Polyethylene film acoustic assembly

By using a polyethylene membrane designed with specific parameters as a component of the acoustic device, the problems of high sound loss and insufficient mechanical protection during the use of the diaphragm are solved, resulting in an acoustic component with low sound loss and stable performance, suitable for mechanical protection in immersion applications.

CN117882392BActive Publication Date: 2026-11-24WL GORE & ASSOC INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202280058852.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-08-30
Filing Date
2022-08-29
Publication Date
2026-11-24
Estimated Expiration
2042-08-29

AI Technical Summary

Technical Problem

Existing acoustic membranes suffer from problems such as high sound loss, unstable performance, and insufficient mechanical protection during use, especially in immersion applications, which can easily lead to plastic deformation and performance degradation of the membrane.

Method used

Polyethylene membranes are used as components of acoustic devices. The polyethylene membranes are designed with specific parameters such as thickness, tensile modulus, porosity and permeability to ensure stable performance while maintaining low sound loss and mechanical protection. Through reasonable structural design and material selection, excessive stretching and plastic deformation of the membrane are avoided.

Benefits of technology

The acoustic components achieve low sound loss and stable performance, providing effective mechanical protection in immersion applications, reducing plastic deformation of the membrane, and maintaining similar performance of the acoustic membrane over time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117882392B_ABST
    Figure CN117882392B_ABST
Patent Text Reader

Abstract

An assembly includes an acoustic device. The acoustic device may include a polyethylene membrane. The polyethylene membrane may have a first orientation and a second orientation, the second orientation being orthogonal to the first orientation. The polyethylene membrane may have a diameter of at least 39 × 10⁻⁶. 6 The surface area per unit volume is given by m. The polyethylene film can have a geometric mean tensile modulus of 250 to 750 MPa. The polyethylene film can have a maximum tensile modulus of 440 to 915 MPa in the first direction. The polyethylene film can have a maximum tensile modulus of 275 to 515 MPa in the second direction. The polyethylene film can be an expanded polyethylene film.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present disclosure relates generally to acoustic assemblies. More specifically, the present disclosure relates to acoustic assemblies comprising a polyethylene membrane. BACKGROUND

[0002] The acoustic membrane assembly can allow sound to propagate through and past the membrane and to and from the acoustic device. The acoustic membrane can also prevent the ingress of water, dust, and other contaminants. SUMMARY

[0003] In some embodiments, the assembly comprises an acoustic device. In some embodiments, the acoustic device comprises a polyethylene membrane. In some embodiments, the polyethylene membrane has a first direction and a second direction, the second direction being orthogonal to the first direction. In some embodiments, the polyethylene membrane has a thickness of 0.5 pm to 14 pm. In some embodiments, the thickness defines a thickness direction and the first and second directions are orthogonal to the thickness direction. In some embodiments, the polyethylene membrane has a specific surface area of at least 39 x 10 6 / m. In some embodiments, the polyethylene membrane has a geometric mean tensile modulus of 250 to 750 MPa. In some embodiments, the polyethylene membrane has a maximum tensile modulus in the first direction of 440 to 915 MPa. In some embodiments, the polyethylene membrane has a maximum tensile modulus in the second direction of 275 to 515 MPa.

[0004] In some embodiments, the acoustic device is one of a loudspeaker, a microphone, or any combination thereof.

[0005] In some embodiments, the acoustic device has a transmission loss (dB) that varies by less than 2.1 dB when tested using the WEP test at 1 bar open hole challenge @ 3 KHz (at 3 KHz) 24 hours after.

[0006] In some embodiments, the polyethylene membrane has a tensile modulus balance of 1 to 2.1.

[0007] In some embodiments, the geometric mean tensile modulus is 350 MPa to 650 MPa.

[0008] In some embodiments, the polyethylene membrane has a porosity of 50% to 95%.

[0009] In some embodiments, the polyethylene membrane has a porosity of 55% to 86%.

[0010] In some embodiments, the recovery rate at 1 hour after 1 bar open hole challenge is at least 69%.

[0011] In some embodiments, the polymeric membrane has a bubble point of 7 psi (pounds per square inch) to 200 psi.

[0012] In some embodiments, the polyethylene film has 1x10 -15 m 2 Up to 8x10 -15 m 2 Penetration rate.

[0013] In some embodiments, the polyethylene film has 3x10 -16 m 2 Up to 7.4x10 -15 m 2 Penetration rate.

[0014] In some embodiments, the polyethylene film is an expanded polyethylene film.

[0015] In some embodiments, the component includes an acoustic device. In some embodiments, the acoustic device includes a polyethylene diaphragm. In some embodiments, the recovery rate at 1 hour after a 1 bar opening challenge is at least 69%.

[0016] In some embodiments, when tested using WEP testing at 24 hours after a 1 bar aperture challenge at 3 kHz, the acoustic device exhibits a transmission loss (dB) variation of less than 2.1 dB.

[0017] In some embodiments, the acoustic device is a loudspeaker, a microphone, or any combination thereof.

[0018] In some embodiments, the polyethylene film has a thickness of 0.5 μm to 14 μm.

[0019] In some embodiments, the polyethylene film has a porosity of 50% to 95%.

[0020] In some embodiments, the polyethylene film has a porosity of 55% to 86%.

[0021] In some embodiments, the polymer film has a bubble point of 7 psi to 200 psi.

[0022] In some embodiments, the polyethylene film has 1x10 -15 m 2 Up to 8x10 -15 m 2 Penetration rate.

[0023] In some embodiments, the polyethylene film has 3x10 -16 m 2 Up to 7.4x10 -15 m 2 Penetration rate.

[0024] In some embodiments, the polyethylene film has a first direction and a second direction, the second direction being orthogonal to the first direction, and the surface area per unit volume is at least 39 x 10⁻⁶.6 / m; geometric mean tensile modulus is 250 to 750 MPa; maximum tensile modulus in the first direction is 440 to 915 MPa; and maximum tensile modulus in the second direction is 275 to 515 MPa.

[0025] In some embodiments, the polyethylene film has a tensile modulus balance of 1 to 2.1.

[0026] In some embodiments, the geometric mean tensile modulus is 250 to 650 MPa.

[0027] In some embodiments, the polyethylene film is an expanded polyethylene film.

[0028] In some embodiments, the component includes an acoustic device. In some embodiments, the acoustic device includes a polyethylene diaphragm. In some embodiments, when tested using WEP testing at a 1 bar aperture challenge @ 3 kHz for 24 hours, the acoustic device exhibits a transmission loss variation of less than 2.1 dB.

[0029] In some embodiments, the polyethylene film has a first direction and a second direction, the second direction being orthogonal to the first direction, and the surface area per unit volume is at least 39 x 10⁻⁶. 6 / m; geometric mean tensile modulus is 250 to 750 MPa; maximum tensile modulus in the first direction is 440 to 915 MPa; and maximum tensile modulus in the second direction is 275 to 515 MPa.

[0030] In some embodiments, the polyethylene film has a tensile modulus balance of 1 to 2.1.

[0031] In some embodiments, the geometric mean tensile modulus is 250 to 650 MPa.

[0032] In some embodiments, the surface area per unit volume is 39 x 10. 6 / m to 70x10 6 / m.

[0033] In some embodiments, the recovery rate at 1 hour after a 1-bar perforation challenge is at least 69%.

[0034] In some embodiments, the acoustic device is a loudspeaker, a microphone, or any combination thereof.

[0035] In some embodiments, the polyethylene film has a thickness of 0.5 μm to 14 μm.

[0036] In some embodiments, the polyethylene film has a porosity of 50% to 95%.

[0037] In some embodiments, the polyethylene film has a porosity of 55% to 86%.

[0038] In some embodiments, the polymer film has a bubble point of 7 psi to 200 psi.

[0039] In some embodiments, the polyethylene film has 1x10 -15 m 2 Up to 8x10 -15 m 2 Penetration rate.

[0040] In some embodiments, the polyethylene film has 3x10 -16 m 2 Up to 7.4x10 -15 m 2 Penetration rate.

[0041] In some embodiments, the polyethylene film is an expanded polyethylene film.

[0042] In some embodiments, the polyethylene film has a thickness that defines a thickness direction, and a first direction and a second direction are each orthogonal to the thickness direction.

[0043] In some embodiments, the maximum tensile modulus in the first direction is greater than the maximum tensile modulus in the second direction.

[0044] In some embodiments, the first direction is one of the longitudinal and transverse directions of the polyethylene film, and the second direction is the other of the longitudinal and transverse directions of the polyethylene film. Attached Figure Description

[0045] Referring to the accompanying drawings, which form part of this disclosure, and illustrating embodiments in which the systems and methods described herein can be practiced.

[0046] Figure 1 A front view of a component including an acoustic device is shown according to some embodiments.

[0047] Figure 2 Illustrations are shown according to some embodiments Figure 1 A top view of the protective covering component.

[0048] Figure 3 Illustrations are shown according to some embodiments Figures 1-2 A cross-sectional view of the protective covering component.

[0049] Figure 4 A schematic diagram of a test configuration for stress testing according to some embodiments is shown.

[0050] The same reference numerals denote the same or similar parts throughout. Detailed Implementation

[0051] There is a persistent need for improved acoustic diaphragms. Some embodiments described herein can advantageously achieve low acoustic loss and variability while providing mechanical protection for immersion applications. Some embodiments described herein can advantageously avoid excessive stretching of the diaphragm, thereby providing similar performance of the acoustic diaphragm over time. That is, avoiding plastic deformation of the diaphragm can reduce performance degradation over time.

[0052] Some embodiments of this disclosure relate to acoustic diaphragms that support a primary reaction. In the primary reaction mode, sound is transmitted through a combination of diaphragm vibration in the effective region (active region) and vibration within the gas phase in the open pores of the diaphragm.

[0053] In some embodiments, the component includes an acoustic device. In some embodiments, the acoustic device is a loudspeaker, a microphone, or any combination thereof. In some embodiments, the acoustic device includes a polyethylene membrane. In some embodiments, the polyethylene membrane is an expanded polyethylene membrane. In some embodiments, the polyethylene membrane has a fibrillated microstructure.

[0054] As used herein, the term "membrane" refers to an article, such as a sheet article, having three dimensions defined by three mutually perpendicular axes or directions, where two dimensions are typically larger than the third dimension. For example, the two larger dimensions are at least an order of magnitude larger than the smallest third dimension. Therefore, the smallest third dimension can represent the thickness of the membrane. This thickness can be measured along the third axis or direction, which is referred to herein as the thickness direction of the membrane.

[0055] The membrane may have opposing first and second surfaces, which are separated by the membrane's thickness, i.e., by the shortest distance between the opposing first and second surfaces. This distance may be defined by a line orthogonal to the plane of both the first and second surfaces. Therefore, the thickness direction may be parallel to the line defining the membrane's thickness.

[0056] Both the first axis or direction and the second axis or direction are orthogonal to the thickness direction of the membrane. Therefore, the first direction and the second direction define a plane perpendicular to the thickness direction of the membrane. Thus, the plane defined by the first direction and the second direction is parallel to or overlaps with the planar sheet of the membrane.

[0057] In some embodiments, the first direction is selected from one of the longitudinal direction and the transverse direction of the membrane, while the second direction is selected from the other of the longitudinal direction and the transverse direction of the membrane. In some embodiments, the first direction is selected from one of the machine direction and the transverse direction of the membrane, while the second direction is selected from the other of the machine direction and the transverse direction of the membrane.

[0058] In some embodiments, a maximum tensile modulus may be determined for each of a first direction and a second direction. The first direction may be specified as the direction with a larger maximum tensile modulus. The second direction may be specified as the direction with a smaller maximum tensile modulus.

[0059] Figure 1 An external front view of an electronic device 10 according to some embodiments is shown. In the illustrated embodiment, the electronic device 10 is a cellular phone with an opening 12. The opening 12 can be a narrow slot or a circular aperture. Although an opening 12 is shown, it should be understood that the number, size, and shape of openings in the electronic device 10 can vary. It is also understood that the type of electronic device 10 can vary beyond a cellular phone. A protective cover assembly 14 is shown to cover the opening 12 to prevent moisture, debris, or other particles from entering the electronic device 10. The protective cover assembly 14 is suitable for openings of any size and is not particularly limited. The structures disclosed herein are equally applicable to openings in the sound channels of protective covers for any comparable electronic device, such as a laptop, tablet, camera, smartwatch, portable microphone, etc. To allow installation of the protective cover assembly 14, the size of the protective cover assembly 14 is larger than the maximum diameter of the opening 12.

[0060] Figure 2 Illustrations are shown according to some embodiments Figure 1 A top view of the protective cover assembly 14. In the illustrated embodiment, the protective cover assembly 14 includes an effective region 16 surrounded by a support region 18. The effective region 16 comprises only the membrane and allows sound to pass easily through it. The support region 18 includes a membrane sandwiched between outer adhesive layers for connecting the protective cover assembly 14 to the electronic device 10. The specific structure used to secure the membrane in place is not intended to be limiting.

[0061] Figure 3 A cross-sectional view of a protective cover assembly 14 according to some embodiments is shown. A layered assembly 20 is inserted into the housing 22 of the electronic device 10. An opening 12 defines an acoustic path 24, across which the protective cover assembly 14 is positioned, separating the external environment 26 of the housing 22 from the internal environment 28, and separating the external environment 26 from the acoustic cavity 30. The housing 22 is arranged around and configured to protect the electronic device 32 (e.g., a circuit board for a mobile device, mobile phone, tablet computer, etc.), and positions the layered assembly 20 to prevent water or debris from entering the internal environment 28, particularly protecting the transducer 34. The transducer 34 is located below an effective area 16 within the opening 12 for generating or receiving sound.

[0062] The layered assembly 20 includes a diaphragm 36 and a support structure 38. Sound waves can travel along an acoustic path 24 through the acoustic cavity 30 and through the diaphragm 36 between the transducer 34 and the external environment 26. The acoustic path 24 is generally defined by an opening 12 in the housing 22. This opening 12 is generally approximately the same size as the unobstructed portion of the diaphragm 36.

[0063] Acoustic pathway 24 can also provide ventilation. Ventilation can provide pressure equalization between acoustic cavity 30 and external environment 26. Ventilation is useful when a pressure difference exists between acoustic cavity 30 and external environment 26 that affects the ability of layering assembly 20 to transmit sound waves. For example, temperature changes in acoustic cavity 30 can cause the air inside the cavity to expand or contract, which can often deform layering assembly 20 and cause acoustic distortion.

[0064] Surface area per unit volume

[0065] In some embodiments, the polyethylene film has a thickness of at least 39 x 10 mm. 6 The surface area per unit volume is 70 × 10 m. In some embodiments, the surface area per unit volume is less than 70 × 10 m. 6 / m. In some embodiments, the polyethylene film has a diameter of 39 × 10 m. 6 / m to 70×10 6 / m is the surface area per unit volume.

[0066] In some embodiments, the polyethylene film has a size of 40 × 10. 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​41 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​42 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​43 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​44 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​45 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​46 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​47 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​48 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​49 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​50 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 51 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 52 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 53 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 54 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 55 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 56 × 10 6 / m to 70×10 6 The surface area per unit volume is 57 × 10 m. In some embodiments, the polyethylene film has a surface area of ​​57 × 10 m. 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 58 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 59 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​60 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​61 × 10⁻⁶ m². 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​62 × 10⁻⁶ m². 6 / m to 70×10 6The surface area per unit volume is 63 × 10 m. In some embodiments, the polyethylene film has a surface area of ​​63 × 10 m. 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​64 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​65 × 10 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​66 × 10. 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​67 × 10⁻⁶ m². 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​68 × 10⁻⁶ m². 6 / m to 70×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has a surface area of ​​69 × 10 6 / m to 70×10 6 / m is the surface area per unit volume.

[0067] In some embodiments, the polyethylene film has a diameter of 39 × 10 mm. 6 / m to 69×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 68×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 67×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 66×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 65×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 64×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 63×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 62×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 61×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 60×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 59×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 58×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 57×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 56×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 55×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 54×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 53×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 52×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 51×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 50×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 49×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 48×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 47×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 46×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 45×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 44×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 43×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 42×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 41×10 6 / m of surface area per unit volume. In some embodiments, the polyethylene film has 39 × 10 6 / m to 40×10 6 / m is the surface area per unit volume.

[0068] Geometric mean tensile modulus

[0069] In some embodiments, the polyethylene film has a geometric mean tensile modulus of 250 MPa to 750 MPa. In some embodiments, the geometric mean tensile modulus is 300 MPa to 750 MPa. In some embodiments, the geometric mean tensile modulus is 350 MPa to 750 MPa. In some embodiments, the geometric mean tensile modulus is 400 MPa to 750 MPa. In some embodiments, the geometric mean tensile modulus is 450 MPa to 750 MPa. In some embodiments, the geometric mean tensile modulus is 500 MPa to 750 MPa. In some embodiments, the geometric mean tensile modulus is 550 MPa to 750 MPa. In some embodiments, the geometric mean tensile modulus is 600 MPa to 750 MPa. In some embodiments, the geometric mean tensile modulus is 650 MPa to 750 MPa. In some embodiments, the geometric mean tensile modulus is 700 MPa to 750 MPa.

[0070] In some embodiments, the geometric mean tensile modulus is 250 MPa to 700 MPa. In some embodiments, the geometric mean tensile modulus is 250 MPa to 650 MPa. In some embodiments, the geometric mean tensile modulus is 250 MPa to 600 MPa. In some embodiments, the geometric mean tensile modulus is 250 MPa to 550 MPa. In some embodiments, the geometric mean tensile modulus is 250 MPa to 500 MPa. In some embodiments, the geometric mean tensile modulus is 250 MPa to 450 MPa. In some embodiments, the geometric mean tensile modulus is 250 MPa to 400 MPa. In some embodiments, the geometric mean tensile modulus is 250 MPa to 350 MPa. In some embodiments, the geometric mean tensile modulus is 250 MPa to 300 MPa.

[0071] In some embodiments, the geometric mean tensile modulus is 350 MPa to 650 MPa.

[0072] Tensile modulus balance

[0073] In some embodiments, the polyethylene film has a tensile modulus balance of 1 to 2.1.

[0074] In some embodiments, the tensile modulus balance is 1.1 to 2.1. In some embodiments, the tensile modulus balance is 1.2 to 2.1. In some embodiments, the tensile modulus balance is 1.3 to 2.1. In some embodiments, the tensile modulus balance is 1.4 to 2.1. In some embodiments, the tensile modulus balance is 1.5 to 2.1. In some embodiments, the tensile modulus balance is 1.6 to 2.1. In some embodiments, the tensile modulus balance is 1.7 to 2.1. In some embodiments, the tensile modulus balance is 1.8 to 2.1. In some embodiments, the tensile modulus balance is 1.9 to 2.1. In some embodiments, the tensile modulus balance is 2 to 2.1.

[0075] In some embodiments, the tensile modulus balance is 1 to 2. In some embodiments, the tensile modulus balance is 1 to 1.9. In some embodiments, the tensile modulus balance is 1 to 1.8. In some embodiments, the tensile modulus balance is 1 to 1.7. In some embodiments, the tensile modulus balance is 1 to 1.6. In some embodiments, the tensile modulus balance is 1 to 1.5. In some embodiments, the tensile modulus balance is 1 to 1.4. In some embodiments, the tensile modulus balance is 1 to 1.3. In some embodiments, the tensile modulus balance is 1 to 1.2. In some embodiments, the tensile modulus balance is 1 to 1.1.

[0076] In some embodiments, the tensile modulus balance is less than 2.

[0077] Maximum tensile modulus

[0078] In some embodiments, the polyethylene film has a maximum tensile modulus of 440 MPa to 915 MPa in a first direction. In some embodiments, the tensile modulus in the first direction is 440 MPa to 900 MPa. In some embodiments, the tensile modulus in the first direction is 440 MPa to 850 MPa. In some embodiments, the tensile modulus in the first direction is 440 MPa to 800 MPa. In some embodiments, the tensile modulus in the first direction is 440 MPa to 750 MPa. In some embodiments, the tensile modulus in the first direction is 440 MPa to 700 MPa. In some embodiments, the tensile modulus in the first direction is 440 MPa to 650 MPa. In some embodiments, the tensile modulus in the first direction is 440 MPa to 600 MPa. In some embodiments, the tensile modulus in the first direction is 440 MPa to 550 MPa. In some embodiments, the tensile modulus in the first direction is 440 MPa to 500 MPa. In some embodiments, the tensile modulus in the first direction is 440 MPa to 450 MPa.

[0079] In some embodiments, the tensile modulus in the first direction is 450 MPa to 915 MPa. In some embodiments, the tensile modulus in the first direction is 500 MPa to 915 MPa. In some embodiments, the tensile modulus in the first direction is 550 MPa to 915 MPa. In some embodiments, the tensile modulus in the first direction is 600 MPa to 915 MPa. In some embodiments, the tensile modulus in the first direction is 650 MPa to 915 MPa. In some embodiments, the tensile modulus in the first direction is 700 MPa to 915 MPa. In some embodiments, the tensile modulus in the first direction is 750 MPa to 915 MPa. In some embodiments, the tensile modulus in the first direction is 800 MPa to 915 MPa. In some embodiments, the tensile modulus in the first direction is 850 MPa to 915 MPa. In some embodiments, the tensile modulus in the first direction is 900 MPa to 915 MPa.

[0080] In some embodiments, the polyethylene film has a maximum tensile modulus of 275 MPa to 515 MPa in a second direction orthogonal to the first direction. In some embodiments, the maximum tensile modulus in the second direction is 275 MPa to 500 MPa. In some embodiments, the maximum tensile modulus in the second direction is 275 MPa to 450 MPa. In some embodiments, the maximum tensile modulus in the second direction is 275 MPa to 400 MPa. In some embodiments, the maximum tensile modulus in the second direction is 275 MPa to 350 MPa. In some embodiments, the maximum tensile modulus in the second direction is 275 MPa to 300 MPa.

[0081] In some embodiments, the maximum tensile modulus in the second direction is 300 MPa to 515 MPa. In some embodiments, the maximum tensile modulus in the second direction is 350 MPa to 515 MPa. In some embodiments, the maximum tensile modulus in the second direction is 400 MPa to 515 MPa. In some embodiments, the maximum tensile modulus in the second direction is 450 MPa to 515 MPa. In some embodiments, the maximum tensile modulus in the second direction is 500 MPa to 515 MPa.

[0082] It is understandable that as long as the first direction and the second direction are orthogonal to each other, the first direction and the second direction can be reversed.

[0083] thickness

[0084] In some embodiments, the polyethylene film has a thickness of 14 μm or less. In some embodiments, the thickness is at least 0.5 μm. In some embodiments, the thickness is from 0.5 μm to 14 μm.

[0085] In some embodiments, the thickness is 1 μm to 14 μm. In some embodiments, the thickness is 2 μm to 14 μm. In some embodiments, the thickness is 3 μm to 14 μm. In some embodiments, the thickness is 4 μm to 14 μm. In some embodiments, the thickness is 5 μm to 14 μm. In some embodiments, the thickness is 6 μm to 14 μm. In some embodiments, the thickness is 7 μm to 14 μm. In some embodiments, the thickness is 8 μm to 14 μm. In some embodiments, the thickness is 9 μm to 14 μm. In some embodiments, the thickness is 10 μm to 14 μm. In some embodiments, the thickness is 11 μm to 14 μm. In some embodiments, the thickness is 12 μm to 14 μm. In some embodiments, the thickness is 13 μm to 14 μm.

[0086] In some embodiments, the thickness is 0.5 μm to 13 μm. In some embodiments, the thickness is 0.5 μm to 12 μm. In some embodiments, the thickness is 0.5 μm to 11 μm. In some embodiments, the thickness is 0.5 μm to 10 μm. In some embodiments, the thickness is 0.5 μm to 9 μm. In some embodiments, the thickness is 0.5 μm to 8 μm. In some embodiments, the thickness is 0.5 μm to 7 μm. In some embodiments, the thickness is 0.5 μm to 6 μm. In some embodiments, the thickness is 0.5 μm to 5 μm. In some embodiments, the thickness is 0.5 μm to 4 μm. In some embodiments, the thickness is 0.5 μm to 3 μm. In some embodiments, the thickness is 0.5 μm to 2 μm. In some embodiments, the thickness is 0.5 μm to 1 μm.

[0087] Porosity

[0088] In some embodiments, the polyethylene film has a porosity of at least 50%. In some embodiments, the porosity is less than 95%. In some embodiments, the porosity is between 50% and 95%.

[0089] In some embodiments, the porosity is 55% to 95%. In some embodiments, the porosity is 60% to 95%. In some embodiments, the porosity is 65% to 95%. In some embodiments, the porosity is 75% to 95%. In some embodiments, the porosity is 80% to 95%. In some embodiments, the porosity is 85% to 95%. In some embodiments, the porosity is 90% to 95%.

[0090] In some embodiments, the porosity is 50% to 90%. In some embodiments, the porosity is 50% to 85%. In some embodiments, the porosity is 50% to 80%. In some embodiments, the porosity is 50% to 75%. In some embodiments, the porosity is 50% to 70%. In some embodiments, the porosity is 50% to 65%. In some embodiments, the porosity is 50% to 60%. In some embodiments, the porosity is 50% to 55%.

[0091] In some embodiments, the porosity is 55% to 86%.

[0092] Recovery after the hole-opening challenge

[0093] In some embodiments, the recovery rate at 1 hour after a 1-bar perforation challenge is at least 69%. In some embodiments, the recovery rate at 1 hour after a 1-bar perforation challenge is 99% or less.

[0094] In some embodiments, the recovery rate at 1 hour after the 1-bar opening challenge is 74% to 99%. In some embodiments, the recovery rate at 1 hour after the 1-bar opening challenge is 79% to 99%. In some embodiments, the recovery rate at 1 hour after the 1-bar opening challenge is 84% ​​to 99%. In some embodiments, the recovery rate at 1 hour after the 1-bar opening challenge is 89% to 99%. In some embodiments, the recovery rate at 1 hour after the 1-bar opening challenge is 94% to 99%.

[0095] In some embodiments, the recovery rate at 1 hour after a 1-bar opening challenge is 69% to 94%. In some embodiments, the recovery rate at 1 hour after a 1-bar opening challenge is 69% to 89%. In some embodiments, the recovery rate at 1 hour after a 1-bar opening challenge is 69% to 84%. In some embodiments, the recovery rate at 1 hour after a 1-bar opening challenge is 69% to 79%. In some embodiments, the recovery rate at 1 hour after a 1-bar opening challenge is 69% to 74%.

[0096] In some embodiments, the recovery rate at 1 hour after the 1-bar opening challenge is 95% to 99%. In some embodiments, the recovery rate at 1 hour after the 1-bar opening challenge is 96% to 99%. In some embodiments, the recovery rate at 1 hour after the 1-bar opening challenge is 97% to 99%. In some embodiments, the recovery rate at 1 hour after the 1-bar opening challenge is 98% to 99%.

[0097] In some embodiments, the recovery rate at 1 hour after the 1-bar perforation challenge is 94% to 98%. In some embodiments, the recovery rate at 1 hour after the 1-bar perforation challenge is 94% to 97%. In some embodiments, the recovery rate at 1 hour after the 1-bar perforation challenge is 94% to 96%. In some embodiments, the recovery rate at 1 hour after the 1-bar perforation challenge is 94% to 95%.

[0098] Bubble

[0099] In some embodiments, the polymer film has a bubble point of 7 psi to 200 psi. In some embodiments, the bubble point is 10 psi to 200 psi. In some embodiments, the bubble point is 15 psi to 200 psi. In some embodiments, the bubble point is 20 psi to 200 psi. In some embodiments, the bubble point is 25 psi to 200 psi. In some embodiments, the bubble point is 30 psi to 200 psi. In some embodiments, the bubble point is 35 psi to 200 psi. In some embodiments, the bubble point is 40 psi to 200 psi. In some embodiments, the bubble point is 45 psi to 200 psi. In some embodiments, the bubble point is 50 psi to 200 psi. In some embodiments, the bubble point is 55 psi to 200 psi. In some embodiments, the bubble point is 60 psi to 200 psi. In some embodiments, the bubble point is 65 psi to 200 psi. In some embodiments, the bubble point is 70 psi to 200 psi. In some embodiments, the bubble point is 75 psi to 200 psi. In some embodiments, the bubble point is 80 psi to 200 psi. In some embodiments, the bubble point is 85 psi to 200 psi. In some embodiments, the bubble point is 90 psi to 200 psi. In some embodiments, the bubble point is 95 psi to 200 psi. In some embodiments, the bubble point is 100 psi to 200 psi. In some embodiments, the bubble point is 105 psi to 200 psi. In some embodiments, the bubble point is 110 psi to 200 psi. In some embodiments, the bubble point is 115 psi to 200 psi. In some embodiments, the bubble point is 120 psi to 200 psi. In some embodiments, the bubble point is 125 psi to 200 psi. In some embodiments, the bubble point is 130 psi to 200 psi. In some embodiments, the bubble point is 135 psi to 200 psi. In some embodiments, the bubble point is 140 psi to 200 psi. In some embodiments, the bubble point is 145 psi to 200 psi. In some embodiments, the bubble point is 150 psi to 200 psi. In some embodiments, the bubble point is 155 psi to 200 psi. In some embodiments, the bubble point is 160 psi to 200 psi. In some embodiments, the bubble point is 165 psi to 200 psi. In some embodiments, the bubble point is 170 psi to 200 psi. In some embodiments, the bubble point is 175 psi to 200 psi. In some embodiments, the bubble point is 180 psi to 200 psi. In some embodiments, the bubble point is 185 psi to 200 psi. In some embodiments, the bubble point is 190 psi to 200 psi. In some embodiments, the bubble point is 195 psi to 200 psi.

[0100] In some embodiments, the bubble point is 7 psi to 195 psi. In some embodiments, the bubble point is 7 psi to 190 psi. In some embodiments, the bubble point is 7 psi to 185 psi. In some embodiments, the bubble point is 7 psi to 180 psi. In some embodiments, the bubble point is 7 psi to 175 psi. In some embodiments, the bubble point is 7 psi to 170 psi. In some embodiments, the bubble point is 7 psi to 165 psi. In some embodiments, the bubble point is 7 psi to 160 psi. In some embodiments, the bubble point is 7 psi to 155 psi. In some embodiments, the bubble point is 7 psi to 150 psi. In some embodiments, the bubble point is 7 psi to 145 psi. In some embodiments, the bubble point is 7 psi to 140 psi. In some embodiments, the bubble point is 7 psi to 135 psi. In some embodiments, the bubble point is 7 psi to 130 psi. In some embodiments, the bubble point is 7 psi to 125 psi. In some embodiments, the bubble point is 7 psi to 120 psi. In some embodiments, the bubble point is 7 psi to 115 psi. In some embodiments, the bubble point is 7 psi to 110 psi. In some embodiments, the bubble point is 7 psi to 105 psi. In some embodiments, the bubble point is 7 psi to 100 psi. In some embodiments, the bubble point is 7 psi to 95 psi. In some embodiments, the bubble point is 7 psi to 90 psi. In some embodiments, the bubble point is 7 psi to 85 psi. In some embodiments, the bubble point is 7 psi to 80 psi. In some embodiments, the bubble point is 7 psi to 75 psi. In some embodiments, the bubble point is 7 psi to 70 psi. In some embodiments, the bubble point is 7 psi to 65 psi. In some embodiments, the bubble point is 7 psi to 60 psi. In some embodiments, the bubble point is 7 psi to 55 psi. In some embodiments, the bubble point is 7 psi to 50 psi. In some embodiments, the bubble point is 7 psi to 45 psi. In some embodiments, the bubble point is 7 psi to 40 psi. In some embodiments, the bubble point is 7 psi to 35 psi. In some embodiments, the bubble point is 7 psi to 30 psi. In some embodiments, the bubble point is 7 psi to 25 psi. In some embodiments, the bubble point is 7 psi to 20 psi. In some embodiments, the bubble point is 7 psi to 15 psi. In some embodiments, the bubble point is 7 psi to 10 psi.

[0101] Penetration

[0102] In some embodiments, the polyethylene film has 3x10 -16 m 2 Up to 7.4x10 -15 m 2The permeability. In some embodiments, the permeability is 3 x 10⁻⁶. -16 m 2 Up to 7x10 -15 m 2 In some embodiments, the penetration rate is 3x10⁻⁶. -16 m 2 Up to 6x10 -15 m 2 In some embodiments, the penetration rate is 3x10⁻⁶. -16 m 2 Up to 5x10 -15 m 2 In some embodiments, the penetration rate is 3x10⁻⁶. -16 m 2 Up to 4x10 -15 m 2 In some embodiments, the penetration rate is 3x10⁻⁶. -16 m 2 Up to 3x10 -15 m 2 In some embodiments, the penetration rate is 3x10⁻⁶. -16 m 2 Up to 2x10 -15 m 2 In some embodiments, the penetration rate is 3x10⁻⁶. -16 m 2 Up to 1x10 -15 m 2 In some embodiments, the penetration rate is 3x10⁻⁶. -16 m 2 Up to 9x10 -16 m 2 In some embodiments, the penetration rate is 3x10⁻⁶. -16 m 2 Up to 8x10 -16 m 2 In some embodiments, the penetration rate is 3x10⁻⁶. -16 m 2 Up to 7x10 -16 m 2 In some embodiments, the penetration rate is 3x10⁻⁶. -16 m 2 Up to 6x10 -16 m 2 In some embodiments, the penetration rate is 3x10⁻⁶. -16 m 2 Up to 5x10 -16 m 2 In some embodiments, the penetration rate is 3x10⁻⁶. -16 m 2 Up to 4x10 -16 m 2 .

[0103] In some embodiments, the penetration rate is 4x10 -16 m 2 Up to 7.4x10 -15 m 2 In some embodiments, the penetration rate is 5 x 10⁻⁶. -16 m 2 Up to 7.4x10 -15 m 2 In some embodiments, the penetration rate is 6 x 10⁻⁶. -16 m 2 Up to 7.4x10 -15 m 2 In some embodiments, the penetration rate is 7 x 10⁻⁶. -16 m 2 Up to 7.4x10 -15 m 2 In some embodiments, the penetration rate is 8 x 10⁻⁶. -16 m 2 Up to 7.4x10 -15 m 2 In some embodiments, the penetration rate is 9 x 10⁻⁶. -16 m 2 Up to 7.4x10 -15 m 2 In some embodiments, the penetration rate is 1x10⁻⁶. -15 m 2 Up to 7.4x10 -15 m 2 In some embodiments, the penetration rate is 2x10⁻¹⁰. -15 m 2 Up to 7.4x10 -15 m 2 In some embodiments, the penetration rate is 3x10⁻⁶. -15 m 2 Up to 7.4x10 -15 m 2 In some embodiments, the penetration rate is 4 x 10⁻⁶. -15 m 2 Up to 7.4x10 -15 m 2 In some embodiments, the penetration rate is 5 x 10⁻⁶. -15 m 2 Up to 7.4x10 -15 m 2 In some embodiments, the penetration rate is 6 x 10⁻⁶. -15 m 2 Up to 7.4x10 -15 m 2 In some embodiments, the penetration rate is 7 x 10⁻⁶. -15 m 2Up to 7.4x10 -15 m 2 .

[0104] In some embodiments, the permeability is 1.0 x 10⁻⁶. -15 m 2 Up to 8.0x10 -15 m 2 In some embodiments, the penetration rate is 2.0 x 10⁻⁶. -15 m 2 Up to 8.0x10 -15 m 2 In some embodiments, the penetration rate is 3.0 x 10⁻⁶. -15 m 2 Up to 8.0x10 -15 m 2 In some embodiments, the penetration rate is 4.0 x 10⁻⁶. -15 m 2 Up to 8.0x10 -15 m 2 In some embodiments, the penetration rate is 5.0 x 10⁻⁶. -15 m 2 Up to 8.0x10 -15 m 2 In some embodiments, the penetration rate is 6.0 x 10⁻⁶. -15 m 2 Up to 8.0x10 -15 m 2 In some embodiments, the penetration rate is 7.0 x 10⁻⁶. -15 m 2 Up to 8.0x10 -15 m 2 .

[0105] In some embodiments, the permeability is 1.0 x 10⁻⁶. -15 m 2 Up to 7.0x10 -15 m 2 In some embodiments, the penetration rate is 1.0 x 10⁻⁶. -15 m 2 Up to 6.0x10 -15 m 2 In some embodiments, the penetration rate is 1.0 x 10⁻⁶. -15 m 2 Up to 5.0x10 -15 m 2 In some embodiments, the penetration rate is 1.0 x 10⁻⁶. -15 m 2 Up to 4.0x10 -15 m 2 In some embodiments, the penetration rate is 1.0 x 10⁻⁶. -15 m2 Up to 3.0x10 -15 m 2 In some embodiments, the penetration rate is 1.0 x 10⁻⁶. -15 m 2 Up to 2.0x10 -15 m 2 .

[0106] Transmission loss @10kHz (at 10kHz)

[0107] In some embodiments, when tested using WEP testing at a 1 bar aperture challenge @ 10 kHz for 24 hours, the acoustic device has a transmission loss (dB) variation (i.e., a change in transmission loss, ΔTL(dB)) of less than 2.1 dB. In some embodiments, the transmission loss (dB) variation is less than 2 dB. In some embodiments, the transmission loss (dB) variation is less than 1.9 dB. In some embodiments, the transmission loss (dB) variation is less than 1.8 dB. In some embodiments, the transmission loss (dB) variation is less than 1.7 dB. In some embodiments, the transmission loss (dB) variation is less than 1.6 dB. In some embodiments, the transmission loss (dB) variation is less than 1.5 dB. In some embodiments, the transmission loss (dB) variation is less than 1.4 dB. In some embodiments, the transmission loss (dB) variation is less than 1.3 dB. In some embodiments, the transmission loss (dB) variation is less than 1.2 dB. In some embodiments, the transmission loss (dB) variation is less than 1.1 dB. In some embodiments, the transmission loss (dB) variation is less than 1 dB. In some embodiments, the transmission loss (dB) variation is less than 0.9 dB. In some embodiments, the transmission loss (dB) variation is less than 0.8 dB. In some embodiments, the transmission loss (dB) variation is less than 0.7 dB. In some embodiments, the transmission loss (dB) variation is less than 0.6 dB. In some embodiments, the transmission loss (dB) variation is less than 0.5 dB. In some embodiments, the transmission loss (dB) variation is less than 0.4 dB. In some embodiments, the transmission loss (dB) variation is less than 0.3 dB. In some embodiments, the transmission loss (dB) variation is less than 0.2 dB.

[0108] Transmission loss @3kHz (at 3kHz)

[0109] In some embodiments, when tested using WEP testing at a 1 bar aperture challenge @ 3 kHz for 24 hours, the acoustic device has a transmission loss (dB) variation (i.e., a change in transmission loss, ΔTL(dB)) of less than 2.1 dB. In some embodiments, the transmission loss (dB) variation is less than 2 dB. In some embodiments, the transmission loss (dB) variation is less than 1.9 dB. In some embodiments, the transmission loss (dB) variation is less than 1.8 dB. In some embodiments, the transmission loss (dB) variation is less than 1.7 dB. In some embodiments, the transmission loss (dB) variation is less than 1.6 dB. In some embodiments, the transmission loss (dB) variation is less than 1.5 dB. In some embodiments, the transmission loss (dB) variation is less than 1.4 dB. In some embodiments, the transmission loss (dB) variation is less than 1.3 dB. In some embodiments, the transmission loss (dB) variation is less than 1.2 dB. In some embodiments, the transmission loss (dB) variation is less than 1.1 dB. In some embodiments, the transmission loss (dB) variation is less than 1 dB. In some embodiments, the transmission loss (dB) variation is less than 0.9 dB. In some embodiments, the transmission loss (dB) variation is less than 0.8 dB. In some embodiments, the transmission loss (dB) variation is less than 0.7 dB. In some embodiments, the transmission loss (dB) variation is less than 0.6 dB. In some embodiments, the transmission loss (dB) variation is less than 0.5 dB. In some embodiments, the transmission loss (dB) variation is less than 0.4 dB. In some embodiments, the transmission loss (dB) variation is less than 0.3 dB. In some embodiments, the transmission loss (dB) variation is less than 0.2 dB.

[0110] Transmission loss @1kHz (at 1kHz)

[0111] In some embodiments, when tested using WEP testing at a 1 bar aperture challenge @ 1 kHz for 24 hours, the acoustic device has a transmission loss (dB) variation (i.e., a change in transmission loss, ΔTL(dB)) of less than 2 dB. In some embodiments, the transmission loss (dB) variation is less than 1.9 dB. In some embodiments, the transmission loss (dB) variation is less than 1.8 dB. In some embodiments, the transmission loss (dB) variation is less than 1.7 dB. In some embodiments, the transmission loss (dB) variation is less than 1.6 dB. In some embodiments, the transmission loss (dB) variation is less than 1.5 dB. In some embodiments, the transmission loss (dB) variation is less than 1.4 dB. In some embodiments, the transmission loss (dB) variation is less than 1.3 dB. In some embodiments, the transmission loss (dB) variation is less than 1.2 dB. In some embodiments, the transmission loss (dB) variation is less than 1.1 dB. In some embodiments, the transmission loss (dB) variation is less than 1 dB. In some embodiments, the transmission loss (dB) variation is less than 0.9 dB. In some embodiments, the transmission loss (dB) variation is less than 0.8 dB. In some embodiments, the transmission loss (dB) variation is less than 0.7 dB. In some embodiments, the transmission loss (dB) variation is less than 0.6 dB. In some embodiments, the transmission loss (dB) variation is less than 0.5 dB. In some embodiments, the transmission loss (dB) variation is less than 0.4 dB. In some embodiments, the transmission loss (dB) variation is less than 0.3 dB. In some embodiments, the transmission loss (dB) variation is less than 0.2 dB.

[0112] Test program

[0113] The following test procedure was used to generate the data in the "Non-restrictive Examples" section. The test procedure in this document is not intended to be restrictive.

[0114] Average surface area per unit volume:

[0115] First, the surface area per unit mass (SSA) of the polyethylene film was measured using the Brunauer-Emmett-Teller (BET) method on a Quantachrome NOV Atouch LX4 gas adsorption system (Quantachrome Instruments - Antonpah-Bointon Beach, Florida), in m³. 2The sample is expressed in g. A sample is cut from the center of the polyethylene film sheet and placed in a Type B long unit with a 9mm LG bulb (reference number 193885). The mass of the polyethylene film sample is approximately 0.1 to 0.2 grams. The tube is placed in a Beckman Coulter SA-Prep surface area degasser (model SA-PREP, P / N5102014) from Fullerton, CA, and purged with helium for 2 hours at room temperature. The sample tube is then removed from the SA-Prep degasser and weighed. A glass filling rod (reference number 193900) is placed in the unit, and the assembly is then placed in a NOV Atouch LX4 gas adsorption system. BET surface area analysis is performed using helium according to the instrument instructions to calculate the free space, with nitrogen as the adsorbed gas. The single BET surface area (m²) of each sample is recorded. 2 / g) measurement value.

[0116] The specific surface area (SSA) can be converted to surface area per volume (Sv) using the following calculation:

[0117] Sv = ρ(polymer) * SSA

[10] 6 / m]

[0118] in:

[0119] ρ(polymer) = 0.94 g / cc

[0120] SSA = Specific surface area [m²] 2 / g]

[0121] Porosity:

[0122] The sample was die-cut to form a circular segment with a radius of 5.64 cm (area = 100 cm²). 2 Each sample was weighed using a Mettler Toledo analytical balance. The bulk density of the samples was calculated using the thickness calculated by a Keyence laser (see instructions below), and the following formula was used:

[0123]

[0124] in:

[0125] ρ (bulk density) = density (g / cc)

[0126] m = mass (g)

[0127] r = radius of the circle (5.64cm)

[0128] t = thickness (cm).

[0129] The skeletal density is the density of a solid calculated by excluding all open pores but including the volume of internal (or blind) pores. The density of polyethylene is assumed to be ρ(polymer) = 0.94 g / cc.

[0130] Therefore, the membrane porosity or total porosity within the substrate is simply the void volume of the sample divided by the total volume of the sample. Membrane porosity can be calculated using the following formula:

[0131] % porosity = 100% * {1 - ρ(packing) / ρ(skeleton)}

[0132] Penetration rate:

[0133] ATEQ airflow test measures the laminar volumetric flow rate of air passing through the membrane sample. Each membrane sample is sealed across the flow path at a distance of 2.99 cm. 2 The area is sandwiched between two plates. Using... (ATEQ Corp., Livonia, Michigan) The Premier D compact flow meter measures the gas flow rate (L / hr) through each membrane sample by challenging the membrane sample with a pressure difference of 1.2 kPa (12 mbar). The instrument operates using calibrated 30-liter and 150-liter flow tubes for gas flow measurements in the ranges of 0.5 to 30 L / h and 3.8 to 150 L / h, respectively.

[0134] For ATEQ measurements at 12 mbar, the Darcy permeability of air at room temperature can be calculated as follows:

[0135] Penetration rate (m) 2 ) = 2.073 x 10 -17 *ATEQ*t

[0136] in:

[0137] ATEQ[@12 mbar (at 12 mbar)](L / h)

[0138] t = thickness (μm).

[0139] thickness:

[0140] The non-contact thickness of the film was measured using a Keyence LS-7600 laser system (commercially available from Keyence America). Optical measurements were performed by gently placing the sample film against a polished stainless steel cylinder with a diameter of 1 inch and smoothing it with minimal applied tension. The sample thickness was determined by measuring the shadow cast in the parallel optical path at both ends of the Keyence laser micrometer. The average of three measurements was used.

[0141] Bubble:

[0142] Liquids with surface free energy less than that of stretched porous polyethylene can be extruded from the structure by applying a pressure differential. This clearing begins with the largest channel. A channel is then created through which a large flow of nitrogen gas can occur. The nitrogen gas flow manifests as a steady stream of small bubbles passing through the liquid layer at the top of the sample. The pressure at which the first large flow occurs is called the bubble point and depends on the surface tension of the test fluid and the size of the largest opening. The bubble point can be used as a relative measure of membrane structure and is often associated with other types of performance metrics, such as filtration efficiency.

[0143] According to the general teachings of ASTM F316-03, the bubble point was measured using a capillary flow porosity meter (model 3Gzh from Quanta Instruments). The sample holder consisted of a porous metal plate (part number: 196450, Anton Paar) with a diameter of 25.4 mm and a plastic mask (part number ABF-300, Professional Plastics) with an inner diameter of 18 mm and an outer diameter of 24.5 mm. The sample was placed between the metal plate and the plastic mask. The sample was then clamped and sealed using an O-ring (part number: 193798, Anton Paar). The sample was wetted with the test fluid (silicone fluid, 10 cSt, surface tension 19.75 dynes / cm).

[0144] Transmission loss:

[0145] Transmission loss and phase angle were tested using Impedance Tube Transmission Matrix Test (“ITTMT”), a modified version of ASTM-E2611-09, a standard test method for measuring normal incident sound transmission loss and phase based on a four-microphone transmission matrix method. This document describes all modifications to ASTM-E2611-09. The transmission matrix of the components was measured, and the T12 element of the transmission matrix was used as the acoustic impedance value for all components described in the example.

[0146] The impedance tube is used for measurements across a frequency range of 500 Hz to 20000 Hz. The tube has an inner diameter of 8 mm. The impedance tube is designed according to ASTM E1050-12 and ASTM E2611-09. A JBL 2426H compression driver is mounted at one end of the impedance tube and powered by a Bruel and Kjaer 2735 amplifier connected to a 31-band ART 351 graphic equalizer. The measurement system uses four Bruel and Kjaer 4138 microphones connected to a 4-channel Bruel and Kjaer 3160-A-042LAN-XI front-end with generator output. Data acquisition and processing are performed using a Bruel and Kjaer PULSE Labshop with version 21 of the 7758 acoustic materials testing software.

[0147] The sample assembly being tested has an inner diameter of 1.5 mm, which is smaller than the inner diameter of the impedance tube. Therefore, a pair of tapered adapters are required to mount the sample assembly. The converging cone has an inlet diameter of 8 mm and an outlet diameter of 1.5 mm. The diverging cone has an inlet diameter of 1.5 mm and an outlet diameter of 8 mm.

[0148] When using a tapered adapter, additional data processing is required to account for the convergent geometry of the tapered body. The theoretical equations for calculating the transmission matrix of the tapered adapter are derived and can be found in the literature (Hua, X. and Herrin, D., “Practical Considerations when using the Two-Load Method to Determine the Transmission Loss of Mufflers and Silencers”, SAE International Passenger Car Magazine - Mechanical Systems, 6(2):1094-1101, 2013 & Mechel, FP (2008). Acoustic Formulas. New York, NY: Springer).

[0149] Maximum tensile modulus:

[0150] To determine the maximum tensile modulus, sample polyethylene films were cut in both the longitudinal and transverse directions using an ASTM D412F die (D412F). A load cell equipped with a flat clamp and a 100N load cell was used. A 5565 (Illinois Tool Works Inc., Norwood, Massachusetts) tensile testing machine was used to measure tensile load as a function of displacement. The clamp separation distance was set to 8.26 cm, and an ASTM-defined gauge length of 5.89 cm was used, with a strain rate of 0.847 cm / s or 14.4% / s. A data point was captured every 20 ms. After the sample was placed in the clamp, it was retracted 1.27 cm (introducing relaxation into the sample), and the test continued at the previously specified strain rate. As the sample relaxed, the load cell recorded a baseline zero force; a certain amount of noise was present in the signal, which was quantified by calculating its standard deviation. Three samples for each condition were tested individually in each orthogonal (e.g., longitudinal and transverse) direction. For each test, the maximum tensile modulus was determined using a maximum linear fit, as further described below, and their corresponding average values ​​were reported.

[0151] The maximum linear fit is determined by importing raw data from the tensile testing machine into a data analysis program.

[0152] The zero-strain point for each sample is established as follows. At each data point in the tensile test, determine whether the load exceeds twice the standard deviation of the baseline zero-force measurement. When a series of five data points meets this criterion, the sample is considered to be under stress. The last data point preceding this series is designated as the zero-strain point.

[0153] The tensile modulus is the gradient of a stress / strain diagram. Starting from the zero strain point, the tensile modulus is calculated by performing a series of linear stress-strain fits on consecutive sets of five data points collected by a tensile testing machine. The specific set of data with the largest gradient linear fit is selected as the maximum tensile modulus. Three samples are tested in each orthogonal direction (e.g., longitudinal and transverse) and their respective averages are reported. The larger of the two average maximum tensile moduli determined for the two orthogonal directions is designated as the maximum tensile modulus in the first direction. The smaller of the two average maximum tensile moduli determined for the two orthogonal directions is designated as the maximum tensile modulus in the second direction.

[0154] Geometric mean modulus:

[0155] Then, the geometric mean of the maximum tensile modulus determined by the maximum linear fit for each membrane discussed above is calculated using the following equation:

[0156] Geometric mean modulus = square root {(maximum longitudinal tensile modulus) * (maximum transverse tensile modulus)}.

[0157] Balance ratio of maximum tensile modulus

[0158] The equilibrium ratio of the maximum tensile modulus is calculated using the following equation:

[0159] Modulus balance ratio = (absolute maximum value of maximum modulus in a single direction) / (value of maximum modulus in a direction orthogonal to the direction with the largest maximum modulus).

[0160] Transmission loss tests before and after stress testing:

[0161] The sample assembly was subjected to the following pressure test procedure. The purpose of this test was to replicate the pressure applied to the membrane assembly in a device immersed at a certain water depth for a given period of time. The transmission loss spectrum was measured before the pressure test and then remeasured 24 hours after the pressure test. The change in transmission loss (dB) due to the pressure test was calculated by subtracting the transmission loss before the test from the transmission loss after the test.

[0162] Biaxial pressure test

[0163] The biaxial, out-of-plane displacement of the membrane caused by air or water pressure stress is based on the test method described in ASTM D3786 / D3786M-13, Bursting Strength of Textile Fabrics, with the addition of a single-point laser (Keyence CCD laser displacement sensor LK-G32) to track the vertical deflection at the center of the membrane. To measure the membrane displacement under applied challenge pressure, a pressure-sensitive adhesive ( 4983) A flat sheet of composite material is inserted into an FR4-membrane-FR4 specimen interlayer with a 1.6 mm diameter orifice, and the entire assembly is held in place in a metal fixture with a 1.6 mm orifice, the top plate being clamped with screws. The metal fixture is connected to an air-containing pressure vessel. The pressure vessel is connected to a control box with programmable features, enabling pressure ramping and air pressure control. The control box is programmed to increase the input pressure at a ramp rate of 1.0 psi per second until a maximum pressure of 14.5 psi is reached. This target pressure (e.g., 14.5 psi) represents a 10-meter immersion depth rating as an industry standard. The sample is held at the target pressure for 30 minutes, then depressurized for an additional 60 minutes. During the protocol, a single-point laser, centered on the material, is used to evaluate the out-of-plane displacement during the 30-minute pressurization phase at 14.5 psi and the 60-minute recovery phase after depressurization from the test sample. The ratio of the membrane deflection at the center point at the end of the 60-minute relaxation phase to the maximum deflection reached under pressure is defined as % elastic recovery.

[0164] Figure 4An example setup for a pressure test is shown. A pressure test can be performed by placing a sample membrane 100 between two rigid supports 102, 104. A pressure (air or water) of a selected level can then be applied to the membrane. The center height of the dome 106 caused by the applied pressure can be measured, for example, using a Keyence laser displacement meter. For instance, a pressure test may include applying 1 bar of air or water pressure to the membrane 100 for 30 minutes. After this period, no further pressure is applied, and the membrane 100 is allowed to return to its initial state.

[0165] Non-restrictive examples

[0166] One method for producing porous polyethylene membranes is via a wet or gel process. In this process, polyethylene is mixed with a hydrocarbon liquid and other additives. The mixture is heated over a polymer melt and extruded into a sheet. The sheet can then be biaxially oriented before and / or after the extraction of the hydrocarbon liquid, thereby producing a microporous membrane. Various process details are known, for example, in US 5,248,461; US ​​4,873,034; US 5,051,183; and US 6566012; each of which is incorporated herein by reference in its entirety. Other discussions include casting and stretching of filled and unfilled UHMW-polyethylene films (Ir. FHAssinck, Centre for Polymers and Composites, Eindhoven University of Technology, November 1995) and (Porous Biaxial, Stretched UHMWPE Films, HMFortuin, DSM Research BV, Department of Materials Technology – 5th International Conference on Environmental Ergonomics).

[0167] Tables 1 and 2 below show the properties of nine example membranes (Examples 1-9) and four comparative membranes (Comparative Examples 1-4). Examples 1-9 all use polyethylene membranes and exhibit low acoustic transmission loss after 24 hours of pressure testing (as shown in Table 3). In contrast, Comparative Examples 1-4 exhibit high acoustic transmission loss after 24 hours of pressure testing.

[0168] The sample components and comparative sample components described and tested in this paper are prepared as follows.

[0169] All example and comparative sample assemblies include two adhesive-backed glass fiber sample carriers used to construct a sandwich containing a flat sheet film—hereafter referred to simply as a glass fiber sample carrier. 4983) was applied to one side of a glass fiber sheet (commercially available from McMaster-Carl, product number 1331T37) to prepare the sample. The glass fiber / adhesive sheet was then laser-cut into a sample. Subsequently, a 1.5 mm diameter hole was made in the center, aligned with the inner hole of the impedance tube and corresponding to the effective area of ​​the sample to be measured.

[0170] Cut a piece of film positioned in a four-sided rectangular cardboard frame from two adjacent sides of the frame to release residual tension, and place it on a smooth, level surface so that the film is flat and without any wrinkles. Remove the adhesive peel liner from the pre-cut fiberglass sample carrier to expose the adhesive. With the adhesive layer exposed, gently place the sample carrier on the film and trim any excess film from the periphery of the sample carrier. Then, place the sample carrier on the alignment jig with the film side up. Remove the peel liner from the second fiberglass sample carrier and place it on the alignment jig with the adhesive side down and towards the film. Apply low (i.e., manually) pressure to bring the bottom and top sample carriers together to form an assembly with the following stack: fiberglass sample carrier / adhesive / film / adhesive / fiberglass sample carrier.

[0171] Example 1

[0172] The gel-processed ultra-high molecular weight polyethylene (UHMWPE) film has a mass / area ratio of 2.44 g / m². 2 The bubble point is 148 psi, and it reaches a concentration of 12 mbar and 2.99 cm. 2 The airflow rate is 4.9 L / hr, the thickness is 9.6 μm, the porosity is 73%, and the surface area per unit volume is 65

[10] . 6 The maximum tensile strength in the first direction is 280 MPa, the maximum tensile strength in the second direction (orthogonal to the first direction) is 241 MPa, the tensile modulus in the first direction is 623 MPa, and the tensile modulus in the second direction is 509 MPa.

[0173] Example 2

[0174] The gel-processed UHMWPE membrane has a mass / area ratio of 2.63 g / m². 2 The bubble point is 148 psi, and it reaches 12 mbar and 2.99 cm. 2 The airflow rate is 3.8 L / hr, the thickness is 9.6 μm, the porosity is 70.9%, and the surface area per unit volume is 59.1

[10] 6 The maximum tensile strength in the first direction is 240 MPa, the maximum tensile strength in the second direction (orthogonal to the first direction) is 216 MPa, the tensile modulus in the first direction is 452 MPa, and the tensile modulus in the second direction is 386 MPa.

[0175] Example 3

[0176] A gel-processed membrane with an oleophobic coating was applied by exposing the membrane of Example 2 to a mixture of 0.5% FluoroPel 800 perfluoroalkyl copolymer (source: Cytonix) and 3M Fluorinert Liquid FC-84 (source: 3M) and drying it in a convection oven at 80°C for approximately 15 minutes. The coated membrane has the following properties: mass / area of ​​2.60 g / m². 2 The bubble point is 178 psi, and it reaches a concentration of 12 mbar and 2.99 cm. 2 The airflow rate is 1.7 L / hr, the thickness is 8.8 μm, the porosity is 68.6%, and the surface area per unit volume is 47.8

[10] 6 The maximum tensile strength in the first direction is 234 MPa, the maximum tensile strength in the second direction is 192 MPa, the tensile modulus in the first direction is 578 MPa, and the tensile modulus in the second direction is 420 MPa.

[0177] Example 4

[0178] The gel-processed UHMWPE membrane has a mass / area ratio of 2.63 g / m². 2 The bubble point is 148 psi, and it reaches 12 mbar and 2.99 cm. 2 The airflow rate is 3.8 L / hr, the thickness is 9.6 μm, the porosity is 70.9%, and the surface area per unit volume is 59.1

[10] 6 The maximum tensile strength in the first direction is 240 MPa, the maximum tensile strength in the second direction is 216 MPa, the tensile modulus in the first direction is 452 MPa, and the tensile modulus in the second direction is 386 MPa.

[0179] Example 5

[0180] The gel-processed UHMWPE membrane has a mass / area ratio of 3.85 g / m². 2 The bubble point is 135 psi, and it reaches 12 mbar and 2.99 cm. 2 The airflow rate is 3.8 L / hr, the thickness is 12.6 μm, the porosity is 67.4%, and the surface area per unit volume is 62.9

[10] 6 The maximum tensile strength in the first direction is 267 MPa, the maximum tensile strength in the second direction is 225 MPa, the tensile modulus in the first direction is 594 MPa, and the tensile modulus in the second direction is 499 MPa.

[0181] Example 6

[0182] The gel-processed UHMWPE membrane has a mass / area ratio of 3.83 g / m². 2 The bubble point is 135 psi, and it reaches 12 mbar and 2.99 cm. 2 The airflow rate is 3.1 L / hr, the thickness is 12.6 μm, the porosity is 67.5%, and the surface area per unit volume is 59.8

[10] 6 The maximum tensile strength in the first direction is 328 MPa, the maximum tensile strength in the second direction is 190 MPa, the tensile modulus in the first direction is 442 MPa, and the tensile modulus in the second direction is 279 MPa.

[0183] Example 7

[0184] A gel-processed membrane with an oleophobic coating was applied by exposing the membrane of Example 6 to a mixture of 0.5% FluoroPel 800 perfluoroalkyl copolymer (source: Cytonix) and 3M fluorinated liquid FC-84 (source: 3M) and drying it in a convection oven at 80°C for approximately 15 minutes. The coated membrane has the following properties: mass / area of ​​2.60 g / m². 2 The bubble point is 165 psi, at 12 mbar and 2.99 cm. 2 The airflow rate is 2.2 L / hr, the thickness is 13.6 μm, the porosity is 69.7%, and the surface area per unit volume is 49.6

[10] 6 The maximum tensile strength in the first direction is 277 MPa, the maximum tensile strength in the second direction is 150 MPa, the tensile modulus in the first direction is 460 MPa, and the tensile modulus in the second direction is 356 MPa.

[0185] Example 8

[0186] The gel-processed UHMWPE membrane has a mass / area ratio of 3.83 g / m². 2 The bubble point is 135 psi, and it reaches 12 mbar and 2.99 cm. 2 The airflow rate is 3.1 L / hr, the thickness is 12.6 μm, the porosity is 67.5%, and the surface area per unit volume is 59.8

[10] 6 The maximum tensile strength in the first direction is 328 MPa, the maximum tensile strength in the second direction is 190 MPa, the tensile modulus in the first direction is 442 MPa, and the tensile modulus in the second direction is 279 MPa.

[0187] Example 9

[0188] The gel-processed UHMWPE membrane has a mass / area ratio of 2.5 g / m². 2 The bubble point is 177 psi, and it reaches a concentration of 2.99 cm at 12 mbar.2 The airflow rate is 2.5 L / hr, the thickness is 6.1 μm, the porosity is 57.1%, and the surface area per unit volume is 64.7

[10] 6 The maximum tensile strength in the first direction is 306 MPa, the maximum tensile strength in the second direction is 155 MPa, the tensile modulus in the first direction is 910 MPa, and the tensile modulus in the second direction is 428 MPa.

[0189] Comparison Example 1

[0190] Using a biaxial scaling apparatus, a gel-processed membrane, identical to the one in Example 1, was heated to 120°C for 180 seconds while being constrained in both the longitudinal and transverse directions. The sample was then scaled back in the transverse direction at a rate of 2% / second to 85% of its initial length in that direction. Final properties included a mass / area of ​​3.3 g / m². 2 At 12 millibars and 2.99 cm 2 The airflow rate is 2.5 L / hr, the thickness is 8.4 μm, the porosity is 58.2%, and the surface area per unit volume is 34.9

[10] 6 The maximum tensile strength in the first direction is 264 MPa, the maximum tensile strength in the second direction is 169 MPa, the tensile modulus in the first direction is 511 MPa, and the tensile modulus in the second direction is 254 MPa.

[0191] Comparison Example 2

[0192] Using a biaxial scaling apparatus, a gel-processed membrane, identical to the one in Example 2, was heated to 120°C for 180 seconds while being constrained in both the longitudinal and transverse directions. The sample was then retracted transversely at a rate of 2% / second to 85% of its initial length in that direction. Final properties included a mass / area of ​​3.24 g / m². 2 The bubble point is 118 psi, and it reaches 12 mbar and 2.99 cm. 2 The airflow rate is 4.7 L / hr, the thickness is 9.8 μm, the porosity is 64.8%, and the surface area per unit volume is 38.3

[10] 6 The maximum tensile strength in the first direction is 289 MPa, the maximum tensile strength in the second direction is 196 MPa, the tensile modulus in the first direction is 655 MPa, and the tensile modulus in the second direction is 323 MPa.

[0193] Comparison Example 3

[0194] Using a biaxial scaling machine, a gel-processed membrane, identical to the one in Example 2, was heated to 120°C for 180 seconds while being constrained in both the longitudinal and transverse directions. Final properties included a mass / area of ​​2.6 g / m².2 The bubble point is 123 psi, and it is at 12 mbar and 2.99 cm. 2 The airflow rate is 4.5 L / hr, the thickness is 7.4 μm, the porosity is 62.9%, and the surface area per unit volume is 36.3

[10] 6 The maximum tensile strength in the first direction is 270 MPa, the maximum tensile strength in the second direction is 172 MPa, the tensile modulus in the first direction is 787 MPa, and the tensile modulus in the second direction is 752 MPa.

[0195] Comparison Example 4

[0196] Commercially available gel-processed lithium-ion battery separators (Gelon LIB Group of China) have a mass / area ratio of 10.7 g / m². 2 A 16-micron thick film with a matrix tensile strength of 28,800 psi in the longitudinal direction and 23,600 psi in the transverse direction was placed in a biaxial scaling machine. The initial film was heated to 125°C for 180 seconds while being constrained in both directions. The sample was then expanded at a rate of 1% / s in both the transverse and machine directions to a ratio of 3:1 in each direction. Final properties included a mass / area of ​​1.63 g / m². 2 The bubble point is 95 psi, and it reaches 12 mbar and 2.99 cm. 2 The airflow rate is 16 L / hr, the thickness is 6.2 μm, the porosity is 72.1%, and the surface area per unit volume is 48.4

[10] 6 The maximum tensile strength in the first direction is 394 MPa, the maximum tensile strength in the second direction is 317 MPa, the tensile modulus in the first direction is 1265 MPa, and the tensile modulus is 890 MPa.

[0197] Table 1

[0198]

[0199]

[0200] Table 2

[0201]

[0202] Table 3

[0203]

[0204] As shown in Table 3, the transmission loss in Comparative Examples 1-4 is higher than that in Examples 1-9 of the present invention.

[0205] Other objects and advantages of this disclosure will become apparent from the following description taken in conjunction with the accompanying drawings, among the benefits and improvements already disclosed. Detailed embodiments of this disclosure are disclosed herein; however, the disclosed embodiments are merely illustrative of the present disclosure as it can be implemented in various forms. Furthermore, each example given with respect to the various embodiments of this disclosure is intended to be illustrative and not restrictive.

[0206] Throughout this specification and claims, unless the context clearly specifies otherwise, the following terms shall have the meaning explicitly associated with this document. The phrases “in one embodiment,” “in an embodiment,” and “in some embodiments” as used herein do not necessarily refer to the same embodiment(s), but may refer to the same embodiment. Furthermore, the phrases “in another embodiment” and “in some other embodiments” as used herein do not necessarily refer to different embodiments, but may refer to different embodiments. All embodiments of this disclosure are intended to be composable without departing from the scope or spirit of this disclosure.

[0207] All existing patents, publications and test methods cited in this article are incorporated herein in their entirety by way of reference.

[0208] The terminology used herein is intended to describe embodiments and is not intended to be limiting. The terms “a,” “an,” and “the” also include plural forms unless otherwise expressly stated. When used in this specification, the terms “comprising” and / or “including” specifically mean the presence of the stated features, integrals, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integrals, steps, operations, elements, and / or components.

[0209] It should be understood that changes in details may be made without departing from the scope of this disclosure, particularly in terms of the construction materials used and the shape, size, and arrangement of components. This specification and the described embodiments are exemplary, and the true scope and spirit of this disclosure are indicated by the appended claims.

Claims

1. A component comprising: An acoustic device, wherein the acoustic device comprises: polyethylene film, The polyethylene film has a first direction and a second direction, wherein the second direction is orthogonal to the first direction: A thickness of 0.5 μm to 14 μm, wherein the thickness defines a thickness direction, and the first direction and the second direction are each orthogonal to the thickness direction; The surface area per unit volume is at least 39 x 10. 6 / m; The geometric mean tensile modulus is 250 to 750 MPa; The maximum tensile modulus in the first direction is 440 to 915 MPa; and the maximum tensile modulus in the second direction is 275 to 515 MPa.

2. The component according to claim 1, characterized in that, The acoustic device is a loudspeaker, a microphone, or any combination thereof.

3. The component according to any one of claims 1 or 2, characterized in that, When tested using WEP testing at 24 hours after a 1 bar aperture challenge at 3 kHz, the acoustic device exhibits an average transmission loss (dB) variation of less than 2.1 dB.

4. The component according to claim 1 or 2, characterized in that, The polyethylene film has a tensile modulus balance of 1 to 2.

1.

5. The component according to claim 1 or 2, characterized in that, The geometric mean tensile modulus is 350 to 650 MPa.

6. The component according to claim 1 or 2, characterized in that, The polyethylene film has a porosity of 50% to 95%.

7. The component according to claim 1 or 2, characterized in that, The polyethylene film has a porosity of 55% to 86%.

8. The component according to claim 1 or 2, characterized in that, The percentage recovery rate was at least 69% one hour after the 1-bar opening challenge.

9. The component according to claim 1 or 2, characterized in that, The polyethylene film has a bubble point of 7 psi to 200 psi.

10. The component according to claim 1 or 2, characterized in that, The polyethylene film has a 1x10 -15 m 2 Up to 8x10 - 15 m 2 Penetration rate.

11. The component according to claim 1 or 2, characterized in that, The polyethylene film has a 3x10 -16 m 2 Up to 7.4x10 -15 m 2 Penetration rate.

12. The component according to claim 1 or 2, characterized in that, The polyethylene film is an expanded polyethylene film.

13. The component according to claim 1 or 2, characterized in that, The maximum tensile modulus in the first direction is greater than the maximum tensile modulus in the second direction.

14. The component according to claim 1 or 2, characterized in that, The first direction is one of the longitudinal and transverse directions of the polyethylene film, while the second direction is the other of the longitudinal and transverse directions of the polyethylene film.

15. The component according to claim 1 or 2, characterized in that, The tensile modulus is the gradient of the stress / strain diagram, calculated starting from the 0 strain point by performing a series of linear stress-strain fits on consecutive sets of five data points collected by a tensile testing machine, and selecting the specific sequence of data with the largest gradient as the maximum tensile modulus; and Three samples were tested in the orthogonal longitudinal and orthogonal transverse directions, and their respective averages were reported. The larger of the two average maximum tensile moduli determined for the orthogonal longitudinal and transverse directions was designated as the maximum tensile modulus in the first direction, and the smaller of the two average maximum tensile moduli determined for the orthogonal longitudinal and transverse directions was designated as the maximum tensile modulus in the second direction.

Citation Information

Patent Citations

  • Process for producing microporous ultra-high-molecular-weight polyolefin membrane

    US4873034A

  • Microporous polyolefin membrane and method of producing same

    US5051183A

  • Process of making microporous films of UHMWPE

    US5248461A

  • Polyolefin microporous film and method for preparing the same

    US6566012B1

  • Vibro acoustic cover using expanded PTFE composite

    CN107820462A