A high-voltage LED chip preparation method and a high-voltage LED chip

By employing a double-layer photoresist structure consisting of positive high-viscosity photoresist and negative low-viscosity photoresist, and controlling the baking temperature and time, the problems of high photoresist cost and poor morphology in high-voltage LED chip fabrication were solved. This enabled the low-cost and high-efficiency fabrication of high-quality isolation trenches, improving production efficiency and yield.

CN117894886BActive Publication Date: 2026-11-20JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410058868.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-16
Publication Date
2026-11-20
Estimated Expiration
2044-01-16

AI Technical Summary

Technical Problem

In the current high-voltage LED chip manufacturing process, positive photoresist is expensive and improper photoresist baking can lead to the morphology of the isolation trench being far from the design requirements, affecting production efficiency and cost.

Method used

A double-layer photoresist structure consisting of positive high-viscosity photoresist and negative low-viscosity photoresist is adopted. The baking temperature and time are controlled, and the preset etching pattern is formed through multiple baking processes, avoiding abnormal isolation trenches caused by improper photoresist baking.

Benefits of technology

This reduces photolithography costs, ensures that the etching angle and appearance of the isolation trench meet requirements, improves production efficiency and yield, and saves photolithography costs per substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117894886B_ABST
    Figure CN117894886B_ABST
Patent Text Reader

Abstract

The application discloses a high-voltage LED chip preparation method and a high-voltage LED chip, and the chip preparation method comprises the following steps: epitaxially growing an epitaxial layer on a substrate; etching from a P-type semiconductor layer to the substrate direction until an N-type semiconductor layer is exposed to form an N-type mesa and a P-type mesa; coating a positive photoresist on the epitaxial layer and sequentially performing soft baking, exposure, development, first hard baking and second hard baking to obtain a first solidified glue layer; coating a negative photoresist on the first solidified glue layer and sequentially performing soft baking, exposure, film hardening and development to obtain a second solidified glue layer; etching the epitaxial layer; removing the two glue layers to obtain an isolation groove containing preset topographic features on the epitaxial wafer; preparing electrodes on the N-type mesa and the P-type mesa and preparing an electrode bridge in the corresponding isolation groove; setting a corresponding number of crystal grains as a group; and connecting the electrodes with different polarities of adjacent crystal grains in the group through the electrode bridge. The application has low photoetching cost and better topographic features of the isolation groove.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of LED chip technology, and in particular to a method for preparing a high-voltage LED chip and a high-voltage LED chip. Background Technology

[0002] High-voltage LED chips are light-emitting diode chips made by dividing the epitaxial layer of a large chip into multiple single-particle chips through etching isolation trenches during the chip manufacturing process, and then connecting the corresponding electrodes of adjacent particles in series.

[0003] To improve production efficiency, when fabricating high-voltage LED chips with high photoelectric performance requirements, it is necessary to ensure that the etching angle and appearance of the isolation trench are both good. For this reason, the isolation trench that meets the requirements is usually formed by two photolithography steps and one etching step. Specifically, firstly, a layer of photoresist is coated on the epitaxial layer and exposed, developed and hardened in sequence. Then, another layer of photoresist is coated on the first layer of photoresist and exposed, developed and hardened in sequence. Finally, the whole layer is etched. The two layers of photoresist are generally positive high-viscosity adhesives with different properties.

[0004] However, on the one hand, the high cost of using positive high-viscosity photoresist leads to a higher overall chip production cost; on the other hand, if the solvent in the first layer of positive photoresist does not evaporate completely or the first layer of positive photoresist is not baked hard enough, when the second layer of positive photoresist is exposed, the areas exposed by the two overlap, and the areas in the first layer of positive photoresist that were not removed during development will be exposed again, which may ultimately lead to the morphology of the isolation trench being far from the design requirements. Summary of the Invention

[0005] Based on this, the purpose of the present invention is to provide a method for preparing a high-voltage LED chip and a high-voltage LED chip. By sequentially forming a positive photoresist layer and a negative photoresist layer containing a preset etching pattern on an epitaxial wafer, and by controlling the temperature, heating time and exposure dose during the photoresist baking process and the exposure dose during the photoresist exposure process, an epitaxial wafer with an isolation trench containing a better etching angle and appearance can be obtained at a lower cost.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0007] On one hand, the present invention provides a method for fabricating a high-voltage LED chip, comprising the following steps:

[0008] A substrate is provided, and an epitaxial layer is epitaxially grown on the substrate, wherein the epitaxial layer includes at least an N-type semiconductor layer, an active layer and a P-type semiconductor layer grown sequentially.

[0009] The P-type semiconductor layer is etched towards the substrate until the N-type semiconductor layer is exposed to form the N-type mesa and P-type mesa of each grain;

[0010] A positive photoresist is coated on the epitaxial layer, and the photoresist layer is subjected to soft baking, exposure, development, first hard baking, and second hard baking in sequence to obtain a first cured photoresist layer containing a preset etched pattern.

[0011] A negative photoresist is coated onto the first cured adhesive layer, and the photoresist layer is subjected to soft baking, exposure, hardening and development in sequence to obtain a second cured adhesive layer containing a preset etching pattern.

[0012] Using the first and second cured adhesive layers as masks, the epitaxial layer is etched.

[0013] Remove the first and second cured adhesive layers to obtain an isolation groove with a preset morphological feature on the epitaxial wafer;

[0014] Electrodes are fabricated on the N-type and P-type mesa of each grain, and electrode bridges are fabricated in the corresponding isolation trenches. A corresponding number of grains are set as a group, and electrodes of different polarities of adjacent grains in the group are connected in series through the electrode bridges.

[0015] In addition, the high-voltage LED chip manufacturing method of the present invention described above may also have the following additional technical features:

[0016] Furthermore, the thickness of the coated positive photoresist is 8μm to 12μm.

[0017] Furthermore, both the soft baking and the first hard baking of the positive photoresist were performed using a hot plate, with a baking temperature of 90℃~120℃ and a baking time of 100S~180S.

[0018] Furthermore, the exposure dose for the positive photoresist is 750 mJ / cm. 2 ~1450mJ / cm 2 .

[0019] Furthermore, the positive photoresist is subjected to a second hard bake in an oven at a temperature of 95℃ to 115℃ for 30 to 45 minutes.

[0020] Furthermore, the thickness of the coated negative photoresist is 2.5 μm to 4.5 μm.

[0021] Furthermore, the negative photoresist is soft-baked using a hot plate method, with a baking temperature of 100℃~120℃ and a baking time of 60S~120S.

[0022] Furthermore, the exposure dose for the negative photoresist is 300 mJ / cm. 2 ~600mJ / cm 2 .

[0023] Furthermore, the negative photoresist is hardened using a hot plate baking method, wherein the baking temperature is 100℃~120℃ and the baking time is 60S~180S.

[0024] On the other hand, based on the same inventive concept, the present invention also provides a high-voltage LED chip, which is prepared by the aforementioned high-voltage LED chip preparation method.

[0025] The present invention has the following beneficial effects: By adopting a double-layer adhesive structure of positive high-viscosity photoresist and negative low-viscosity photoresist, since the cost of negative low-viscosity photoresist is lower than that of positive high-viscosity photoresist, and the amount of negative low-viscosity photoresist used on a single substrate is also lower than that used in existing solutions, the photolithography cost of negative low-viscosity photoresist on a single substrate can be significantly reduced compared to the positive high-viscosity photoresist used in existing solutions. In addition, by baking the positive high-viscosity photoresist and negative low-viscosity photoresist multiple times and controlling the baking time and temperature within an optimal range, the phenomenon of photoresist collapse and cracking caused by excessively high baking temperature and time is avoided, which would result in a smaller etching angle of the isolation trench, a smaller light-emitting area of ​​the LED chip, and abnormal etching appearance of the isolation trench. At the same time, the phenomenon of excessively sagging photoresist and air bubbles in the photoresist caused by excessively low baking temperature and time is also avoided, which would result in an excessively large etching angle of the isolation trench, abnormal metal coating, and abnormal etching appearance of the isolation trench. Attached Figure Description

[0026] Figure 1 This is a flowchart of the high-voltage LED chip fabrication method in an embodiment of the present invention;

[0027] Figure 2 This is a schematic diagram of the overall exposure of an epitaxial wafer in the existing double-layer positive photoresist process;

[0028] Figure label:

[0029] First layer of positive photoresist 100, second layer of positive photoresist 200, unremoved area after development 300;

[0030] The following detailed description, in conjunction with the accompanying drawings, will further illustrate the present invention. Detailed Implementation

[0031] To facilitate understanding of the present invention, a more complete description will be given below with reference to the accompanying drawings. Several embodiments of the invention are illustrated in the drawings. However, the invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete.

[0032] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there may be an intervening component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there may be an intervening component. The terms "vertical," "horizontal," "left," "right," and similar expressions used in this document are for illustrative purposes only.

[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0034] Generally, the cost of using positive photoresist is twice that of negative photoresist, and in a process involving two photolithography steps and one etching step, such as... Figure 2 As shown, after the first layer of positive photoresist 100 is exposed, developed, and hardened sequentially, if the solvent in the first layer of positive photoresist 100 does not evaporate completely or the first layer of positive photoresist 100 is not baked hard enough, when the second layer of positive photoresist 200 is exposed, since the exposure areas of the two overlap, the unremoved area 300 in the first layer of positive photoresist 100 located in the exposure area will be exposed again, which may eventually lead to the morphology of the isolation trench being far from the design requirements.

[0035] Therefore, this application provides a method for fabricating a high-voltage LED chip and a high-voltage LED chip, which can obtain an epitaxial wafer containing isolation trenches that meet the required morphological characteristics at a lower cost.

[0036] refer to Figure 1 This invention provides a method for fabricating a high-voltage LED chip, specifically including steps S100-S700:

[0037] S100. A substrate is provided, and an epitaxial layer is epitaxially grown on the substrate, wherein the epitaxial layer includes at least an N-type semiconductor layer, an active layer and a P-type semiconductor layer grown sequentially.

[0038] Specifically, the substrate material can be one of sapphire, SiC, Si, and ZnO, and the substrate can also be a patterned substrate or a flat substrate. As an example, the basic structure of a single GaN-based high-voltage LED chip can be: a patterned sapphire substrate, an N-type GaN layer, a multi-layer quantum well layer, and a P-type GaN layer.

[0039] S200: Etch from the P-type semiconductor layer toward the substrate until the N-type semiconductor layer is exposed to form the N-type mesa and P-type mesa of each grain;

[0040] Specifically, using a MESA layer as a mask, photoresist is sequentially applied, exposed, and developed on the epitaxial layer. Then, ICP etching is performed on the epitaxial layer to expose N-type and P-type mesa. The etched areas of the epitaxial layer form N-type mesa, and the unetched areas of the epitaxial layer after the photoresist is cleaned off form P-type mesa.

[0041] S300. A positive photoresist is coated on the epitaxial layer. Specifically, the thickness of the coated positive photoresist is 8μm to 12μm. The positive photoresist layer is then subjected to soft baking, exposure, development, first hard baking, and second hard baking in sequence to obtain a first cured photoresist layer containing a preset etching pattern.

[0042] Since moisture on the substrate surface greatly reduces the adhesion of positive photoresist, in order to enhance the adhesion between the substrate and the positive photoresist, the substrate is first dehydrated and baked, and then immediately coated with a layer of positive photoresist using a spin coating method. Specifically, during the coating process, the substrate is fixed on a vacuum chuck, a certain amount of positive photoresist is dropped onto the center of the substrate, and then the substrate is rotated to obtain a uniform photoresist coating.

[0043] In this process, the positive photoresist is soft-baked using a hot plate. The main purpose of soft baking is to allow the organic solvents in the positive photoresist to evaporate initially and to enhance its adhesion. If the organic solvents are not removed, excessively high solvent concentrations will reduce the selectivity of the developer for exposed and unexposed photoresist, resulting in incomplete removal of exposed areas during development. Furthermore, if the positive photoresist is not baked sufficiently, in addition to poor adhesion, the accuracy of subsequent exposures will also deteriorate due to the high solvent content making the positive photoresist less sensitive to light. If the positive photoresist is over-baked, it will become brittle, reducing its adhesion, and may also cause some of the photosensitizers in the positive photoresist to react, further reducing its sensitivity to light during exposure and prolonging or even making development more difficult. Therefore, the baking temperature is preferably set to 90℃~120℃, and the baking time is set to 100S~180S.

[0044] The exposure dose for the positive photoresist is controlled at 750 mJ / cm. 2 ~1450mJ / cm 2 Within a certain range, by changing the exposure dose, the morphology of the etched pattern in the first cured adhesive layer can be freely adjusted within a certain angle range.

[0045] The positive photoresist undergoes a first hard bake using a hot plate method. The main purpose of this first hard bake is to further evaporate the organic solvents in the positive photoresist. Preferably, the temperature for the first hard bake is set to 90℃~120℃, and the baking time is set to 100S~180S.

[0046] The positive photoresist undergoes a second hard bake in an oven. The main purpose of this second hard bake is to slowly expel all the tiny air bubbles in the first layer of positive photoresist, preventing them from being expelled during the baking of the second layer of negative photoresist. This avoids the formation of tiny holes at the bottom of the second layer of negative photoresist, which could lead to defects after the isolation trench is etched, thus affecting the yield. Preferably, the temperature for the second hard bake is set to 95℃~115℃, and the baking time is set to 30min~45min.

[0047] S400. A negative photoresist is coated onto the first cured adhesive layer, and the negative photoresist layer is subjected to soft baking, exposure, hardening and development in sequence to obtain a second cured adhesive layer containing a preset etching pattern.

[0048] The negative photoresist is soft-baked using a hot plate method. The main purpose of soft baking is to allow the organic solvents in the negative photoresist to evaporate initially and to enhance its adhesion. If the organic solvents are not removed, excessively high solvent concentrations will reduce the selectivity of the developer for exposed and unexposed photoresist, resulting in incomplete removal of exposed areas during development. Furthermore, insufficient baking of the negative photoresist will not only lead to poor adhesion but also decrease the accuracy of subsequent exposures due to the high solvent content making the negative photoresist less sensitive to light. Overbaking, on the other hand, will make the negative photoresist brittle, reducing its adhesion and causing some of the photosensitizer to react, further reducing its light sensitivity during exposure and prolonging or even making development more difficult. Therefore, the baking temperature is preferably set to 100℃~120℃, and the baking time is set to 60S~120S.

[0049] The exposure dose for the negative photoresist is controlled at 300 mJ / cm. 2 ~600mJ / cm 2 Within a certain range, by changing the exposure dose, the morphology of the etched pattern in the second cured adhesive layer can be freely adjusted within a certain angle range.

[0050] Since the negative photoresist needs to be heated and react with the developer to complete the development process, a hardening process is performed on the second negative photoresist layer before development. Specifically, a hot plate baking method is used for hardening, with the baking temperature set to 100℃~120℃ and the baking time set to 60S~180S.

[0051] Because the exposure areas of the positive and negative photoresists are opposite, even if the solvent in the first layer of positive photoresist does not evaporate completely or the first layer of positive photoresist is not baked hard enough, when the second layer of negative photoresist is exposed, the unremoved areas in the first layer of positive photoresist located in the exposure area will not be exposed again, thus avoiding the morphology of the isolation trench between the grains being far from the design requirements.

[0052] S500: Using the first and second cured adhesive layers as masks, the epitaxial layer is etched.

[0053] Specifically, since a preset etching pattern is formed in the first and second cured adhesive layers at this time, ICP etching is performed on the epitaxial layer based on this pattern.

[0054] S600. In preparation for the next step of electrode fabrication, the first and second cured photoresist layers need to be removed, ultimately forming isolation trenches on the epitaxial wafer for separating multiple grains. These isolation trenches have ideal sidewall bevels and appearance. The photoresist can be removed using a wet method, a dry method, or a combination of wet and dry methods.

[0055] S700. Electrodes are prepared on the N-type and P-type mesa of each grain, and electrode bridges are prepared in the corresponding isolation trenches. The corresponding number of grains are set as a group, and the electrodes of different polarities of adjacent grains in the group are connected in series through the electrode bridges.

[0056] This application employs a double-layer photoresist structure consisting of a positive high-viscosity photoresist and a negative low-viscosity photoresist. Since the cost of the negative low-viscosity photoresist is half that of the positive high-viscosity photoresist, and the amount of negative low-viscosity photoresist used on a single substrate is also half that of the positive high-viscosity photoresist used in existing solutions, the photolithography cost of a single substrate using negative low-viscosity photoresist can be reduced by 75% compared to existing solutions. Taking GaN substrates as an example, the photolithography cost of a single substrate using this application can be reduced by approximately two yuan, as detailed in Table 1.

[0057] Table 1

[0058]

[0059] To avoid current congestion caused by the injected current concentrated directly below the P-type electrode, in some optional embodiments, a current blocking layer is epitaxially grown between the P-type semiconductor layer and the P-type electrode. Specifically, firstly, a SiO2 layer is deposited on the epitaxial wafer using PECVD technology, with nitrous oxide and silane as the working gases. The working gases are decomposed by an RF pass voltage, followed by a chemical reaction to obtain SiO2, which is then deposited on the surface of the epitaxial wafer. Then, using a CBL layer as a mask, photoresist is sequentially coated, exposed, and developed on the SiO2 layer. Finally, wet etching is performed, and the current blocking layer is obtained after etching. Optionally, a BOE solution can be used for wet etching. BOE solution is a weakly acidic solution with a main component of HF:HN4F = 4:1, which can react with silicon dioxide, thereby effectively etching the portion of SiO2 in the mask that is not protected by the photoresist.

[0060] P-type doping is challenging in some material systems, such as p-type GaN, where the carrier concentration is capped at 10-1. 18 cm -3 Therefore, when applied as a cladding layer on blue GaN-based LEDs, its resistance is relatively high, making it difficult to distribute the electrode current evenly. The current density is highest near the P-type metal electrode, resulting in uneven light emission, strong light emission near the P-type metal electrode, and light blocking by the P-type metal electrode. If a transparent conductive layer is added under the P-type metal electrode, the resistance of the transparent conductive layer is very low, and the current diffusion on the surface has almost no voltage gradient. The current can be evenly distributed in the transparent conductive layer and injected into the light-emitting layer, reducing electrode shading. Therefore, in some optional embodiments, a transparent conductive layer is epitaxially grown between the current-blocking layer and the P-type electrode. This arrangement of the transparent conductive layer achieves both low-resistance contact with the current-blocking layer and high visible light transmittance. Since the transparent conductive layer requires low resistance and transparency to visible light, ITO is an ideal material, achieving a transmittance of over 95% for visible light with very low resistance.

[0061] Specifically, when preparing the transparent conductive layer, ITO transparent conductive film is deposited using magnetron sputtering technology, and then RTA (rapid thermal annealing) annealing is performed after the film is deposited.

[0062] To protect the epitaxial layer and metal electrodes, in some optional embodiments, a passivation layer is epitaxially grown on the epitaxial layer. Specifically, a 60 nm thick SiO2 layer is deposited on the surface of the epitaxial layer using PECVD technology.

[0063] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for fabricating a high-voltage LED chip, characterized in that, Includes the following steps: A substrate is provided on which an epitaxial layer is epitaxially grown, wherein the epitaxial layer comprises at least an N-type semiconductor layer, an active layer and a P-type semiconductor layer grown sequentially. The P-type semiconductor layer is etched toward the substrate until the N-type semiconductor layer is exposed to form the N-type mesa and P-type mesa of each grain; Positive photoresist is coated onto the epitaxial layer, and the photoresist layer is subjected to soft baking, exposure, development, first hard baking, and second hard baking in sequence to obtain a first cured adhesive layer containing a preset etched pattern. A negative photoresist is coated onto the first cured adhesive layer, and the photoresist layer is subjected to soft baking, exposure, hardening and development in sequence to obtain a second cured adhesive layer containing a preset etching pattern. Using the first and second cured adhesive layers as masks, the epitaxial layer is etched. Remove the first cured adhesive layer and the second cured adhesive layer to obtain an isolation groove with a preset morphological feature on the epitaxial layer; Electrodes are fabricated on the N-type and P-type mesa of each grain, and electrode bridges are fabricated in the corresponding isolation trenches. A corresponding number of grains are set as a group, and electrodes of different polarities of adjacent grains in the group are connected in series through the electrode bridges.

2. The method for fabricating a high-voltage LED chip according to claim 1, characterized in that, The thickness of the positive photoresist coating is 8μm to 12μm.

3. The method for fabricating a high-voltage LED chip according to claim 1 or 2, characterized in that, Both the soft bake and the first hard bake of the positive photoresist were performed using a hot plate, with a baking temperature of 90℃~120℃ and a baking time of 100S~180S.

4. The method for fabricating a high-voltage LED chip according to claim 1 or 2, characterized in that, The exposure dose for positive photoresist is 750 mJ / cm. 2 ~1450mJ / cm 2 .

5. The method for fabricating a high-voltage LED chip according to claim 1 or 2, characterized in that, The positive photoresist was subjected to a second hard bake in an oven at a temperature of 95℃ to 115℃ for 30 to 45 minutes.

6. The method for fabricating a high-voltage LED chip according to claim 1 or 2, characterized in that, The thickness of the coated negative photoresist is 2.5μm to 4.5μm.

7. The method for fabricating a high-voltage LED chip according to claim 1 or 2, characterized in that, The negative photoresist is baked using a hot plate method, wherein the baking temperature is 100℃~120℃ and the baking time is 60S~120S.

8. The method for fabricating a high-voltage LED chip according to claim 1 or 2, characterized in that, The exposure dose for negative photoresist is 300 mJ / cm. 2 ~600mJ / cm 2 .

9. The method for fabricating a high-voltage LED chip according to claim 1 or 2, characterized in that, The negative photoresist is hardened by hot plate baking, wherein the baking temperature is 100℃~120℃ and the baking time is 60S~180S.

10. A high-voltage LED chip, characterized in that, The high-voltage LED chip is prepared by the high-voltage LED chip preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Manufacturing method of semiconductor chip

    CN104409583A

  • Method for manufacturing semiconductor strip, circuit board and electronic equipment having semiconductor strip, and method for dicing substrate

    JP2015029063A