A laser fusion additive manufacturing pre-internal defect test piece and a preparation method thereof

By using hydrogels and ceramic clay to prepare pre-fabricated internal defects, combined with laser melting additive manufacturing and industrial CT inspection, the problem of simulating and evaluating internal void defects in laser melting additive manufacturing, which is difficult in existing technologies, is solved, thus improving the accuracy of test pieces and the reliability of mechanical property evaluation.

CN117900507BActive Publication Date: 2026-11-24BEIJING AERONAUTIC SCI & TECH RES INST OF COMAC +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410013672.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-04
Publication Date
2026-11-24
Estimated Expiration
2044-01-04

AI Technical Summary

Technical Problem

Existing technologies cannot accurately simulate and prefabricate internal void defects in laser melting additive manufacturing, which affects the evaluation of the mechanical properties of structural components and the formulation of acceptance standards.

Method used

Pre-fabricated internal defects are prepared using hydrogel and ceramic clay. Pre-fabricated defects are introduced during the laying of metal powder using laser melting additive manufacturing. Thin-walled defect blanks are formed by low-temperature freezing and high-temperature drying. Industrial CT inspection is then used to ensure that the location and size of the defects meet the requirements.

Benefits of technology

It enables accurate simulation of internal void defects in additive manufacturing, reduces the impact on the mechanical properties of test pieces, and improves the accuracy of defect assessment and the basis for the formulation of acceptance criteria.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117900507B_ABST
    Figure CN117900507B_ABST
Patent Text Reader

Abstract

This invention relates to a laser melting additive manufacturing method for producing a pre-fabricated internal defect test piece. The method includes the following steps: preparing a pre-fabricated internal defect; preparing a metal powder raw material; uniformly spreading the metal powder raw material on a laser melting bed, placing the pre-fabricated internal defect at a predetermined position during spreading; melting the uniformly spread metal powder raw material and the pre-fabricated internal defect piece using a laser; fixing the treated product into a molded shape; inspecting the molded product, and if it passes inspection, obtaining the pre-fabricated internal defect test piece. This invention introduces ultra-thin ceramic defects, which can relatively accurately simulate the shape and size of internal voids generated in additive manufacturing; the pre-fabricated defect is placed in a powder metal matrix, which can simulate void defects or inclusions at any location.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of additive manufacturing technology, specifically relating to a laser melting additive manufacturing method for producing prefabricated internal defect test specimens. Background Technology

[0002] Metal additive manufacturing technology has greatly liberated the constraints of metal processing, broadened the creative freedom of designers, shortened the design process, and formed an efficient product realization capability integrating design, optimization, and manufacturing. Combined with force flow topology optimization methods, high-performance, complex, and lightweight metal additive manufacturing structures have been widely applied in industrial fields such as aerospace, medical devices, and automotive manufacturing. Metal additive manufacturing technologies can be broadly classified into two categories: powder bed fusion and direct energy deposition (DED). The former mainly includes laser selective melting and electron beam selective melting; the latter mainly includes laser near-net-shape forming and wire-fed laser additive manufacturing. DED additive manufacturing is not affected by the forming dimensions, but the forming accuracy and surface quality are relatively poor, requiring secondary processing. Powder bed fusion additive manufacturing has high precision and surface quality and is currently the mainstream additive manufacturing technology. However, products manufactured using this process still have internal void defects, such as porosity, inclusions, and missed defects, due to equipment, operation, and environmental factors.

[0003] Voids are an unavoidable defect in laser melting because it's difficult to achieve 100% density in localized metal melting. Voids typically fall into two categories: round holes (pores) and irregularly shaped holes (bonding defects). Pores are a common defect in additive manufacturing. During the melting process, the molten pool dissolves some gas; if this gas doesn't escape quickly enough during solidification, pores form inside the product. Bonding defects result from insufficient melting of the raw material, leading to reduced fluidity and poor coverage. Void sizes range from 50 μm to several millimeters, and as crack initiation points in structural components, they often significantly reduce the fatigue life of these components during use. Therefore, studying the impact of void structural characteristics on the mechanical properties of laser additive manufactured components has been a hot topic in engineering and academic research. Meanwhile, the process has been continuously focused on controlling and improving void defects, whose occurrence is random. Whether the final product meets design requirements requires mechanical property testing combined with an industrial CT system for evaluation. Acceptance standards need to be standardized.

[0004] In order to qualitatively and quantitatively assess the impact of these component defects on product performance, study the relationship between defect characteristics and distribution and mechanical properties, and formulate acceptance criteria, it is necessary to prefabricate internal defects during the additive manufacturing process.

[0005] Currently, the common method is to pre-fabricate typical defects of different types and sizes by setting parameters of the digital model during the printing process. Because the appearance of voids is random, and their shape and size are uncontrollable during liquid metal forming, pre-fabricating internal defects is always unpredictable. Existing controllable pre-fabrication defect technologies include: 1. Introducing solid inclusions into the preparation process, and then removing them from the cross-section through chemical or physical methods after the finished product, such as CN 111044426B and CN 110658122B; 2. Cutting the finished metal product, processing and filling the defect shape on the cross-section, and finally welding, such as CN 113109439A; 3. Using mechanical indentation or laser drilling to prepare unfused areas on the surface of the test block to introduce nickel-plated inclusions, such as CN 113182531A, or placing foreign objects during powder spreading to simulate void defects; 4. For porosity defects, the method of omitting the corresponding void positions is often used, such as CN114839010A.

[0006] Besides internal prefabrication, another method simulates "defects" by drilling holes to a certain depth from the outside after molding. However, none of these methods can accurately simulate relatively realistic internal defects. The resulting inclusions differ from the base material and can easily affect the mechanical performance of the structural components.

[0007] In summary, current methods for addressing pre-fabricated internal defects in laser melting additive manufacturing still fall short in accurately evaluating the impact of naturally formed void defects and guiding the development of reasonable process acceptance standards. How to prepare high-confidence voids for standard test evaluation remains a bottleneck in fatigue damage tolerance design. Summary of the Invention

[0008] In order to overcome the above-mentioned problems in the prior art, the present invention provides a laser melting additive manufacturing prefabricated internal defect test piece and preparation method, which is used to solve the above-mentioned problems in the prior art.

[0009] A method for preparing a prefabricated internal defect test specimen using laser melting additive manufacturing, the method comprising the following steps:

[0010] S1. Preparing for internal defects in the prefabrication process;

[0011] S2. Prepare metal powder raw materials;

[0012] S3. The metal powder raw material is evenly spread on a laser melting bed, and the pre-made internal defects are placed in a determined position during the spreading process;

[0013] S4. The uniformly laid metal powder raw material and the prefabricated internal standard defect part are melted using laser melting additive manufacturing;

[0014] S5. Fix the processed product into a fixed shape;

[0015] S6. Inspect the fixed product. If it is qualified, a pre-made internal defect test piece is obtained. The order of S1 and S2 is adjustable.

[0016] In addition to the aspects and any possible implementations described above, an implementation is further provided, wherein S1 specifically includes:

[0017] S11. Determine the shape and size information of prefabricated internal defects;

[0018] S12. Make the female mold and the male mold according to the shape and size information;

[0019] S13. The hydrogel is poured into the female mold at room temperature and then subjected to low-temperature cryogenic molding.

[0020] S14. Place the processed hydrogel solid and ceramic clay slurry into the positive mold;

[0021] S15. The positive mold is subjected to high-temperature shaping and drying treatment to obtain a thin-walled defect blank, which is used as a pre-made internal defect.

[0022] In addition to the aspects described above and any possible implementations, a further implementation is provided in which the metal powder comprises one or a mixture of several of aluminum alloys, titanium alloys, stainless steel, and nickel-based alloys with melting points below 1700°C.

[0023] In addition to the aspects and any possible implementations described above, an implementation is further provided in which the parameters used by the laser include: control power less than or equal to 120W, scanning rate less than or equal to 90mm / s, and molten metal temperature less than 2000℃.

[0024] In addition to the aspects described above and any possible implementation, a further implementation is provided in which the ceramic clay comprises Al2O3, SiO2, H2O and trace amounts of Fe2O3 and TiO2.

[0025] In addition to the aspects described above and any possible implementation, a further implementation is provided in which the low temperature in S13 is below -10°C and the high temperature in S15 is 70°C-80°C.

[0026] In addition to the aspects described above and any possible implementation, a further implementation is provided in which the wall thickness of the prefabricated internal defect is 10μm-40μm and the size is between 100μm and 10mm.

[0027] In addition to the aspects described above and any possible implementations, a further implementation is provided in which the metal powder is spherical or nearly spherical, with a size range of about 10-100 μm and a volume fraction of 10%-50%.

[0028] According to the above aspect and any possible implementation manners, a further implementation manner is provided, and the inspection includes detecting the position and size of the prefabricated internal defect, and the test piece is qualified if it meets the requirements.

[0029] The invention also provides a laser melting additive manufacturing test piece with prefabricated internal defects, which is prepared by the preparation method of the test piece with prefabricated internal defects, the test piece includes prefabricated internal defects, and the prefabricated internal defects are at any set positions of the test piece.

[0030] Beneficial Effects of the Invention

[0031] Compared with the prior art, the invention has the following beneficial effects:

[0032] The method for preparing a laser melting additive manufacturing test piece with prefabricated internal defects of the invention includes: preparing prefabricated internal defects; preparing metal powder raw materials; uniformly laying the metal powder raw materials on a laser melting bed, and placing the prefabricated internal defects at determined positions during laying; performing melting treatment on the uniformly laid metal powder raw materials and the prefabricated internal standard defect piece by using laser melting additive manufacturing; performing fixed forming on the treated product; and inspecting the fixed-formed product, and if the product is qualified, obtaining the test piece with prefabricated internal defects. The method has the following beneficial effects:

[0033] 1) Ultra-thin ceramic defects are introduced, which can relatively accurately simulate the shapes and sizes of internal voids generated in additive manufacturing;

[0034] 2) The prefabricated defects are placed in a powder metal matrix, which can simulate void defects or inclusions at any positions;

[0035] 3) The prefabricated defects formed by using the characteristics of ceramics, such as high rigidity, low elongation at break, high temperature resistance, smooth surface, high surface tension, and poor bonding after being infiltrated with liquid metal, have little impact on the real mechanical properties of the test piece;

[0036] 4) Clay blanks have good formability at room temperature and can be integrally formed with laser-melted metal additive manufacturing at high temperature;

[0037] 5) The proposed method for laser melting additive manufacturing test pieces with prefabricated internal defects has the characteristics of low cost, good effect, high void precision and strong applicability. Description of Drawings

[0038] Figure 1 is a detailed method flow of the invention Figure 1 ;

[0039] Figure 2 is a schematic diagram of a powder bed fusion additive manufacturing metal material fatigue performance test piece of the invention;

[0040] Figure 3 This is a schematic diagram of the prefabricated defect test specimen of the present invention;

[0041] Figure 4 The method flow of the present invention Figure 2 . Detailed Implementation

[0042] To better understand the technical solution of this invention, the content of this invention includes, but is not limited to, the specific embodiments described below. Similar technologies and methods should be considered within the scope of protection of this invention. To make the technical problems to be solved, the technical solutions, and advantages of this invention clearer, a detailed description will be provided below in conjunction with the accompanying drawings and specific embodiments.

[0043] It should be understood that the embodiments described in this invention are merely some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without inventive effort are within the scope of protection of this invention.

[0044] The terminology used in the embodiments of this invention is for the purpose of describing particular embodiments only and is not intended to limit the invention. The singular forms “a,” “the,” and “the” as used in the embodiments of this invention and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise.

[0045] like Figure 4 As shown, this invention provides a method for preparing a prefabricated internal defect test specimen using laser melting additive manufacturing, the method comprising the following steps:

[0046] S1. Preparing for internal defects in the prefabrication process;

[0047] S2. Prepare metal powder raw materials;

[0048] S3. The metal powder raw material is evenly spread on a laser melting bed, and the pre-made internal defects are placed in a determined position during the spreading process;

[0049] S4. The uniformly laid metal powder raw material and the prefabricated internal standard defect part are melted using laser melting additive manufacturing;

[0050] S5. Fix the processed product into a fixed shape;

[0051] S6. Inspect the fixed product. If it is qualified, a pre-made internal defect test piece is obtained. The order of S1 and S2 is adjustable.

[0052] Preferably, S1 specifically includes:

[0053] S11. Determine the shape and size information of prefabricated internal defects;

[0054] S12. Fabricate a female mold and a male mold according to the shape and size information;

[0055] S13. Pour the hydrogel into the female mold at room temperature, and perform low-temperature freezing molding treatment;

[0056] S14. Place the hydrogel solid obtained from the treatment and the ceramic clay slurry into the male mold;

[0057] S15. Perform high-temperature setting and drying treatment on the male mold to obtain a thin-walled defective blank, which serves as a prefabricated internal defect.

[0058] Preferably, the metal powder includes one or a mixture of several of aluminum alloy, titanium alloy, stainless steel, and nickel-based alloy with a melting point lower than 1700°C.

[0059] Preferably, the parameters adopted by the laser include: a control power of ≤120W, a scanning rate of ≤90mm / s, and a molten metal temperature lower than 2000°C.

[0060] Preferably, the ceramic clay includes Al₂O₃, SiO₂, H₂O, and trace amounts of Fe₂O₃ and TiO₂.

[0061] Preferably, the low temperature in S13 is lower than -10°C, and the high temperature in S15 is 70°C to 80°C.

[0062] Preferably, the wall thickness of the prefabricated internal defect is 10 μm to 40 μm, and the size ranges from 100 μm to 10 mm.

[0063] Preferably, the metal powder is spherical or approximately spherical, with a size range of about 10-100 μm and a volume fraction of 10% to 50%.

[0064] Preferably, the inspection includes detecting the position and size of the prefabricated internal defect, and if it meets the requirements, it is qualified.

[0065] The specific implementation process of the present invention is as follows:

[0066] As Figure 1 shown:

[0067] Steps A1 to A6 of this invention provide a method for prefabricating internal defect test specimens using laser melting additive manufacturing. These test specimens are based on laser melting powder bed additive manufacturing and are used for mechanical property testing. Specifically, A1 involves preparing the raw materials, which are metal powder matrices. The matrix can be a type of metal additive manufacturing powder with a melting point below 1700℃, such as aluminum alloy, titanium alloy, stainless steel, or nickel-based alloy. After the size and location of the pre-embedded defects are inspected and found to be acceptable, this test specimen is used for mechanical property evaluation after pore damage. Subsequent evaluations can establish acceptance criteria for defect size and morphology. Therefore, the test specimen obtained in A6 serves as a mechanical property test specimen, which can include static tensile, compression, and shear tests, fatigue and crack propagation tests, fracture toughness tests, etc. The dimensions of the test specimens conform to ASTM / GB / HB standards, such as the fatigue test specimen dimensions specified in HB5287. Figure 2 As shown;

[0068] Step A2: The powder spreading process is set by the machine program, spreading the powder layer by layer and solidifying it with laser melting. The layer thickness depends on the size of the laser melting area. For pre-fabricated defects, a specific layer of powder is spread (at a specific location) using a metal wire to carry it in. Pre-fabricated internal defects are placed in appropriate positions during powder spreading and are integrally formed with the laser melting area.

[0069] like Figure 1 In step A3, the laser control power should be within 120W and the scanning rate within 90mm / s. The temperature of the laser-melted metal monitored by the thermal imager should be below 2000℃, and the temperature should be controlled between 1800℃ and 1900℃. Considering the temperature resistance of the defect material, and due to the temperature resistance limitation of Al2O3, the laser melting temperature should be controlled below 2000℃. Considering the forming rate and thermal diffusivity of the laser for metals molten below 1700℃, the above parameters are adopted. If the forming is too fast and the power is too high, it will affect the defect deformation control, because the defect needs to maintain a solid shape at all times. The thermal imager monitors the laser-melted metal to detect the forming temperature to prevent the defect from melting. The pre-made defect is wrapped in a metal wire pit and sent into the laser forming area.

[0070] Steps A4-A5: A4. Solidification and molding: A high-energy laser beam partially melts the laid metal powder into a liquid state. Due to the internal tension of the liquid, it agglomerates to form a larger solid. This process is repeated to form additive manufacturing.

[0071] A5. CT Inspection: After surface treatment, the prepared additive blank is scanned in an industrial CT imaging area to identify the size and location of defects. The formed additive blank is then inspected using industrial CT to determine whether the location, shape, and size of pre-fabricated defects meet the expected pre-embedded specifications.

[0072] In steps C1 to C2, the prefabrication defect is assisted by two materials: hydrogel and ceramic clay. Hydrogel is easy to volatilize, while ceramic clay is generally fired at 1360℃ to form a white blank. Its main component, alumina ceramic, has a melting point of 2050℃ and good shape retention. The present invention preferably prepares ceramic clay by mixing powder (Al2O3 content greater than 99.8%) and deionized water in a mass ratio of 1:1 using an electromagnetic stirrer to form a clay slurry.

[0073] In steps D1 to D2, the prefabricated defect is formed using two temperature fields to assist in its molding. By utilizing the solid-gas phase conversion of water, a hollow defect that can withstand high temperatures is formed. The preferred low temperature step in D1 is freezing and shaping at -10℃. The preferred high temperature step in D2 is hot air drying at 70℃-80℃ with a wind speed of less than 3m / s for 30 minutes.

[0074] Steps B1 through B5: In B1, the shape and size of the pre-fabricated defect are used as input for preparing the B2 defect male mold and the B4 defect female mold, with sizes ranging from 50 μm to 10 mm. The hydrogel is poured into the B2 mold at room temperature and then cryogenically frozen for shaping. Further, the hydrogel solid and prepared clay slurry are placed in the B4 defect female mold, controlling the clay slurry wall thickness to approximately 10 μm. After molding, the mold is placed in a high-temperature oven to dry the moisture and solidify the hydrogel, forming a thin-walled defect blank. The defects obtained in these steps have the following advantages: the ceramic has higher high-temperature resistance than metal powder, less thermal deformation, and is formed at high temperatures; the ceramic clay has good formability; the hydrogel-assisted molding and subsequent drying ensure that the defect contains only dry clay; the defect wall thickness is relatively thin, more closely resembling a bubble defect; and it has minimal impact on the mechanical properties of the test piece, especially fatigue crack propagation performance.

[0075] The pre-fabricated thin-walled defects are placed at the pre-fabricated test piece location during the powder spreading process. Laser additive manufacturing process parameters are set to ensure that the metal melts into a liquid while the void defects remain solid. After the additive manufacturing blank is completed, industrial CT is used as a non-destructive testing method to perform non-destructive testing on the blank to verify the location and size of the pre-fabricated defects. A schematic diagram of the pre-fabricated defect test piece is shown below. Figure 3 As shown;

[0076] Preferably, the metal matrix powder is spherical or nearly spherical, with a size range of about 10-100 μm and a volume fraction of about 10%-50%. The defect wall thickness is about 10 μm-40 μm, and the pore size is distributed between 100 μm and several millimeters.

[0077] Furthermore, the main chemical components of ceramic clay are Al₂O₃, SiO₂, H₂O, and trace amounts of Fe₂O₃ and TiO₂. Chemical composition is a crucial factor in evaluating clay quality; higher Al₂O₃ content results in better high-temperature resistance and a stronger finished product. This invention preferably uses alumina ceramics, which have a melting point of up to 2050℃, but industrial ceramics, which have a high-temperature resistance of up to 2600℃, can also be used.

[0078] To obtain a standard defect, a defect female mold is manufactured using a preset defect shape and size as the initial input. Hydrogel is placed in the mold and solidified at low temperature to form an inner mold (male mold); the gap between the female and male molds is approximately 50 μm. Ceramic clay is placed between the male and female molds and dried in an oven at 70-80℃ to remove moisture and solidify the hydrogel, forming a thin-walled defect blank. If the laser melting temperature exceeds 2000℃, pre-fabricated defects can also be prepared using vapor deposition to produce SiC industrial ceramics. The test specimen dimensions conform to ASTM / GB / HB standards, such as the fatigue test specimen dimensions specified in HB5287. Figure 2 As shown. The additive manufacturing process is as follows. Figure 1 As shown in A1 to A6. The main metal raw materials suitable for this process are titanium alloys, aluminum alloys, stainless steel, and other metals with melting points below 1700℃.

[0079] Preferably, among the metals commonly used in additive manufacturing of aerospace load-bearing components, titanium alloys have the highest melting point temperature, which is 1670℃.

[0080] After the additive manufacturing blank is completed, industrial CT is used to perform non-destructive testing on the blank to determine the location and size of pre-fabrication defects. If the test is passed, the blank is qualified; otherwise, it is scrapped.

[0081] As an embodiment of the present invention, the present invention also provides a laser melting additive manufacturing prefabricated internal defect test specimen, the test specimen being prepared by the aforementioned preparation method, the test specimen including prefabricated internal defects, and the prefabricated internal defects being located at any predetermined position on the test specimen.

[0082] The foregoing description illustrates and describes several preferred embodiments of the present invention. However, as previously stated, it should be understood that the present invention is not limited to the forms disclosed herein and should not be construed as excluding other embodiments. It can be used in various other combinations, modifications, and environments, and can be altered within the scope of the inventive concept described herein through the foregoing teachings or techniques or knowledge in related fields. Any modifications and variations made by those skilled in the art that do not depart from the spirit and scope of the present invention should be within the protection scope of the appended claims.

Claims

1. A method for preparing a prefabricated internal defect test specimen using laser melting additive manufacturing, characterized in that, The method includes the following steps: S1. Preparing prefabricated internal defects, specifically including: S11. Determining the shape and size information of the prefabricated internal defects; S12. Fabricating a female mold and a male mold according to the shape and size information; S13. Pouring a hydrogel into the female mold at room temperature, and performing low-temperature freeze forming treatment, where the low temperature is lower than -10℃; S14. Placing the treated hydrogel solid and ceramic clay slurry into the male mold; S15. Performing high-temperature setting and drying treatment on the male mold to obtain a thin-walled defect blank, which serves as the prefabricated internal defect, the wall thickness of the prefabricated internal defect is 10 μm to 40 μm, and the high temperature in S15 is 70℃ to 80℃; S2. Preparing a metal powder raw material, which includes one or a mixture of several of aluminum alloy, titanium alloy, stainless steel, and nickel-based alloy with a melting point lower than 1700℃; S3. Uniformly laying the metal powder raw material on a laser melting bed, and placing the prefabricated internal defect at a determined position during laying, where the prefabricated internal defect is conveyed by being wrapped with a metal wire when laying a specific powder layer; S4. Performing melting treatment on the uniformly laid metal powder raw material and the prefabricated internal defect by laser melting additive manufacturing, where the parameters of the laser include: a controlled power of no more than 120 W, a scanning speed of no more than 90 mm / s, and a molten metal temperature lower than 2000℃; S5. Fixing and forming the treated product; S6. Inspecting the fixed and formed product, and if qualified, obtaining a prefabricated internal defect test piece, where the order of S1 and S2 can be adjusted.

2. The method for preparing a prefabricated internal defect test specimen using laser melting additive manufacturing according to claim 1, characterized in that, The inspection includes detecting the position and size of the prefabricated internal defect, and the product is qualified if it meets the requirements.

Citation Information

Patent Citations

  • A method for manufacturing a porosity comparison test block and the porosity comparison test block itself.

    CN110658122B

  • A method for manufacturing a porosity comparison test block and the porosity comparison test block itself.

    CN111044426B

  • Method for preparing inclusion defect with controllable size and position in metal material

    CN113109439A

  • Additive manufacturing test piece and manufacturing method

    CN114839010A

  • Composite defect for nondestructive testing of metal additive manufacturing and preparation method of composite defect

    CN113182531A