A self-supporting silicon-based lithium ion battery anode material and a preparation method thereof
By encapsulating silicon particles in a double carbon shell using a Si-x@CP-y@rGO structure, a multi-dimensional conductive network is constructed, solving the capacity and volume variation problem of graphite anode materials for lithium-ion batteries. This achieves high energy density and stable electrochemical performance, making it suitable for lithium-ion battery anode materials.
Patent Information
- Application Number
- CN202410031825.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-09
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-01-09
AI Technical Summary
Existing graphite anode materials for lithium-ion batteries have low theoretical specific capacity, making it difficult to meet the demand for high energy density. They also suffer from problems such as lithium dendrite formation and ion migration orientation. Silicon-based anode materials experience large volume changes during cycling, leading to the collapse of the conductive network and failing to meet the lightweight and portable requirements of new electronic devices.
A Si-x@CP-y@rGO structure is adopted to encapsulate silicon particles in a double carbon shell. A multi-dimensional conductive network is constructed through electrospinning and carbonization technology. Combined with porous carbon fibers and reduced graphene oxide, an interwoven three-dimensional conductive pathway is formed, which alleviates volume changes and improves conductivity.
It achieves high specific capacity, excellent rate performance and cycle performance, reduces the weight of electrode materials, avoids the use of binders and conductive agents, and meets the lightweight requirements of portable electronic devices.
Smart Images

Figure CN117894941B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of lithium ion battery materials, and specifically relates to a lithium ion battery negative electrode material and a preparation method thereof. Background Art
[0002] As highly efficient green energy storage devices, lithium ion batteries have attracted increasing attention, and their applications in economy and daily life are becoming more and more widespread. However, the theoretical specific capacity of the currently commercial graphite negative electrode material for lithium ion batteries is only 372mAh g -1 , which is difficult to meet the application demands of high energy density batteries in the future. Meanwhile, lithium dendrites are easily formed during the high-current discharge process of graphite negative electrode materials, which further brings potential safety hazards to the batteries; in addition, the ion migration orientation problem caused by the layered structure of graphite limits the excellent performance of its rate characteristics. Therefore, it is extremely urgent to develop new-type high specific capacity and high rate lithium ion battery negative electrode materials to meet the demands of next-generation energy storage batteries.
[0003] Silicon-based negative electrode materials (Si, SiOx(0<x<2)) are considered as the most promising lithium ion battery negative electrode materials, which have the following characteristics: (1) Silicon element is abundant in reserves on the earth; (2) The theoretical specific capacity of silicon negative electrode materials (up to 4200mAhg -1 ), which is much higher than that of elemental negative electrode materials such as Ag, Al, Ge, Sn and Zn; (3) Its charge-discharge plateau is relatively low (<0.5V); however, the huge volume effect leads to changes in the morphology and volume of the entire silicon electrode, making the silicon materials lose contact with each other, even causing the electrode materials to gradually separate from the current collector, further leading to the collapse of the conductive network and the failure of the electrode. In addition, silicon itself also has a low electrical conductivity of only 6.7×10 -4 S cm -1 , which severely limits electron conduction during cycling, and further affects its lithium storage performance.
[0004] Traditional powder electrodes need to be combined with conductive agents, binders, current collectors and the like during use, which cannot meet the requirements of new electronic devices for light and portable energy storage equipment, and the electrode materials of powder electrodes will fall off from the current collector during long-term cycling. Compared with traditional powder electrodes, self-supporting electrodes do not require the addition of binders, and have the advantages of light weight, good conductivity and excellent performance.
[0005] Aiming at the problem of poor conductivity of silicon particles themselves, it is generally improved by simply introducing carbon materials, and few people construct a multi-dimensional conductive network through reasonable structural design. In addition, aiming at the problem of large volume change of silicon particles during cycling, the conventional single-layer coating layer has limited buffering capacity. Contents of the Invention
[0006] To overcome the shortcomings of existing technologies, this invention provides a self-supporting silicon-based lithium-ion battery anode material. The conductive network constructed by multi-dimensional conductive pathways gives the final electrode excellent conductivity. Furthermore, the construction of multiple buffer layers and reserved pores is used to maintain the volume change of the electrode during cycling, which can effectively alleviate the problems of poor inherent conductivity of silicon particles and large volume change during cycling, thus achieving better electrochemical performance.
[0007] The technical solution adopted by the present invention to solve its technical problem is: a self-supporting silicon-based lithium-ion battery anode material, comprising silicon particles Si-x@CP-y@rGO encapsulated in a double carbon shell, wherein the first carbon shell is a porous carbon fiber CP-y containing cobalt particles, and the second carbon shell is reduced graphene oxide rGO.
[0008] The present invention also provides a method for preparing the above-mentioned self-supporting silicon-based lithium-ion battery anode material, comprising the following steps:
[0009] (1) Mesoporous silica was prepared by sol-gel method; silica particles were obtained by magnesium thermoelectric reduction.
[0010] (2) Dissolve the soluble polymer and pore-forming agent in an organic solvent, then add silicon particles and cobalt nitrate hexahydrate, and disperse them evenly to obtain an electrospinning precursor solution;
[0011] (3) The spinning solution obtained in step (2) is subjected to an electrospinning process to obtain a fiber film;
[0012] (4) The fiber film obtained in step (3) is immersed in 2-methylimidazole solution and then dried.
[0013] (5) The fiber film obtained in step (4) is pre-oxidized in air and carbonized in argon to obtain Si-x@CP-y carbon fiber film;
[0014] (6) The Si-x@CP-y carbon fiber film obtained in step (5) is immersed in a mixed solution of stannous chloride and hydrochloric acid, and then taken out and dried to obtain M-Si-x@CP-y carbon fiber film.
[0015] (7) The M-Si-x@CP-y carbon fiber film obtained in step (6) is immersed in a graphene oxide solution, and then taken out and dried. The resulting Si-x@CP-y@rGO carbon fiber film can be directly used as a negative electrode material.
[0016] In step (1), the silicon particles obtained have a particle size of 100-600 nm.
[0017] In step (2), the mass fraction of soluble polymer is 8-12 wt%, the mass fraction of pore-forming agent is 8-12 wt%, the mass ratio of silicon particles to soluble polymer is 1:3-1:1, and the mass ratio of cobalt nitrate hexahydrate to soluble polymer is 1:2.
[0018] In step (2), the soluble polymer is at least one of polyacrylonitrile, polyvinylpyrrolidone, and polyvinyl alcohol; the pore-forming agent is at least one of polyvinylpyrrolidone, polymethyl methacrylate, and polylactic acid; and the organic solvent is one or a combination of two or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and acetone in any proportion.
[0019] In step (3), the positive electrode voltage of electrospinning is 12-14kV, the negative electrode voltage is -3.0-1.5kV, the receiver rotation speed is 200-400r / min, the receiving distance is 15-18cm, the syringe injection speed is 0.035-0.06mm / min, the syringe needle size is 18-20, the humidity of the spinning process is 20%-40%, and the spinning process temperature is 20℃-30℃.
[0020] In step (4), the solvent used to disperse 2-methylimidazole is at least one of water, methanol, and ethanol; the concentration of 2-methylimidazole is 0.06–0.08 mol / L. -1 .
[0021] In step (5), the pre-oxidation temperature is 220–280°C, the time is 1–4 h, and the heating rate is 1–5°C / min. -1 The carbonization temperature is 700–900℃, and the heating rate is 1–5℃ / min. -1 .
[0022] In step (6), the concentration of stannous chloride is 0.02–0.03 mol / L. -1 The concentration of hydrochloric acid is 0.05–0.15 mol / L. -1 .
[0023] In step (7), the concentration of the graphene oxide solution is 2.0–3.0 mg / mL. -1 .
[0024] The beneficial effects of this invention are as follows: Compared to traditional powder electrodes, the self-supporting thin film obtained through electrospinning, carbonization technology, and electrostatic self-assembly can be directly used as the electrode material, avoiding the introduction of inactive substances such as conductive agents and binders, which is beneficial to the improvement of the final electrochemical performance. Simultaneously, the self-supporting electrode avoids the introduction of current collector copper foil, greatly reducing the weight of the electrode material and meeting the lightweight requirements of new portable electronic devices for energy storage devices. Through reasonable structural design, a conductive structure with multi-dimensional conductive pathways is constructed, which can significantly improve the inherent poor conductivity of silicon particles. Porous carbon fibers have one-dimensional electronic pathways; highly conductive reduced graphene oxide has two-dimensional electronic pathways; the final thin film electrode has interwoven three-dimensional conductive pathways, with different dimensional conductive pathways complementing each other to jointly construct an excellent conductive network. Compared to the limitations of commonly existing single-layer coating structures in alleviating silicon particle volume changes, the double carbon shell CP-y and rGO introduced in this invention can provide stronger protection against volume changes, better improving the problem of silicon particle volume changes during cycling. Furthermore, the introduction of the void structure provides more buffer space for stress changes during cycling, further increasing the stability of the electrode structure during cycling. Furthermore, the construction of the double-layer coating structure and the porous structure significantly increases the specific surface area of the final electrode, providing numerous active sites for the electrochemical lithium storage process and facilitating efficient lithium storage. The resulting Si-x@CP-y@rGO anode material exhibits excellent rate performance, cycle performance, and initial coulombic efficiency. Moreover, the self-supporting silicon-based thin film (Si-x@CP-y@rGO) encapsulating silicon particles in a porous carbon fiber and reduced graphene oxide double carbon shell can be directly used as an anode material for lithium-ion batteries without the need for binders and conductive agents. Attached Figure Description
[0025] Figure 1 This is a schematic diagram illustrating the synthesis of the Si-2@CP-2@rGO thin film self-supporting electrode prepared in Example 1 of the present invention;
[0026] Figure 2 SEM image of the silicon particles prepared in Comparative Example 1 of this invention;
[0027] Figure 3 This is a SEM image of the Si-1@CP-2 thin film, a lithium-ion battery anode material prepared in Comparative Example 2 of this invention.
[0028] Figure 4 SEM image (a), TEM image (b) and EDS mapping image (c) of the Si-2@CP-2 thin film, a lithium-ion battery anode material prepared in Comparative Example 3 of this invention;
[0029] Figure 5This is a SEM image of the Si-3@CP-2 thin film, the lithium-ion battery anode material prepared in Comparative Example 4 of this invention.
[0030] Figure 6 This is a SEM image of the Si-4@CP-2 thin film, the lithium-ion battery anode material prepared in Comparative Example 5 of this invention.
[0031] Figure 7 This is a SEM image of the Si-2@CP-1 thin film, a lithium-ion battery anode material prepared in Comparative Example 6 of this invention.
[0032] Figure 8 This is a SEM image of the Si-2@CP-3 thin film, a lithium-ion battery anode material prepared in Comparative Example 7 of this invention.
[0033] Figure 9 SEM image (a), TEM image (b) and EDS mapping image (c) of the self-supporting electrode of the Si-2@CP-2@rGO thin film, which is the lithium-ion battery anode material prepared in Example 1 of the present invention;
[0034] Figure 10 The images show the XRD patterns of the lithium-ion battery anode materials prepared in Comparative Examples 2-5 and Example 1 of this invention.
[0035] Figure 11 XPS image of the lithium-ion battery anode material prepared in Example 1 of this invention;
[0036] Figure 12 The nitrogen adsorption-desorption curves are shown for the lithium-ion battery anode materials prepared in Comparative Examples 2-7 and Example 1 of this invention.
[0037] Figure 13 Cyclic voltammetry curves of the Si-2@CP-2@rGO thin film, a lithium-ion battery anode material prepared in Example 1 of this invention;
[0038] Figure 14 The Si-2@CP-2@rGO thin film, a lithium-ion battery anode material prepared in Example 1 of this invention, was subjected to a 100 mAg test. -1 Charge-discharge curves at current density;
[0039] Figure 15 The first coulombic efficiency of the lithium-ion battery anode materials prepared in Comparative Examples 1, 3 and 1 of this invention;
[0040] Figure 16 The lithium-ion battery anode materials prepared for Comparative Examples 1-7 and Example 1 of this invention were subjected to a 50 mA g⁻¹ test. -1 100mAg -1 200mA g -1 500mA g-1 1000mA g -1 2000mA g -1 and 100mA g -1 Rate performance at current density;
[0041] Figure 17 The lithium-ion battery anode materials prepared for Comparative Examples 1-7 and Example 1 of this invention were tested at 100 mA g. -1 Cyclic performance at current density;
[0042] Figure 18 The lithium-ion battery anode materials prepared for Comparative Example 3 and Example 1 of this invention were subjected to a test at 1000 mA g. -1 Cyclic performance at current density;
[0043] Figure 19 The images show the electrochemical impedance spectroscopy of the lithium-ion battery anode materials prepared in Comparative Examples 1, 3 and 1 of this invention. Detailed Implementation
[0044] The present invention will be further described below with reference to the accompanying drawings, comparative examples and embodiments. The present invention includes, but is not limited to, the following embodiments.
[0045] This invention provides a self-supporting silicon-based lithium-ion battery anode material, comprising silicon particles Si-x@CP-y@rGO encapsulated in a double carbon shell. The first carbon shell is a porous carbon fiber CP-y containing cobalt particles, and the second carbon shell is reduced graphene oxide (rGO). The resulting Si-x@CP-y@rGO thin-film electrode exhibits excellent conductivity due to a conductive network constructed from multi-dimensional conductive pathways. Furthermore, the construction of multiple buffer layers and reserved pores helps maintain the volume change of the electrode during cycling.
[0046] The present invention also provides a method for preparing the above-mentioned self-supporting silicon-based lithium-ion battery anode material, comprising the following steps:
[0047] (1) Mesoporous silica was prepared by sol-gel method; silicon particles were obtained by magnesium thermoelectric reduction.
[0048] (2) Dissolve the soluble polymer and pore-forming agent in an organic solvent, then add silicon particles and cobalt nitrate hexahydrate, and disperse them evenly to obtain an electrospinning precursor solution;
[0049] (3) The spinning solution obtained in step (2) is subjected to an electrospinning process to obtain a fiber film;
[0050] (4) The fiber film obtained in step (3) is immersed in 2-methylimidazole solution and then dried.
[0051] (5) The fiber film obtained in step (4) is pre-oxidized in air and carbonized in argon to obtain Si-x@CP-y carbon fiber film;
[0052] (6) The Si-x@CP-y carbon fiber film obtained in step (5) is immersed in a mixed solution of stannous chloride and hydrochloric acid, and then dried to obtain M-Si-x@CP-y carbon fiber film.
[0053] (7) The M-Si-x@CP-y carbon fiber film obtained in step (6) is immersed in a graphene oxide solution and then dried. The resulting Si-x@CP-y@rGO carbon fiber film can be directly used as a negative electrode material.
[0054] Furthermore, the silicon particles in step (1) have a particle size of 100–600 nm. If the silicon particles are too large, they cannot be well coated by the cobalt-containing porous carbon fibers; if the silicon particles are too small, severe agglomeration will occur.
[0055] Furthermore, in step (2), the mass fraction of the soluble polymer is 8-12 wt%, the mass fraction of the pore-forming agent is 8-12 wt%, the mass ratio of silicon particles to soluble polymer is 1:3-1:1, and the mass ratio of cobalt nitrate hexahydrate to soluble polymer is 1:2.
[0056] Furthermore, in step (2), the soluble polymer is at least one of polyacrylonitrile, polyvinylpyrrolidone, and polyvinyl alcohol; the pore-forming agent is at least one of polyvinylpyrrolidone, polymethyl methacrylate, and polylactic acid; and the organic solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and acetone in any proportion.
[0057] Furthermore, in step (3), the positive electrode voltage of electrospinning is 12-14 kV, the negative electrode voltage is -3.0--1.5 kV, the receiver rotation speed is 200-400 r / min, the receiving distance is 15-18 cm, the syringe injection speed is 0.035-0.06 mm / min, and the syringe needle size is 18-20. The humidity during the spinning process is 20%-40%, and the temperature during the spinning process is 20℃-30℃. Poor control of voltage, distance, and syringe injection speed can lead to fibers that are too coarse, too fine, or beaded, resulting in an inability to obtain uniform fibers. Suitable humidity and temperature are conducive to the evaporation of organic solvents, resulting in fibers with uniform morphology.
[0058] Furthermore, the solvent used to disperse 2-methylimidazole in step (4) includes at least one of water, methanol, and ethanol.
[0059] Furthermore, in step (4), the concentration of 2-methylimidazole is 0.06–0.08 mol / L. -1 Both excessively high and excessively low concentrations are not conducive to obtaining porous carbon fibers containing ultra-small cobalt particles.
[0060] Furthermore, in step (5), the pre-oxidation temperature in the air is 220–280°C, the time is 1–4 h, and the heating rate is 1–5°C / min. -1 Too low a pre-oxidation temperature, too short a time, or too rapid a heating rate will all result in incomplete pre-oxidation. Too high a pre-oxidation temperature will lead to fiber decomposition.
[0061] Furthermore, in step (5), the carbonization temperature under argon gas is 700–900℃, and the heating rate is 1–5℃ / min. -1 Too low a pre-oxidation temperature, too short a time, or too rapid a heating rate will all result in incomplete carbonization. Too high a carbonization temperature will reduce the strength of the fiber, thereby affecting its electrochemical performance.
[0062] Furthermore, the concentration of stannous chloride in step (6) is 0.02–0.03 mol / L. -1 The concentration of hydrochloric acid is 0.05–0.15 mol / L. -1 Excessive or insufficient concentrations of stannous chloride and hydrochloric acid can affect the modification effect on carbon fibers.
[0063] Furthermore, in step (7), the concentration of the graphene oxide solution is 2.0–3.0 mg / mL. -1 Too low a concentration results in insufficient coating of reduced graphene oxide, failing to adequately address the poor conductivity of silicon particles and their large volume changes during cycling. Conversely, excessive coating leads to an overly high carbon content in the final film, hindering the improvement of final electrochemical performance.
[0064] A self-supporting silicon-based thin film (Si-x@CP-y@rGO) containing cobalt particles and a porous carbon fiber and reduced graphene oxide double carbon shell encapsulating silicon particles was prepared by the above method.
[0065] The above-mentioned cobalt-containing porous carbon fiber and reduced graphene oxide double carbon shell encapsulating silicon particles (Si-x@CP-y@rGO) are used as a negative electrode material for lithium-ion batteries.
[0066] Furthermore, a self-supporting silicon-based thin film (Si-x@CP-y@rGO) containing cobalt particles, with porous carbon fibers and reduced graphene oxide double carbon shells encapsulating silicon particles, can be directly used as a negative electrode material for lithium-ion batteries without the need to introduce binders and conductive agents.
[0067] Comparative Example 1
[0068] 3.0 g of hexadecyltrimethylammonium bromide was dissolved in a mixture of 200 mL ethanol and 100 mL deionized water, then 4 mL of tetraethyl orthosilicate and 2 mL of ammonia were added, and the mixture was stirred at 35 °C for 24 h. Silica particles were obtained by centrifugation, and the sample was then immersed in deionized water at 90 °C for a period of time before filtration and drying. Finally, the collected silica particles were calcined at 550 °C for 3 h to remove residual hexadecyltrimethylammonium bromide. Silica particles, magnesium powder, and sodium chloride (1:1:2) were mixed and calcined at 3 °C for 3 min. -1 The rate was maintained at 650℃ for 6 hours. Subsequently, the magnesium thermal reduction product was processed in 2 mol L... -1 The product was soaked in hydrochloric acid for 6 hours to remove impurities. Finally, the resulting product was placed in a vacuum drying oven at 60°C overnight to obtain silicon particles.
[0069] The silicon particles obtained in this embodiment were mixed with PVDF and acetylene black in a ratio of 7:1:2 and dispersed in N-methylpyrrolidone. After stirring evenly, the mixture was coated onto copper foil. After drying, it was cut into circular electrodes with a diameter of 0.8 cm. Using lithium metal as the counter electrode, the electrodes were assembled into CR2016 button batteries in a glove box and subjected to electrochemical performance testing.
[0070] Comparative Example 2
[0071] 3.0 g of hexadecyltrimethylammonium bromide was dissolved in a mixture of 200 mL ethanol and 100 mL deionized water, then 4 mL of tetraethyl orthosilicate and 2 mL of ammonia were added, and the mixture was stirred at 35 °C for 24 h. Silica particles were obtained by centrifugation, and the sample was then immersed in deionized water at 90 °C for a period of time before filtration and drying. Finally, the collected silica particles were calcined at 550 °C for 3 h to remove residual hexadecyltrimethylammonium bromide. Silica particles, magnesium powder, and sodium chloride (1:1:2) were mixed and calcined at 3 °C for 3 min. -1 The rate was maintained at 650℃ for 6 hours. Subsequently, the magnesium thermal reduction product was processed in 2 mol L... -1 The product was soaked in hydrochloric acid for 6 hours to remove impurities. Finally, the resulting product was placed in a vacuum drying oven at 60°C overnight to obtain silicon particles.
[0072] 0.1 g of silicon particles were uniformly dispersed in a 9 wt% polyacrylonitrile solution by ultrasonic stirring. Subsequently, 0.3 g of cobalt nitrate hexahydrate and 0.15 g of polyvinylpyrrolidone were added to obtain the final electrospinning precursor solution. The positive and negative electrode voltages during the electrospinning process were 13.0 and -2.0 kV, respectively, the receiving distance was 18 cm, and the injection speed was 0.06 mm / min. -1After the electrospinning process is complete, the yellowish-brown film is removed from the receiver and dried overnight in an oven at 60°C. The film is then immersed in 0.07 mol / L... -1 The film was immersed in a 2-methylimidazole solution for 6 hours, during which time the yellowish-brown film gradually turned into a purple film. The purple film was then further incubated in air at 260°C for 2 hours, with a heating rate of 3°C / min. -1 Subsequently, under argon atmosphere, the temperature was maintained at 800℃ for 3 hours, with a heating rate of 3℃ / min. -1 A thin film of silicon particles wrapped with porous carbon fibers containing cobalt particles was obtained, denoted as Si-1@CP-2.
[0073] The porous carbon fiber-encapsulated silicon particle film Si-1@CP-2 containing cobalt particles obtained in this embodiment was directly used as the electrode material, cut into circular electrodes with a diameter of 0.8 cm, and lithium metal was used as the counter electrode. The cells were assembled into CR2016 button cells in a glove box and their electrochemical performance was tested.
[0074] Comparative Example 3
[0075] 3.0 g of hexadecyltrimethylammonium bromide was dissolved in a mixture of 200 mL ethanol and 100 mL deionized water, then 4 mL of tetraethyl orthosilicate and 2 mL of ammonia were added, and the mixture was stirred at 35 °C for 24 h. Silica particles were obtained by centrifugation, and the sample was then immersed in deionized water at 90 °C for a period of time before filtration and drying. Finally, the collected silica particles were calcined at 550 °C for 3 h to remove residual hexadecyltrimethylammonium bromide. Silica particles, magnesium powder, and sodium chloride (1:1:2) were mixed and calcined at 3 °C for 3 min. -1 The rate was maintained at 650℃ for 6 hours. Subsequently, the magnesium thermal reduction product was processed in 2 mol L... -1 The product was soaked in hydrochloric acid for 6 hours to remove impurities. Finally, the resulting product was placed in a vacuum drying oven at 60°C overnight to obtain silicon particles.
[0076] 0.2 g of silicon particles were uniformly dispersed in a 9 wt% polyacrylonitrile solution by ultrasonic stirring. Subsequently, 0.3 g of cobalt nitrate hexahydrate and 0.15 g of polyvinylpyrrolidone were added to obtain the final electrospinning precursor solution. The positive and negative electrode voltages during the electrospinning process were 13.0 and -2.0 kV, respectively, the receiving distance was 18 cm, and the injection speed was 0.06 mm / min. -1 After the electrospinning process is complete, the yellowish-brown film is removed from the receiver and dried overnight in an oven at 60°C. The film is then immersed in 0.07 mol / L... -1 The film was immersed in a 2-methylimidazole solution for 6 hours, during which time the yellowish-brown film gradually turned into a purple film. The purple film was then further incubated in air at 260°C for 2 hours, with a heating rate of 3°C / min. -1Subsequently, under argon atmosphere, the temperature was maintained at 800℃ for 3 hours, with a heating rate of 3℃ / min. -1 A thin film of silicon particles wrapped with porous carbon fibers containing cobalt particles was obtained, denoted as Si-2@CP-2.
[0077] The porous carbon fiber-encapsulated silicon particle film Si-2@CP-2 containing cobalt particles obtained in this embodiment was directly used as the electrode material, cut into circular electrodes with a diameter of 0.8 cm, and lithium metal was used as the counter electrode. The cells were assembled into CR2016 button cells in a glove box and their electrochemical performance was tested.
[0078] Comparative Example 4
[0079] 3.0 g of hexadecyltrimethylammonium bromide was dissolved in a mixture of 200 mL ethanol and 100 mL deionized water, then 4 mL of tetraethyl orthosilicate and 2 mL of ammonia were added, and the mixture was stirred at 35 °C for 24 h. Silica particles were obtained by centrifugation, and the sample was then immersed in deionized water at 90 °C for a period of time before filtration and drying. Finally, the collected silica particles were calcined at 550 °C for 3 h to remove residual hexadecyltrimethylammonium bromide. Silica particles, magnesium powder, and sodium chloride (1:1:2) were mixed and calcined at 3 °C for 3 min. -1 The rate was maintained at 650℃ for 6 hours. Subsequently, the magnesium thermal reduction product was processed in 2 mol L... -1 The product was soaked in hydrochloric acid for 6 hours to remove impurities. Finally, the resulting product was placed in a vacuum drying oven at 60°C overnight to obtain silicon particles.
[0080] 0.3 g of silicon particles were uniformly dispersed in a 9 wt% polyacrylonitrile solution by ultrasonic stirring. Subsequently, 0.3 g of cobalt nitrate hexahydrate and 0.15 g of polyvinylpyrrolidone were added to obtain the final electrospinning precursor solution. The positive and negative electrode voltages during the electrospinning process were 13.0 and -2.0 kV, respectively, the receiving distance was 18 cm, and the injection speed was 0.06 mm / min. -1 After the electrospinning process is complete, the yellowish-brown film is removed from the receiver and dried overnight in an oven at 60°C. The film is then immersed in 0.07 mol / L... -1 The film was immersed in a 2-methylimidazole solution for 6 hours, during which time the yellowish-brown film gradually turned into a purple film. The purple film was then further incubated in air at 260°C for 2 hours, with a heating rate of 3°C / min. -1 Subsequently, under argon atmosphere, the temperature was maintained at 800℃ for 3 hours, with a heating rate of 3℃ / min. -1 A thin film of silicon particles wrapped with porous carbon fibers containing cobalt particles was obtained, denoted as Si-3@CP-2.
[0081] The porous carbon fiber-encapsulated silicon particle film Si-3@CP-2 containing cobalt particles obtained in this embodiment was directly used as the electrode material, cut into circular electrodes with a diameter of 0.8 cm, and lithium metal was used as the counter electrode. The cells were assembled into CR2016 button cells in a glove box and their electrochemical performance was tested.
[0082] Comparative Example 5
[0083] 3.0 g of hexadecyltrimethylammonium bromide was dissolved in a mixture of 200 mL ethanol and 100 mL deionized water, then 4 mL of tetraethyl orthosilicate and 2 mL of ammonia were added, and the mixture was stirred at 35 °C for 24 h. Silica particles were obtained by centrifugation, and the sample was then immersed in deionized water at 90 °C for a period of time before filtration and drying. Finally, the collected silica particles were calcined at 550 °C for 3 h to remove residual hexadecyltrimethylammonium bromide. Silica particles, magnesium powder, and sodium chloride (1:1:2) were mixed and calcined at 3 °C for 3 min. -1 The rate was maintained at 650℃ for 6 hours. Subsequently, the magnesium thermal reduction product was processed in 2 mol L... -1 The product was soaked in hydrochloric acid for 6 hours to remove impurities. Finally, the resulting product was placed in a vacuum drying oven at 60°C overnight to obtain silicon particles.
[0084] 0.5 g of silicon particles were uniformly dispersed in a 9 wt% polyacrylonitrile solution by ultrasonic stirring. Subsequently, 0.3 g of cobalt nitrate hexahydrate and 0.15 g of polyvinylpyrrolidone were added to obtain the final electrospinning precursor solution. The positive and negative electrode voltages during the electrospinning process were 13.0 and -2.0 kV, respectively, the receiving distance was 18 cm, and the injection speed was 0.06 mm / min. -1 After the electrospinning process is complete, the yellowish-brown film is removed from the receiver and dried overnight in an oven at 60°C. The film is then immersed in 0.07 mol / L... -1 The film was immersed in a 2-methylimidazole solution for 6 hours, during which time the yellowish-brown film gradually turned into a purple film. The purple film was then further incubated in air at 260°C for 2 hours, with a heating rate of 3°C / min. -1 Subsequently, under argon atmosphere, the temperature was maintained at 800℃ for 3 hours, with a heating rate of 3℃ / min. -1 A thin film of silicon particles wrapped with porous carbon fibers containing cobalt particles was obtained, denoted as Si-4@CP-2.
[0085] The porous carbon fiber-encapsulated silicon particle film Si-4@CP-2 containing cobalt particles obtained in this embodiment was directly used as the electrode material, cut into circular electrodes with a diameter of 0.8 cm, and lithium metal was used as the counter electrode. The cells were assembled into CR2016 button cells in a glove box and their electrochemical performance was tested.
[0086] Comparative Example 6
[0087] 3.0 g of hexadecyltrimethylammonium bromide was dissolved in a mixture of 200 mL ethanol and 100 mL deionized water, then 4 mL of tetraethyl orthosilicate and 2 mL of ammonia were added, and the mixture was stirred at 35 °C for 24 h. Silica particles were obtained by centrifugation, and the sample was then immersed in deionized water at 90 °C for a period of time before filtration and drying. Finally, the collected silica particles were calcined at 550 °C for 3 h to remove residual hexadecyltrimethylammonium bromide. Silica particles, magnesium powder, and sodium chloride (1:1:2) were mixed and calcined at 3 °C for 3 min. -1 The rate was maintained at 650℃ for 6 hours. Subsequently, the magnesium thermal reduction product was processed in 2 mol L... -1 The product was soaked in hydrochloric acid for 6 hours to remove impurities. Finally, the resulting product was placed in a vacuum drying oven at 60°C overnight to obtain silicon particles.
[0088] 0.2 g of silicon particles were uniformly dispersed in a 9 wt% polyacrylonitrile solution by ultrasonic stirring. Subsequently, 0.3 g of cobalt nitrate hexahydrate and 0.07 g of polyvinylpyrrolidone were added to obtain the final electrospinning precursor solution. The positive and negative electrode voltages during the electrospinning process were 13.0 and -2.0 kV, respectively, the receiving distance was 18 cm, and the injection speed was 0.06 mm / min. -1 After the electrospinning process is complete, the yellowish-brown film is removed from the receiver and dried overnight in an oven at 60°C. The film is then immersed in 0.07 mol / L... -1 The film was immersed in a 2-methylimidazole solution for 6 hours, during which time the yellowish-brown film gradually turned into a purple film. The purple film was then further incubated in air at 260°C for 2 hours, with a heating rate of 3°C / min. -1 Subsequently, under argon atmosphere, the temperature was maintained at 800℃ for 3 hours, with a heating rate of 3℃ / min. -1 A thin film of silicon particles wrapped with porous carbon fibers containing cobalt particles was obtained, denoted as Si-2@CP-1.
[0089] The porous carbon fiber-encapsulated silicon particle film Si-2@CP-1 containing cobalt particles obtained in this embodiment was directly used as the electrode material, cut into circular electrodes with a diameter of 0.8 cm, and lithium metal was used as the counter electrode. The cells were assembled into CR2016 button cells in a glove box and their electrochemical performance was tested.
[0090] Comparative Example 7
[0091] 3.0 g of hexadecyltrimethylammonium bromide was dissolved in a mixture of 200 mL ethanol and 100 mL deionized water, then 4 mL of tetraethyl orthosilicate and 2 mL of ammonia were added, and the mixture was stirred at 35 °C for 24 h. Silica particles were obtained by centrifugation, and the sample was then immersed in deionized water at 90 °C for a period of time before filtration and drying. Finally, the collected silica particles were calcined at 550 °C for 3 h to remove residual hexadecyltrimethylammonium bromide. Silica particles, magnesium powder, and sodium chloride (1:1:2) were mixed and calcined at 3 °C for 3 min. -1 The rate was maintained at 650℃ for 6 hours. Subsequently, the magnesium thermal reduction product was processed in 2 mol L... -1 The product was soaked in hydrochloric acid for 6 hours to remove impurities. Finally, the resulting product was placed in a vacuum drying oven at 60°C overnight to obtain silicon particles.
[0092] 0.2 g of silicon particles were uniformly dispersed in a 9 wt% polyacrylonitrile solution by ultrasonic stirring. Subsequently, 0.3 g of cobalt nitrate hexahydrate and 0.3 g of polyvinylpyrrolidone were added to obtain the final electrospinning precursor solution. The positive and negative electrode voltages during the electrospinning process were 13.0 and -2.0 kV, respectively, the receiving distance was 18 cm, and the injection speed was 0.06 mm / min. -1 After the electrospinning process is complete, the yellowish-brown film is removed from the receiver and dried overnight in an oven at 60°C. The film is then immersed in 0.07 mol / L... -1 The film was immersed in a 2-methylimidazole solution for 6 hours, during which time the yellowish-brown film gradually turned into a purple film. The purple film was then further incubated in air at 260°C for 2 hours, with a heating rate of 3°C / min. -1 Subsequently, under argon atmosphere, the temperature was maintained at 800℃ for 3 hours with a heating rate of 3℃ / min to obtain a porous carbon fiber-encapsulated silicon particle film containing cobalt particles, denoted as Si-2@CP-3.
[0093] The porous carbon fiber-encapsulated silicon particle film Si-2@CP-3 containing cobalt particles obtained in this embodiment was directly used as the electrode material, cut into circular electrodes with a diameter of 0.8 cm, and lithium metal was used as the counter electrode. The cells were assembled into CR2016 button cells in a glove box and their electrochemical performance was tested.
[0094] Compared to all other comparative examples, Comparative Example 3 has the best performance in all aspects. Based on this, we obtained the final Example 1.
[0095] Example 1
[0096] 3.0 g of hexadecyltrimethylammonium bromide was dissolved in a mixture of 200 mL ethanol and 100 mL deionized water, then 4 mL of tetraethyl orthosilicate and 2 mL of ammonia were added, and the mixture was stirred at 35 °C for 24 h. Silica particles were obtained by centrifugation, and the sample was then immersed in deionized water at 90 °C for a period of time before filtration and drying. Finally, the collected silica particles were calcined at 550 °C for 3 h to remove residual hexadecyltrimethylammonium bromide. Silica particles, magnesium powder, and sodium chloride (1:1:2) were mixed and calcined at 3 °C for 3 min. -1 The rate was maintained at 650℃ for 6 hours. Subsequently, the magnesium thermal reduction product was processed in 2 mol L... -1 The product was soaked in hydrochloric acid for 6 hours to remove impurities. Finally, the resulting product was placed in a vacuum drying oven at 60°C overnight to obtain silicon particles.
[0097] 0.2 g of silicon particles were uniformly dispersed in a 9 wt% polyacrylonitrile solution by ultrasonic stirring. Subsequently, 0.3 g of cobalt nitrate hexahydrate and 0.15 g of polyvinylpyrrolidone were added to obtain the final electrospinning precursor solution. The positive and negative electrode voltages during the electrospinning process were 13.0 and -2.0 kV, respectively, the receiving distance was 18 cm, and the injection speed was 0.06 mm / min. -1 After the electrospinning process is complete, the yellowish-brown film is removed from the receiver and dried overnight in an oven at 60°C. The film is then immersed in 0.07 mol / L... -1 The film was incubated in a 2-methylimidazole solution for 6 hours, during which time the yellowish-brown film gradually turned into a purple film. The purple film was then incubated in air at 260°C for 2 hours at a heating rate of 3°C / min. Subsequently, it was incubated in argon at 800°C for 3 hours at a heating rate of 3°C / min. -1 A porous carbon fiber-coated silicon particle film containing cobalt particles was obtained. The cobalt-containing porous carbon fiber-coated silicon particle film was then immersed in 0.026 mol / L... -1 Stannous chloride and 0.1 mol L -1 A mixed solution of acids was used to adhere tin ions to the surface of the film, thus giving the entire film a positive charge. The film was then placed in an oven at 60°C for 3 hours. Subsequently, it was placed in an oven with 2.5 mg / mL... -1 The silicon particles were immersed in a GO solution for 5 minutes and then dried for 3 hours. This impregnation process was repeated three times to obtain a thin film containing cobalt particles, porous carbon fibers, and reduced graphene oxide double carbon shells encapsulating silicon particles, denoted as Si-2@CP-2@rGO.
[0098] The porous carbon fiber containing cobalt particles and the thin film Si-2@CP-2@rGO wrapped with silicon particles in the double carbon shell of reduced graphene oxide obtained in this embodiment were directly used as electrode materials, cut into circular electrodes with a diameter of 0.8 cm, and lithium metal was used as the counter electrode. They were assembled into CR2016 button batteries in a glove box and electrochemical performance was tested.
[0099] Performance testing:
[0100] The materials prepared in the above embodiments were analyzed for their composition and morphology using X-ray diffraction (XRD), X-ray photoelectron spectroscopy (XPS), scanning electron microscopy (SEM), and transmission electron microscopy (TEM).
[0101] The CR2016 button cell assembled in the above embodiment was left to stand for 6 hours, and then tested using a LAND battery testing system (LANDCT200IA) at a current density of 50 mA g. -1 ~2000mA g -1 Under these conditions, its rate performance and cycle performance were tested by constant current charge-discharge, with a test voltage range of 0.1V to 0.3V and a test temperature of 25℃. Cyclic voltammetry and AC impedance spectroscopy were performed using an electrochemical workstation (Autolab, PGSTAT302 N).
Claims
1. A method for preparing a self-supporting silicon-based lithium-ion battery anode material, characterized in that, Includes the following steps: (1) Mesoporous silica was prepared by sol-gel method; silica particles were obtained by magnesium thermoelectric reduction; (2) Dissolve the soluble polymer and pore-forming agent in an organic solvent, then add silicon particles and cobalt nitrate hexahydrate, and disperse them evenly to obtain an electrospinning precursor solution; The soluble polymer is polyacrylonitrile; the pore-forming agent is polyvinylpyrrolidone. (3) The spinning solution obtained in step (2) is subjected to an electrospinning process to obtain a fiber film; (4) The fiber film obtained in step (3) is immersed in a 2-methylimidazole solution and then dried. (5) The fiber film obtained in step (4) is pre-oxidized in air and carbonized in argon to obtain Si-x@CP-y carbon fiber film; x represents the amount of Si particles added, and y represents the amount of pore-forming agent PVP added. Adding 0.1g of Si particles and 0.15g of PVP particles yields Si-1@CP-2; adding 0.2g of Si particles and 0.15g of PVP particles yields Si-2@CP-2; adding 0.3g of Si particles and 0.15g of PVP particles yields Si-3@CP-2; adding 0.5g of Si particles and 0.15g of PVP particles yields Si-4@CP-2; adding 0.2g of Si particles and 0.07g of PVP particles yields Si-2@CP-1; and adding 0.2g of Si particles and 0.3g of PVP particles yields Si-2@CP-3. (6) The Si-x@CP-y carbon fiber film obtained in step (5) is immersed in a mixed solution of stannous chloride and hydrochloric acid, and then taken out and dried to obtain M-Si-x@CP-y carbon fiber film. (7) The M-Si-x@CP-y carbon fiber film obtained in step (6) is immersed in graphene oxide solution, and then taken out and dried. The resulting Si-x@CP-y@rGO carbon fiber film can be directly used as a negative electrode material.
2. The method for preparing the self-supporting silicon-based lithium-ion battery anode material according to claim 1, characterized in that, In step (1), the silicon particles obtained have a particle size of 100~600 nm.
3. The method for preparing the self-supporting silicon-based lithium-ion battery anode material according to claim 1, characterized in that, In step (2), the mass fraction of soluble polymer is 8-12 wt%, the mass fraction of pore-forming agent is 8-12 wt%, the mass ratio of silicon particles to soluble polymer is 1:3-1:1, and the mass ratio of cobalt nitrate hexahydrate to soluble polymer is 1:
2.
4. The method for preparing the self-supporting silicon-based lithium-ion battery anode material according to claim 1, characterized in that, In step (2), the organic solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and acetone in any proportion.
5. The method for preparing the self-supporting silicon-based lithium-ion battery anode material according to claim 1, characterized in that, In step (3), the positive electrode voltage of electrospinning is 12~14 kV, the negative electrode voltage is -3.0~-1.5 kV, the receiver rotation speed is 200~400 r / min, the receiving distance is 15~18 cm, the syringe injection speed is 0.035~0.06 mm / min, the syringe needle size is 18-20, the humidity of the spinning process is 20%~40%, and the spinning process temperature is 20℃~30℃.
6. The method for preparing the self-supporting silicon-based lithium-ion battery anode material according to claim 1, characterized in that, In step (4), the solvent used to disperse 2-methylimidazole is at least one of water, methanol, and ethanol; the concentration of 2-methylimidazole is 0.06~0.08 mol / L. -1 .
7. The method for preparing the self-supporting silicon-based lithium-ion battery anode material according to claim 1, characterized in that, In step (5), the pre-oxidation temperature is 220~280℃, the time is 1~4 h, and the heating rate is 1~5℃ min. -1 The carbonization temperature is 700~900℃, and the heating rate is 1~5℃ / min. -1 .
8. The method for preparing the self-supporting silicon-based lithium-ion battery anode material according to claim 1, characterized in that, In step (6), the concentration of stannous chloride is 0.02~0.03 mol L. -1 The concentration of hydrochloric acid is 0.05~0.15 mol L. -1 .