A kind of trimanganese tetraoxide for lithium manganate battery and its preparation method and application

By controlling the reaction conditions to prepare manganese tetroxide with a particle size of 5-7 μm, the problem of grain agglomeration was solved, and efficient production and performance improvement of lithium manganese oxide batteries were achieved.

CN117886362BActive Publication Date: 2026-11-24JIAOZUO BANLV NANOMATERIALS ENG CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211253228.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-13
Publication Date
2026-11-24
Estimated Expiration
2042-10-13

AI Technical Summary

Technical Problem

In the current production process of manganese tetroxide, grain agglomeration is prone to occur, and the reaction time cannot be flexibly controlled, which affects the performance of lithium manganese oxide batteries.

Method used

Manganese sulfate solution and alkali metal hydroxide solution are reacted in a reactor containing ammonium salt solution. By controlling reaction conditions such as temperature, stirring speed and feeding method, manganese tetroxide with a particle size of 5-7 μm is generated, inhibiting grain agglomeration and flexibly controlling the synthesis time.

Benefits of technology

Stabilizes the particle size of manganese tetroxide, improves yield and purity, and is suitable for the preparation of lithium manganese oxide batteries, enhancing the cycle performance of the batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117886362B_ABST
    Figure CN117886362B_ABST
Patent Text Reader

Abstract

This invention provides manganese tetroxide (MnO) for lithium manganese oxide batteries, its preparation method, and its application. The preparation method includes the following steps: manganese sulfate solution and alkali metal hydroxide solution are continuously or intermittently pumped into a reactor containing an ammonium salt solution using metering pumps; air or oxygen is continuously introduced into the reactor, and the reaction is carried out under stirring for a period of time; after the addition of reactants, the reaction continues for 3-5 hours until the reaction is completed; the precipitate is filtered out, washed, and dried to obtain manganese tetroxide. This method controls the addition of reactants to allow for the on / off agglomeration of the generated manganese tetroxide crystals, stabilizing the particle size of manganese tetroxide during the synthesis process. The synthesis time can be freely set according to the reactor volume or other factors, resulting in high synthesis yield. The manganese tetroxide particles of this invention have a particle size distribution concentrated at around 6 μm, making it suitable for the preparation of lithium manganese oxide batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of manganese tetroxide material preparation technology, specifically relating to manganese tetroxide for lithium manganese oxide batteries, its preparation method and application. Background Technology

[0002] Lithium manganese oxide is an important cathode material for lithium-ion batteries, offering advantages such as abundant resources, low material cost, good safety, and no environmental pollution. Manganese tetroxide (MTO) has the same spinel structure as lithium manganese oxide; therefore, using MTO as a precursor for sintering to prepare lithium manganese oxide can reduce the crystal transformation time and significantly shorten the solid-state sintering time. For producing high-quality lithium manganese oxide, spherical MTO is preferred as a raw material. This is because its spherical shape and small specific surface area facilitate battery processing and reduce capacity decay caused by manganese dissolution. Furthermore, the wet process for producing MTO allows for excellent control of impurity content, which helps maintain the battery's cycle performance.

[0003] Currently, the main method for producing manganese tetroxide (MnO) from manganese sulfate is to control the pH value of the reaction process, maintain a specific reaction temperature, aeration rate, and feeding rate to ensure uniform MnO formation in the reactor. However, if the pH value is too low during synthesis, it will generate recalcitrant basic manganese sulfate, resulting in excessive sulfur content in the produced MnO and affecting the electrochemical performance of lithium manganese oxide. Conversely, at higher pH values, the continuously generated MnO crystals will aggregate on the surface of existing particles, causing the particle size to increase over time. Large-sized MnO particles will negatively impact the capacity and rate performance of lithium manganese oxide.

[0004] Therefore, there is a need to provide an improved technical solution that addresses the shortcomings of the existing technology. Summary of the Invention

[0005] The purpose of this invention is to provide a manganese tetroxide for lithium manganese oxide batteries, its preparation method and application, to solve the problems of easy grain agglomeration and inflexible control of reaction time in the current production process of manganese tetroxide.

[0006] To achieve the above objectives, the present invention provides the following technical solution:

[0007] A method for preparing manganese tetroxide for lithium manganese oxide batteries, the method comprising the following steps:

[0008] Manganese sulfate solution and alkali metal hydroxide solution are continuously or intermittently pumped into a reactor containing ammonium salt solution using metering pumps.

[0009] Air or oxygen is continuously introduced into the reactor, and the reaction is carried out for a period of time under stirring conditions;

[0010] After the feeding is completed, continue to ventilate and react for 3-5 hours until the reaction is finished. Filter out the precipitate, and after washing and drying, obtain manganese tetroxide.

[0011] In the above-described method for preparing manganese tetroxide for lithium manganese oxide batteries, preferably, the concentration of the ammonium salt solution is 0.1-0.25 mol / L;

[0012] The manganese sulfate solution has a mass fraction of 20-30%, and the manganese sulfate is added at a rate of 0.06-0.07 mol / min.

[0013] In the above-described method for preparing manganese tetroxide for lithium manganese oxide batteries, preferably, the alkali metal hydroxide includes sodium hydroxide or potassium hydroxide.

[0014] The concentration of the alkali metal hydroxide solution is 20-30%.

[0015] In the method for preparing manganese tetroxide for lithium manganese oxide batteries as described above, preferably, the molar ratio of manganese sulfate to alkali metal hydroxide is 1:(2-2.05) within the same feeding cycle.

[0016] In the method for preparing manganese tetroxide for lithium manganese oxide batteries as described above, preferably, the reaction temperature in the reactor is 55-80°C and the reaction time is 9-13 h.

[0017] In the preparation method of manganese tetroxide for lithium manganese oxide batteries as described above, the stirring speed is preferably 500-750 r / min.

[0018] In the method for preparing manganese tetroxide for lithium manganese oxide batteries as described above, preferably, the ammonium salt solution is an aqueous solution of an ammonium salt, and the ammonium salt solution is one or more of ammonium chloride solution, ammonium sulfate solution, and ammonium nitrate solution.

[0019] In the method for preparing manganese tetroxide for lithium manganese oxide batteries as described above, preferably, within the same feeding cycle, the feeding time of the alkali metal hydroxide solution is shorter than the feeding time of the manganese sulfate solution.

[0020] A manganese tetroxide for use in lithium manganese oxide batteries, wherein the particle size Dv50 of the manganese tetroxide is 5-7 μm.

[0021] An application of manganese tetroxide in the preparation of lithium manganese oxide batteries.

[0022] Beneficial effects:

[0023] This invention provides a method for preparing manganese tetroxide, which involves the direct oxidation of high-purity manganese tetroxide by manganese sulfate solution and alkali metal hydroxide in an ammoniacal medium. This method controls the addition of reactants to initiate or interrupt the agglomeration of manganese tetroxide crystals, stabilizing the particle size of manganese tetroxide during synthesis. The synthesis time can be freely set according to the reactor volume or other factors, eliminating the need to passively determine the synthesis time due to crystal agglomeration.

[0024] The manganese tetroxide particles produced by this invention do not increase in size over time, with a particle size (Dv50) of 5-7 μm, specifically around 6 μm, making them suitable for the preparation of lithium manganese oxide batteries. The synthesis time can be freely controlled, eliminating the need for forced shutdowns and increasing yield.

[0025] The overall pH value is well controlled during the reaction process of this invention, ranging from 8.8 to 9.4, which inhibits the formation of basic manganese salts, improves the purity of the product, and the prepared manganese tetroxide has a manganese content of ≥70% and good sphericity. When applied to the preparation of lithium manganese oxide batteries, it is beneficial to the processing of the battery production process and improves the cycle performance of the battery. Attached Figure Description

[0026] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. Wherein:

[0027] Figure 1 The particle size distribution curve of manganese tetroxide prepared in Example 1 of this invention;

[0028] Figure 2 The data are the discharge specific capacity of the lithium manganese oxide battery sintered from manganese tetroxide in Example 1 of the present invention under different cycle numbers.

[0029] Figure 3 This is the capacity retention data of the lithium manganese oxide battery sintered from manganese tetroxide in Example 1 of the present invention under different cycle numbers. Detailed Implementation

[0030] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention are within the scope of protection of the present invention.

[0031] The present invention will now be described in detail with reference to embodiments. It should be noted that, unless otherwise specified, the embodiments and features described in the embodiments of the present invention can be combined with each other.

[0032] The present invention provides a method for preparing manganese tetroxide for lithium manganese oxide batteries. By controlling the addition of reaction raw materials, the agglomeration of manganese tetroxide crystals can be started or stopped, stabilizing the particle size of manganese tetroxide during the synthesis process. The synthesis time can be freely set according to the reactor volume or other factors, without having to passively determine the length of the synthesis time due to crystal agglomeration. This method can extend the synthesis time, increase the yield, and is suitable for mass production. The manganese tetroxide synthesized in this invention is an agglomerated particle, which is formed by the stacking of multiple manganese tetroxide crystals. It has suitable looseness and packing density, and the manganese tetroxide has high purity, with a manganese content of more than 70%. It has good sphericity, a small grain size range, and a particle size Dv50 of 5-7 μm, specifically about 6 μm. The particle size distribution is relatively concentrated. Using the manganese tetroxide prepared in this invention for the preparation of lithium manganese oxide battery materials can facilitate the processing of battery production, improve the cycle performance of the battery, and avoid the problem of increased particle size due to agglomeration, which would affect the capacity and rate performance of lithium manganese oxide.

[0033] This invention provides a method for preparing manganese tetroxide for lithium manganese oxide batteries, the method comprising the following steps:

[0034] Manganese sulfate solution and alkali metal hydroxide solution are continuously or intermittently pumped into a reactor containing ammonium salt solution using metering pumps.

[0035] Air or oxygen is continuously introduced into the reactor, and the reaction is carried out for a period of time under stirring conditions;

[0036] After the feeding is completed, continue aeration for 3-5 hours (e.g., 3.5h, 4h, 4.5h, 5h) until the reaction is complete. Filter out the precipitate, wash and dry it to obtain manganese tetroxide. Continuing aeration for 3-5 hours can completely convert the synthesized manganese hydroxide in the reactor into manganese tetroxide, improving the utilization rate of raw materials and the amount of product generated.

[0037] In a specific embodiment of the present invention, a manganese sulfate solution is continuously pumped into a reactor containing an ammonium salt solution using a metering pump, while an alkali metal hydroxide solution is intermittently pumped into the reactor containing an ammonium salt solution using a metering pump.

[0038] In a specific embodiment of the present invention, the concentration of the ammonium salt solution is 0.1-0.25 mol / L (e.g., 0.15 mol / L, 0.2 mol / L, 0.22 mol / L, 0.24 mol / L). The ammonium salt solution serves as a catalyst for the reaction synthesis. The concentration of the ammonium salt solution in the reactor needs to be maintained within a certain range to facilitate the final formation of manganese tetroxide with a particle size of approximately 6 μm. If the ammonium salt concentration is too low, the resulting manganese tetroxide particles will be small, resulting in loosely packed and low-density agglomerates, which is detrimental to the preparation of lithium manganese oxide batteries and affects battery performance. The ammonium salt solution concentration of 0.1-0.25 mol / L in this invention is suitable for a 50L reactor. Within this concentration range, manganese sulfate solution can be continuously added and alkaline solution can be added intermittently to generate manganese tetroxide with a concentrated particle size distribution and suitable size. The resulting manganese tetroxide agglomerates have high particle density and are tightly packed, making them suitable for the preparation and production of lithium manganese oxide batteries. The manganese sulfate solution has a mass fraction of 20-30% (e.g., 21%, 22%, 24%, 26%, 28%), preferably 25%.

[0039] The feeding rate of manganese sulfate is 0.06-0.07 mol / min (e.g., 0.061 mol / min, 0.062 mol / min, 0.064 mol / min, 0.066 mol / min, 0.068 mol / min), preferably 0.0607 mol / min. In one feeding cycle, such as 30 min, the amount of manganese sulfate added is 1.821 mol.

[0040] In a specific embodiment of the present invention, the alkali metal hydroxide includes sodium hydroxide or potassium hydroxide, and the concentration of the alkali metal hydroxide solution is 20-30% (e.g., 21%, 22%, 24%, 26%, 28%), preferably 25%. A higher concentration of alkali solution will cause an increase in viscosity, and the feeding speed of the metering pump will be unstable.

[0041] Within the same feeding cycle, the amount of alkali metal hydroxide added needs to be matched with the amount of manganese sulfate added. The molar ratio of manganese sulfate to alkali metal hydroxide is 1:(2-2.05) (e.g., 1:2, 1:2.01, 1:2.02, 1:2.03, 1:2.04). This ratio ensures complete product reaction and improves raw material utilization. The manganese sulfate solution and alkali metal hydroxide solution should be pumped into the reactor at a synchronized rate to facilitate the reaction and produce manganese tetroxide particles with a particle size of approximately 6 μm and appropriate bulk density. Within the same feeding cycle, the feeding time for the alkali metal hydroxide solution is shorter than that for the manganese sulfate solution. Specifically, within the same feeding cycle, for example, 30 minutes, the molar ratio of alkali metal hydroxide to manganese sulfate is 1:(2-2.05). The required alkali solution can be added within 15-25 minutes, and the manganese sulfate within 30 minutes, before proceeding to the next feeding cycle. This means that the alkali solution feeding can be intermittent, while the manganese sulfate can be fed at a continuous and stable rate. A faster alkali solution feeding rate allows the solution pH to be maintained at a higher range (8.8-9.4) in the early stages, reducing the formation of basic manganese sulfate impurities and improving product purity.

[0042] In a specific embodiment of the present invention, the ammonium salt solution is an aqueous solution of an ammonium salt, and the ammonium salt solution is one or more of ammonium chloride solution, ammonium sulfate solution, and ammonium nitrate solution;

[0043] In a specific embodiment of the present invention, the reaction temperature in the reactor is 55-80℃ (e.g., 55℃, 60℃, 65℃, 70℃, 75℃, 80℃), and the reaction time is 9-13h (e.g., 10h, 11h, 12h, 13h). The reaction time in the reactor in this invention refers to the total time from initial feeding to subsequent oxidation by introducing air or oxygen. The stirring speed is 500-750r / min (e.g., 550r / min, 580r / min, 600r / min, 620r / min, 650r / min, 680r / min, 700r / min, 720r / min, 740r / min). The reaction temperature and stirring speed affect the particle size and bulk density of the final product. Different reaction temperatures result in different oxidation rates of manganese hydroxide, which in turn affects the concentration of manganese amine in the feed solution. If the reaction temperature is too high, the particle size of the generated manganese tetroxide particles will increase. If the stirring speed is too low, the shear force will be small, and the particle size of manganese tetroxide will increase; if the reaction temperature is below 55℃, the reaction process will be too slow and difficult to control; if the stirring speed is too high, it will affect the crystallization of manganese tetroxide.

[0044] This invention provides an application of manganese tetroxide in lithium manganese oxide batteries, wherein manganese tetroxide is used in the preparation of lithium manganese oxide batteries.

[0045] Example 1

[0046] This embodiment provides a method for preparing manganese tetroxide for lithium manganese oxide batteries, comprising the following steps:

[0047] Add 20L of pure water to a 50L reactor. Use ammonium chloride as the ammonium salt, with NH4+ as the solvent. 4+ For measurement standard purposes, 4.67 mol of NH3 was added at one time. 4+ The concentration of manganese sulfate solution was 25 wt%. The manganese sulfate solution was pumped in using a metering pump at a rate of 2200 g / h (i.e., a manganese sulfate feeding rate of 0.0607 mol / min), and the feeding rate remained constant after startup. A 25 wt% sodium hydroxide solution was pumped in using a metering pump at a rate of 582.7 g / 15 min, with a 15-minute pause between pumping and stopping. The reaction temperature was controlled at 60℃; the stirring speed was controlled at 700 r / min; the air flow rate was 1.5 L / min; the feeding period was 9 hours, and after the feeding was completed, aeration continued for 4 hours until the reaction was finished, for a total reaction time of 13 hours.

[0048] The product in the reactor was sampled and tested at different reaction times, specifically after 2h, 4h, 6h, and 9h of reaction. The analysis and performance test data of the manganese tetroxide particles obtained in this example are shown in Table 1.

[0049] Table 1. Particle size distribution and purity of manganese tetroxide particles at different reaction times.

[0050]

[0051]

[0052] As shown in Table 1, the particle size did not change significantly with increasing reaction time. The particle size distribution (Dv50) of manganese tetroxide was mainly concentrated at 6 micrometers, with a relatively concentrated particle size distribution. The manganese content was 70.72%, and the tap density was 2.53 g / cm³. 3 It should be noted that the manganese content and tap density in this embodiment refer to the test values ​​of the sample after the reaction is completed, that is, the sample obtained after air or oxygen is introduced for oxidation after the feeding is completed. The data in the following embodiments and control examples are the same.

[0053] Example 2

[0054] This embodiment provides a method for preparing manganese tetroxide for lithium manganese oxide batteries, comprising the following steps:

[0055] 20L of pure water was added to the 50L reactor. Ammonium sulfate was used as the ammonium salt, with NH4+ as the solvent. 4+ For measurement standard purposes, 3.74 mol of NH3 was added at one time. 4+The concentration of manganese sulfate solution was 25 wt%. The manganese sulfate solution was pumped in using a metering pump at a rate of 2200 g / h (i.e., the manganese sulfate feeding rate was 0.0607 mol / min), and the feeding was continuous during the reaction. The 25 wt% sodium hydroxide solution was pumped in using a metering pump at a rate of 582.7 g / 20 min, with a 10-minute pause after every 20 minutes of pumping. The reaction temperature was controlled at 65℃. The stirring speed was controlled at 600 r / min. The air flow rate was 2 L / min. The feeding period was 9 hours. After the feeding period ended, the aeration continued for 4 hours until the reaction was completed. The total reaction time was 13 hours.

[0056] The product in the reactor was sampled and tested at different reaction times, specifically after 2h, 4h, 6h, and 9h of reaction. The analysis and performance test data of the manganese tetroxide particles obtained in this example are shown in Table 2.

[0057] Table 2. Particle size distribution and purity of manganese tetroxide particles at different reaction times.

[0058]

[0059] As shown in Table 2, the particle size did not change significantly with increasing reaction time. The particle size distribution (Dv50) of manganese tetroxide was mainly concentrated around 6 micrometers, with a relatively concentrated particle size distribution. The manganese content was 70.97%, and the tap density was 2.57 g / cm³. 3 .

[0060] Example 3

[0061] This embodiment provides a method for preparing manganese tetroxide for lithium manganese oxide batteries, comprising the following steps:

[0062] Add 20L of pure water to a 50L reactor. Ammonium nitrate is used as the ammonium salt, with NH4+ as the solvent. 4+ For measurement standard, 2.8 mol of NH3 was added at one time. 4+ The concentration of manganese sulfate solution was 25 wt%. The manganese sulfate solution was pumped in at a rate of 2200 g / h using a metering pump, without stopping the flow during the reaction. The concentration of 25 wt% sodium hydroxide solution was pumped in at a rate of 582.7 g / 20 min using a metering pump, with a 10-minute pause after each 20-minute pumping cycle. The reaction temperature was controlled at 70℃. The stirring speed was controlled at 600 r / min. The air flow rate was 1.5 L / min. The feeding period was 9 hours. After the feeding period ended, the air flow continued for 3 hours until the reaction was completed. The total reaction time was 12 hours.

[0063] The product in the reactor was sampled and tested at different reaction times, specifically after 2h, 4h, 6h, and 9h of reaction. The analysis and performance test data of the manganese tetroxide particles obtained in this example are shown in Table 3.

[0064] Table 3. Particle size distribution and purity of manganese tetroxide particles at different reaction times.

[0065]

[0066] As shown in Table 3, the particle size did not change significantly with increasing reaction time. The particle size distribution (Dv50) of manganese tetroxide was mainly concentrated around 6 micrometers, with a relatively concentrated particle size distribution. The manganese content was 70.56%, and the tap density was 2.49 g / cm³. 3 .

[0067] Example 4

[0068] The difference between this embodiment and Embodiment 1 is that the alkali metal hydroxide solution used is potassium hydroxide with a mass concentration of 25%. It is pumped in at a rate of 815.4 g / 15 min using a metering pump, with a 15-minute pause after each pumping. The rest is the same as in Embodiment 1 and will not be repeated here.

[0069] The manganese tetroxide particles prepared in this embodiment have a similar particle size to those in Example 1, with Dv50 mainly concentrated at 6 micrometers and a relatively concentrated particle size distribution.

[0070] Compare with Example 1

[0071] The difference between the steps in this embodiment and those in Example 1 lies in the method of adding sodium hydroxide. Other steps are the same as in Example 1, except that the sodium hydroxide solution is added continuously at a rate of 582.7 g / 30 min, without interruption. The addition time for both manganese sulfate solution and sodium hydroxide solution is 9 hours, until the reaction is complete.

[0072] The product in the reactor was sampled and tested at different reaction times, specifically after 2h, 4h, 6h, and 9h of reaction. The analysis and performance test data of the manganese tetroxide particles obtained in this example are shown in Table 4.

[0073] Table 4. Particle size distribution and purity of manganese tetroxide particles at different reaction times.

[0074]

[0075] As shown in Table 4, the particle size of the generated manganese tetroxide particles increases significantly with prolonged feeding time. Therefore, to obtain a product with a particle size of 6 micrometers, feeding should be stopped when the manganese tetroxide particle size reaches the standard. Aeration should continue for 3-5 hours until all manganese hydroxide in the feed solution is converted to manganese tetroxide. Afterward, the feed solution should be discharged, filtered, dried, and the next production cycle restarted. The time required for one production cycle is limited by the product particle size specification, preventing the reactor from reaching its maximum capacity.

[0076] Compare with Example 2

[0077] The difference between this comparative example and Example 1 is that the concentration of ammonium salt in the reactor is 0.05 mol / L, while the other steps and methods are the same as in Example 1.

[0078] In this comparative example, the Dv50 of the prepared manganese tetroxide was approximately 4 micrometers, but the tap density of the prepared manganese tetroxide was relatively low at 2.17 g / cm³. 3 This is not conducive to improving the compaction density of lithium manganese oxide batteries, and will indirectly lead to a decrease in battery energy density.

[0079]

[0080] Application examples

[0081] The manganese tetroxide prepared in Example 1 of this invention was applied to the preparation of lithium manganese oxide batteries. The discharge specific capacity and capacity retention rate of lithium manganese oxide were tested, and the performance data are shown in Table 5 below. These data are plotted as a line graph. Figure 2 and 3 As shown.

[0082] Table 5 Electrochemical performance of lithium manganese oxide

[0083]

[0084] As shown in Table 5 above, the lithium manganese oxide prepared by calcining manganese tetroxide in Example 1 of this invention exhibits high discharge specific capacity and capacity retention rate, good cycle performance, and meets the usage requirements.

[0085] In summary, this invention provides a method for preparing manganese tetroxide, which directly oxidizes manganese sulfate solution with alkali metal hydroxide in an ammoniacal medium to produce high-purity manganese tetroxide. This method controls the addition of reactants to initiate or interrupt the agglomeration of manganese tetroxide crystals, stabilizing the particle size of manganese tetroxide during synthesis. The synthesis time can be freely set according to the reactor volume or other factors, eliminating the need to passively determine the synthesis time due to crystal agglomeration.

[0086] The manganese tetroxide particles produced by this invention do not increase in size over time, with a particle size (Dv50) of 5-7 μm, specifically around 6 μm. The synthesis time can be freely controlled, eliminating the need for forced shutdowns and increasing yield.

[0087] The overall pH value is well controlled during the reaction process of this invention, ranging from 8.8 to 9.4, which inhibits the formation of basic manganese salts, improves the purity of the product, and the prepared manganese tetroxide has a manganese content of ≥70% and good sphericity. When applied to the preparation of lithium manganese oxide batteries, it is beneficial to the processing of the battery production process and improves the cycle performance of the battery.

[0088] The above are merely preferred embodiments of the present invention and are not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing manganese tetroxide for lithium manganese oxide batteries, characterized in that, The preparation method includes the following steps: continuously pumping a manganese sulfate solution into a reactor using a metering pump; intermittently pumping an alkali metal hydroxide solution into the reactor using a metering pump; the reactor contains an ammonium salt solution with a concentration of 0.1-0.25 mol / L; within the same 30-minute feeding cycle, the alkali metal hydroxide solution is added within 15-25 minutes; the molar ratio of manganese sulfate to alkali metal hydroxide is 1:(2.01-2.05); the mass fraction of the manganese sulfate solution is 20-30%. The manganese sulfate is fed at a rate of 0.06-0.07 mol / min; the alkali metal hydroxide solution has a mass concentration of 20-30%; air or oxygen is continuously introduced into the reactor; the reaction temperature is 55-80℃; the reaction is carried out for 9-13 hours under stirring; and the pH is controlled between 8.8 and 9.4 during the reaction. After the feeding is completed, the reaction continues for 3-5 hours until the reaction is finished. The precipitate is filtered out, washed, and dried to obtain manganese tetroxide, wherein the particle size Dv50 of the manganese tetroxide is 5-7 μm.

2. The method for preparing manganese tetroxide for lithium manganese oxide batteries as described in claim 1, characterized in that, The alkali metal hydroxides include sodium hydroxide or potassium hydroxide.

3. The method for preparing manganese tetroxide for lithium manganese oxide batteries as described in claim 1, characterized in that, The stirring speed is 500-750 r / min.

4. The method for preparing manganese tetroxide for lithium manganese oxide batteries as described in claim 1, characterized in that, The ammonium salt solution is an aqueous solution of an ammonium salt, and the ammonium salt solution is one or more of ammonium chloride solution, ammonium sulfate solution, and ammonium nitrate solution.

Citation Information

Patent Citations

  • Multi-element composite positive pole material for lithium secondary battery and preparation thereof

    CN101478044A

  • Preparation method of nanometer trimanganese tetroxide

    CN102627330A