prepolarization potential rises to 0.7V. ocp After that, Et p A slight negative shift was observed, but it is still far superior to the original coating. The pre-polarization potential is 0.6V. ocp The samples exhibited superior corrosion resistance. 0.84 Reduced to 2.13 × 10 -8 A / cm 2 The passivation potential reaches 1.36V.
[0166] (3) Dynamic potential cyclic polarization based on NEDC (E peak In the sample with a voltage of 1.22V, pre-polarization altered the capacitive current generated during potential transitions, which is attributed to changes in the surface capacitance of the coating. The Faraday current density after pre-polarization was significantly lower than that of the original sample, and the pre-polarization voltage was 0.7V. ocp The good stability of the post-current indicates that the pre-polarization treatment reduced the corrosion rate of the coating.
[0167] (4) Pre-polarization treatment reduces the coating dissolution rate; pre-polarization 0.7V ocp The thickness of the sample did not change significantly before and after dynamic potential cyclic polarization. Based on XPS and TEM analysis, the enhanced performance mechanism of the coating after pre-polarization is mainly due to the formation of an oxide layer of C on the surface, which reduces ΔE. dl Furthermore, the intermediate CO formed by C oxidation reduces corrosion sites on the coating surface and increases coating stability.
[0168] (5) Pre-polarization treatment slowed down the rapid increase in ICR of the coating after dynamic potential cyclic polarization. The original sample's ICR rapidly decreased from 1.4 mΩ·cm after dynamic potential cyclic polarization. 2 Increased to 5.6 mΩ·cm 2 And pre-polarization 0.6V ocp The sample only increased to 4.8 mΩ·cm after cyclic polarization. 2 The increase was only 0.2 mΩ·cm compared to the original sample. 2 It exhibits more stable conductivity.
[0169] In summary, the pre-polarized C / Ti coating in this application significantly improves its corrosion resistance, and the resulting oxide layer effectively mitigates the rapid dissolution and increased conductivity of the C / Ti coating during NEDC dynamic potential cycling. This provides new insights and more practically valuable test results for further optimization of C / Ti coatings.
[0170] (Third Implementation)
[0171] [Bipolar plates with C / Ti coating and oxide coating]
[0172] The bipolar plate 3 in the third embodiment is composed of a substrate 2 and at least one C / Ti coating 1 and at least one C / Ti oxide coating 4 attached to the surface of the substrate 2. The C / Ti coating 1 and the C / Ti oxide coating 4 can be stacked in a cross manner.
[0173] (Fourth Implementation)
[0174] [A hydrogen fuel cell with the first embodiment]
[0175] Figure 22 This is a schematic diagram of the structural distribution of a hydrogen fuel cell according to the fourth embodiment of this application. Figure 22 As shown, the hydrogen fuel cell 5 involved in this embodiment is composed of a proton exchange membrane (PEM), a catalyst layer (CCL), a gas diffusion layer (GDL), and a bipolar plate 3 (BPP). Here, the bipolar plate 3 refers to a bipolar plate 3 having any structure / composition of the first embodiment, particularly a bipolar plate 3 composed of a substrate 2 and a C / Ti coating 1 attached to the surface of the substrate 2.
[0176] The proton exchange membrane (PEM) is a crucial component in hydrogen fuel cells. Typically made of polymer materials, it boasts high proton conductivity and effectively isolates hydrogen and oxygen, ensuring proton transfer while preventing direct mixing of the two gases. The carbon-coated polymer (CCL) layer, located on either side of the proton exchange membrane, usually contains a noble metal catalyst. Its primary function is to facilitate the electrochemical reaction between hydrogen and oxygen, combining protons from hydrogen and electrons from oxygen to form water. The carbon-coated polymer (GDL) layer, situated outside the catalyst layer, is typically composed of porous carbon materials. Its role is to provide channels for hydrogen and oxygen, ensuring their uniform distribution across the catalyst layer surface. Furthermore, the GDL contributes to electrical conductivity, promoting electron flow within the cell.
[0177] [Hydrogen fuel cell equipped with bipolar plates according to the second embodiment]
[0178] The hydrogen fuel cell 5 involved in this embodiment is also composed of a proton exchange membrane (PEM), a catalyst layer (CCL), a gas diffusion layer (GDL), and a bipolar plate 3 (BPP). The difference is that the bipolar plate 3 here refers to a bipolar plate 3 having any structure / composition of the second embodiment, especially a bipolar plate 3 composed of a substrate 2 and a C / Ti oxide coating 4 attached to the surface of the substrate 2.
[0179] [Hydrogen fuel cell equipped with bipolar plates according to a third embodiment]
[0180] The hydrogen fuel cell 5 involved in this embodiment also consists of a proton exchange membrane (PEM), a catalyst layer (CCL), a gas diffusion layer (GDL), and a bipolar plate 3 (BPP). The difference is that the bipolar plate 3 here refers to a bipolar plate 3 having any structure / composition as described in the third embodiment.
Claims
1. A C / Ti oxide coating adhered to the surface of a substrate to form a bipolar plate, the C / Ti oxide coating comprising: C / Ti coating; An oxide layer adhering to at least a portion of the surface of the C / Ti coating; The C / Ti coating comprises: Ti layer; A C-Ti composite layer, which is attached to at least a portion of the surface of the Ti layer; and aC surface layer, which is attached to at least a portion of the surface of the C-Ti composite layer; In the C-Ti composite layer, the atomic ratio of C to Ti is 2:1 to 6:5; Among them, the surface layer of aC is dominated by CC sp2 bonding, and the peak area of CC sp2 after XPS fitting accounts for 55%-60%; The method for preparing the C / Ti oxide coating is carried out in a three-electrode electrochemical workstation and includes: a) The bipolar plate with C / Ti coating and the three electrodes connected to the electrochemical workstation were placed in a corrosion electrolysis cell for corrosion testing; b) Obtain the potentiodynamic polarization curves of the C / Ti coating surface and use them to determine the anodic region and the corresponding potential; c) The anodic region on the surface of the C / Ti coating is placed at different potentials to perform constant potential polarization treatment, so as to form an oxide layer on at least a portion of the surface of the C / Ti coating, thereby preparing the C / Ti oxide coating.
2. The C / Ti oxide coating according to claim 1, wherein, The thickness of the Ti layer and the C-Ti composite layer is 20-80 nm, and the thickness of the aC surface layer is 20-60 nm.
3. The C / Ti oxide coating according to claim 2, wherein, The thickness of the Ti layer and the C-Ti composite layer is 70 nm, and the thickness of the aC surface layer is 45 nm.
4. A bipolar plate comprising a substrate and at least one C / Ti oxide coating as described in any one of claims 1-3, attached to at least a portion of the surface of the substrate.
5. A hydrogen fuel cell comprising the bipolar plate of claim 4.
6. A method for preparing a C / Ti oxide coating according to any one of claims 1-3, wherein, The preparation of the C / Ti coating includes the following steps: i) Select a substrate, ensure its surface is clean, and fix it in a vacuum chamber; ii) Using a Ti target as the target material, the material on the Ti target is released by magnetron sputtering and deposited on at least a portion of the surface of the substrate to form a Ti layer; iii) Using graphite and Ti targets as target materials, the material on the graphite and Ti targets is released by magnetron sputtering and deposited on at least a portion of the surface of the Ti layer to form a C-Ti composite layer; iv) With the Ti target off, only the graphite target is used as the target material. The material on the graphite target is released by magnetron sputtering and deposited on at least a portion of the surface of the C-Ti composite layer to form the aC surface layer.
7. The preparation method according to claim 6, wherein, In step ii), the Ti target current is set to 80 A, the bias voltage is set to 350 V, the duty cycle is 40%, and the deposition time is 30 min.
8. The preparation method according to claim 6, wherein, In step iii), the Ti target current is set to 60 A, the graphite target current is set to 40 A, and the deposition time is 30 min.
9. The preparation method according to claim 6, wherein, In step iv), the graphite target current is set to 60 A and the deposition time is 20 min.
10. The preparation method according to claim 6, wherein, The different potentials are 0.4 Vocp, 0.5 Vocp, 0.6 Vocp and 0.7 Vocp.
11. The preparation method according to claim 6, wherein, The constant potential polarization time is 3 hours.
12. The preparation method according to claim 6, wherein, The substrate material is selected as SS316L.
13. The preparation method according to claim 6, wherein, The thickness of the oxide layer is 5-15 nm.
14. The preparation method according to claim 6, wherein, The oxygen content of the oxide layer has an atomic percentage of 10%-25%.
Citation Information
Patent Citations
Bipolar plate for hydrogen fuel cell coated with carbon-containing coating
CN114006003A
Method for evaluating corrosion resistance of metal bipolar plate of fuel cell
CN115452697A