High-strength thermal insulation mortar and preparation method thereof
By optimizing the composition and proportion of high-strength thermal insulation mortar, and combining it with coal gangue, fly ash, silica fume, basalt fiber and polypropylene fiber, the problem of balancing thermal conductivity and mechanical properties in existing technologies has been solved, and the effective application of high-strength thermal insulation mortar in high-temperature tunnels has been realized.
Patent Information
- Application Number
- CN202410229347.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-02-29
AI Technical Summary
Existing high-strength thermal insulation mortars have limitations in improving load-bearing capacity and thermal conductivity, making it difficult to balance thermal conductivity and mechanical properties.
The mortar uses a combination of fine aggregates, cementitious materials, aerogels, fiber admixtures, early strength agents and water-reducing agents. By incorporating coal gangue, fly ash, silica fume, basalt fiber and polypropylene fiber, the proportions are optimized to improve the overall performance of the mortar, including reducing the thermal conductivity and increasing the compressive strength.
The application of high-strength thermal insulation mortar as a long-term support material in high-temperature tunnels has been realized. It has a low thermal conductivity and meets the high strength requirements, which enhances the load-bearing and thermal insulation performance of the thermal insulation mortar in many ways.
Smart Images

Figure CN117902863B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of environmentally friendly building materials technology, and specifically relates to a high-strength heat-insulating mortar and its preparation method. Background Technology
[0002] With the gradual development of tunnel engineering, the problem of heat hazards caused by high ground temperatures has become increasingly prominent, becoming one of the unavoidable geological hazards in tunnel construction. Thermal insulation materials, due to their low thermal conductivity, can significantly reduce the release of heat from the surrounding rock into the tunnel and are widely used in high-temperature underground engineering. However, these materials often suffer from low strength and poor durability, limiting their use to temporary insulation measures rather than load-bearing and long-term support structures. Thermal insulation mortar offers a new solution to this problem. Thermal insulation mortar is a new generation of green and environmentally friendly insulation material, characterized by high strength, low thermal conductivity, good workability, excellent thermal insulation performance, low cost, good cohesion after mixing with water, and ease of construction.
[0003] Currently, research on high-strength thermal insulation mortar mainly focuses on the development of high-strength thermal insulation mortar with one or two admixtures, or on adding materials such as fibers to thermal insulation mortar to increase compressive strength. However, these studies still employ relatively singular methods to improve the thermal insulation and load-bearing performance of mortar, primarily concentrating on single or limited aspects such as aggregate replacement, cementitious material addition, porosity optimization, and fiber incorporation. This approach has limitations in improving the overall performance of load-bearing thermal insulation mortar, and the drawback of difficulty in simultaneously achieving optimal thermal conductivity and load-bearing capacity remains. Furthermore, the development process often lacks evaluation indicators for the overall thermal performance of mortar, making it difficult to accurately assess the merits of different mix proportions of mortar.
[0004] Therefore, how to provide a high-strength thermal insulation mortar that not only has a low thermal conductivity but also meets the strength requirements of long-term support concrete for high-temperature tunnels is a problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0005] The technical problem to be solved by the present invention is that the existing technology has certain limitations in improving the comprehensive performance of load-bearing heat-insulating mortar, and there are still technical problems such as the difficulty in balancing thermal conductivity and mechanical properties.
[0006] To address the aforementioned problems, a first aspect of the present invention provides a high-strength thermal insulation mortar, comprising fine aggregate, cementitious material, aerogel, fiber admixture, early-strength agent, water-reducing agent, and water; wherein the fine aggregate includes river sand and coal gangue, with the mass content of coal gangue being 30% of the total mass of the high-strength thermal insulation mortar; the cementitious material includes ordinary silicate cement, fly ash, and silica fume, with the mass content of fly ash being 7.06% of the total mass of the high-strength thermal insulation mortar, and the mass content of silica fume being 3.35% of the total mass of the high-strength thermal insulation mortar; the mass content of aerogel is 0.26% of the total mass of the high-strength thermal insulation mortar; and the fiber admixture includes basalt fiber and polypropylene fiber, with the volume content of basalt fiber being 0.05% of the total volume of the high-strength thermal insulation mortar, and the volume content of polypropylene fiber being 0.45% of the total volume of the high-strength thermal insulation mortar.
[0007] In the first aspect, the mass concentration of the fine aggregate is 1600 kg / m³. 3 The mass concentration of the cementitious material is 340 kg / m³. 3 The water has a mass concentration of 310 kg / m³. 3 .
[0008] In the first aspect, the fineness modulus of the river sand is 2.8, and the bulk density of the river sand is 1600 kg / m³. 3 The gradation standard area is Class II; the mesh size of the coal gangue is 6-8 mesh, and the bulk density of the coal gangue is 1835.4 kg / m³. 3 .
[0009] Secondly, the present invention provides a method for preparing high-strength thermal insulation mortar, the method comprising: designing a first orthogonal experiment to obtain several sets of first experimental results; selecting preferred experimental results from the several sets of first experimental results using thermal conductivity ratio, thermal conductivity, and uniaxial compressive strength as performance evaluation indicators; obtaining an optimal mix ratio of high-strength thermal insulation mortar based on the preferred experimental results; designing a second orthogonal experiment to reduce the horizontal span of each factor based on the preferred mix ratio to obtain several sets of second experimental results; selecting the optimal experimental results from the several sets of second experimental results using thermal conductivity ratio, thermal conductivity, and uniaxial compressive strength as performance evaluation indicators; obtaining an optimal mix ratio of high-strength thermal insulation mortar based on the optimal experimental results; and preparing high-strength thermal insulation mortar based on the optimal mix ratio; wherein the high-strength thermal insulation mortar is composed of fine aggregate, cementitious materials, aerogel, fiber admixture, early-strength agent, water-reducing agent, and water.
[0010] In the second aspect, the thermal conductivity ratio is set as: RST = σ / λ; where RST is the thermal conductivity ratio, in MPa·m·K / W; σ is the uniaxial compressive strength, in MPa; and λ is the thermal conductivity, in W / m·K.
[0011] In the second aspect, the mass concentration of the water is 310 kg / m³. 3 The mass concentration of the fine aggregate is 1600 kg / m³. 3 The fine aggregate includes river sand and coal gangue, and the cementitious material has a mass concentration of 340 kg / m³. 3 The cementitious material includes ordinary silicate cement, fly ash and silica fume, and the fiber admixture includes basalt fiber and polypropylene fiber.
[0012] In the second aspect, in the optimal proportions: the mass content of coal gangue is 30% of the total mass of the high-strength thermal insulation mortar, the mass content of fly ash is 7.06% of the total mass of the high-strength thermal insulation mortar, the mass content of silica fume is 3.35% of the total mass of the high-strength thermal insulation mortar, the mass content of aerogel is 0.26% of the total mass of the high-strength thermal insulation mortar, the volume content of basalt fiber is 0.05% of the total volume of the high-strength thermal insulation mortar, and the volume content of polypropylene fiber is 0.45% of the total volume of the high-strength thermal insulation mortar.
[0013] In the second aspect, the design of the first orthogonal experiment to obtain several sets of first test results includes: designing the first orthogonal experiment to obtain 25 sets of first mix proportion schemes, preparing a corresponding first mortar sample according to each set of first mix proportion schemes, and conducting performance tests on the 25 first mortar samples to obtain 25 sets of first test results; wherein, the first orthogonal experiment is a six-factor, five-level orthogonal experiment, the six factors include coal gangue, fly ash, silica fume, aerogel, basalt fiber and polypropylene fiber, and the performance tests include compressive strength testing and thermal conductivity testing.
[0014] In the second aspect, the step of narrowing the horizontal span of each factor based on the preferred mix proportion to design a second orthogonal experiment to obtain several sets of second test results includes: narrowing the horizontal span of each factor based on the preferred mix proportion to design a second orthogonal experiment to obtain 18 sets of second mix proportion schemes, preparing a corresponding second mortar sample according to each set of second mix proportion schemes, and conducting performance tests on the 18 second mortar samples to obtain 18 sets of second test results; wherein, the second orthogonal experiment is the six-factor, three-level orthogonal experiment.
[0015] In the second aspect, the preparation of high-strength thermal insulation mortar according to the optimal proportion includes: weighing fine aggregate, cementitious material, aerogel, fiber admixture, early-strength agent, water-reducing agent, and water according to the optimal proportion; after weighing, adding the cementitious material, early-strength agent, water-reducing agent, and aerogel to the fine aggregate in sequence, mixing and stirring until the color is uniform to obtain an admixture; dispersing the fiber admixture into the admixture and mixing it; adding the water to the admixture and stirring for 3 minutes to obtain an initial mortar; pouring the initial mortar into a standard cylindrical mold with a diameter of 50 mm and a height of 100 mm, and tamping it evenly from the edge to the center 20 times with a tamping rod in a spiral direction; after molding, smoothing the top surface of the initial mortar 2 hours before the initial setting of the initial mortar; after demolding the initial mortar, placing the initial mortar in a standard curing box for curing for 14 days to obtain the high-strength thermal insulation mortar.
[0016] Beneficial Effects: This invention proposes a high-strength thermal insulation mortar, which is composed of fine aggregate, cementitious materials, aerogel, fiber admixtures, early-strength agent, water-reducing agent, and water. The thermal conductivity of the high-strength thermal insulation mortar is reduced by incorporating aerogel, coal gangue, and fly ash, and the compressive strength of the mortar is improved by incorporating silica fume, basalt fiber, and polypropylene fiber, thereby enhancing the load-bearing and thermal insulation performance of the mortar in multiple ways. Furthermore, the mass percentages of coal gangue, fly ash, silica fume, and aerogel are 30% of the total mass of the high-strength thermal insulation mortar. The volumetric admixtures of basalt fiber and polypropylene fiber are 7.06%, 3.35%, and 0.26%, respectively, representing 0.05% and 0.45% of the total volume of the high-strength thermal insulation mortar. By rationally combining the proportions of coal gangue, fly ash, silica fume, aerogel, basalt fiber, and polypropylene fiber, the upper limit of the mortar's performance optimization is improved. This results in the high-strength thermal insulation mortar of the present invention not only possessing a low thermal conductivity but also meeting the strength requirements of long-term support concrete for high-temperature tunnels, making it an excellent thermal insulation and load-bearing material for high-temperature tunnels. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of this specification or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 This is a flowchart illustrating the preparation method of high-strength thermal insulation mortar in an embodiment of the present invention; Detailed Implementation
[0019] The technical solutions of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention are within the scope of protection of the present invention.
[0020] Furthermore, throughout this specification, unless otherwise specified, the terminology used herein should be understood as having the meaning commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In the event of any conflict, this specification shall prevail.
[0021] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.
[0022] Example 1
[0023] This embodiment provides a high-strength thermal insulation mortar, which is composed of fine aggregate, cementitious materials, aerogel, fiber admixtures, early-strength agent, water-reducing agent, and water. The fine aggregate includes river sand and coal gangue, with the coal gangue comprising 30% of the total mass of the high-strength thermal insulation mortar. The cementitious materials include ordinary silicate cement, fly ash, and silica fume, with the fly ash comprising 7.06% of the total mass of the high-strength thermal insulation mortar and the silica fume comprising 3.35% of the total mass. The aerogel comprises 0.26% of the total mass of the high-strength thermal insulation mortar. The fiber admixture includes basalt fiber and polypropylene fiber, with the basalt fiber comprising 0.05% of the total volume of the high-strength thermal insulation mortar and the polypropylene fiber comprising 0.45% of the total volume.
[0024] Specifically, this invention proposes a high-strength thermal insulation mortar, which is composed of fine aggregate, cementitious materials, aerogel, fiber admixtures, early-strength agent, water-reducing agent, and water. The thermal conductivity of the high-strength thermal insulation mortar is reduced by incorporating aerogel, coal gangue, and fly ash, and the compressive strength of the mortar is improved by incorporating silica fume, basalt fiber, and polypropylene fiber, thereby enhancing the load-bearing and thermal insulation performance of the mortar in multiple ways. Furthermore, the mass percentages of coal gangue, fly ash, silica fume, and aerogel are 30% of the total mass of the high-strength thermal insulation mortar. The volumetric admixtures of basalt fiber and polypropylene fiber are 7.06%, 3.35%, and 0.26%, respectively, representing 0.05% and 0.45% of the total volume of the high-strength thermal insulation mortar. By rationally combining the proportions of coal gangue, fly ash, silica fume, aerogel, basalt fiber, and polypropylene fiber, the upper limit of the mortar's performance optimization is improved. This results in the high-strength thermal insulation mortar of the present invention not only possessing a low thermal conductivity but also meeting the strength requirements of long-term support concrete for high-temperature tunnels, making it an excellent thermal insulation and load-bearing material for high-temperature tunnels.
[0025] In some possible implementations, the mass concentration of the fine aggregate is 1600 kg / m³. 3 The mass concentration of the cementitious material is 340 kg / m³. 3 The water has a mass concentration of 310 kg / m³. 3 .
[0026] In some possible implementations, the fineness modulus of the river sand is 2.8, and the bulk density of the river sand is 1600 kg / m³. 3 The gradation standard area is Class II; the mesh size of the coal gangue is 6-8 mesh, and the bulk density of the coal gangue is 1835.4 kg / m³. 3 .
[0027] Those skilled in the art will understand that the fineness modulus of the river sand in the fine aggregate is 2.8, and the bulk density of the river sand is 1600 kg / m³. 3 The gradation standard area is Class II, the mesh size of the coal gangue is 6-8 mesh, and the bulk density of the coal gangue is 1835.4 kg / m³. 3 This results in high-strength thermal insulation mortar having greater density, porosity, and smaller specific surface area. When preparing concrete, relatively less water is needed, which can improve the mechanical properties and durability of high-strength thermal insulation mortar.
[0028] Example 2
[0029] This embodiment two provides a method for preparing high-strength thermal insulation mortar. The preparation method includes: S1 designing a first orthogonal experiment to obtain several sets of first test results, selecting the preferred test results from the several sets of first test results using the thermal conductivity ratio, thermal conductivity, and uniaxial compressive strength as performance evaluation indicators, and obtaining the preferred mix ratio of high-strength thermal insulation mortar based on the preferred test results; S2 designing a second orthogonal experiment based on the preferred mix ratio to narrow the horizontal span of each factor and obtain several sets of second test results, selecting the optimal test results from the several sets of second test results using the thermal conductivity ratio, thermal conductivity, and uniaxial compressive strength as performance evaluation indicators, and obtaining the optimal mix ratio of high-strength thermal insulation mortar based on the optimal test results; S3 preparing high-strength thermal insulation mortar based on the optimal mix ratio; wherein, the high-strength thermal insulation mortar is composed of fine aggregate, cementitious materials, aerogel, fiber admixture, early strength agent, water-reducing agent, and water.
[0030] Specifically, this invention proposes a method for preparing high-strength thermal insulation mortar. First, several sets of first test results are obtained through a first orthogonal experiment. Then, the optimal test results are selected from these first test results. Based on the optimal test results, the optimal mix ratio of the high-strength thermal insulation mortar is obtained. Further, the optimal mix ratio of the mortar is preliminarily determined through limited experiments. Next, based on the optimal mix ratio, a second orthogonal experiment is designed to narrow the horizontal span of each factor, resulting in several sets of second test results. The optimal test results are selected from these second test results. Based on the optimal test results, the optimal mix ratio of the high-strength thermal insulation mortar is obtained. Further, the optimal mix ratio is optimized through limited experiments. In addition, this invention introduces the "thermal conductivity ratio" to evaluate the comprehensive performance of the mortar, linking the thermal insulation and load-bearing performance of the mortar, indicating the optimization direction of the comprehensive thermal performance of the mortar. Finally, the optimal mix ratio is selected based on the thermal conductivity ratio, resulting in high-strength thermal insulation mortar prepared with the optimal mix ratio achieving a lower thermal conductivity and higher compressive strength. In addition, thermal conductivity and compressive strength are also used as performance evaluation indicators to avoid the situation where the strength-to-conductivity ratio fails when thermal conductivity and compressive strength are both high or low.
[0031] In some possible implementations, the thermal conductivity ratio is set as: RST = σ / λ; where RST is the thermal conductivity ratio, in MPa·m·K / W; σ is the uniaxial compressive strength, in MPa; and λ is the thermal conductivity, in W / m·K.
[0032] This is because the ratio of a material's uniaxial compressive strength to its thermal conductivity is defined as the "strength-to-conductivity ratio." According to the definition, when both strength and thermal conductivity change simultaneously, the strength-to-conductivity ratio can effectively measure the changes in their combined performance, indicating the direction for optimizing the overall thermal performance of mortar. Consequently, the optimal mix ratio can be accurately selected based on the strength-to-conductivity ratio.
[0033] In some possible implementations, the water has a mass concentration of 310 kg / m³. 3 The mass concentration of the fine aggregate is 1600 kg / m³. 3 The fine aggregate includes river sand and coal gangue, and the cementitious material has a mass concentration of 340 kg / m³. 3 The cementitious material includes ordinary silicate cement, fly ash and silica fume, and the fiber admixture includes basalt fiber and polypropylene fiber.
[0034] In some possible implementations, the optimal proportions are as follows: the mass fraction of coal gangue is 30% of the total mass of the high-strength thermal insulation mortar; the mass fraction of fly ash is 7.06% of the total mass of the high-strength thermal insulation mortar; the mass fraction of silica fume is 3.35% of the total mass of the high-strength thermal insulation mortar; the mass fraction of aerogel is 0.26% of the total mass of the high-strength thermal insulation mortar; the volume fraction of basalt fiber is 0.05% of the total volume of the high-strength thermal insulation mortar; and the volume fraction of polypropylene fiber is 0.45% of the total volume of the high-strength thermal insulation mortar.
[0035] In some possible implementations, the design of the first orthogonal experiment to obtain several sets of first test results includes: designing the first orthogonal experiment to obtain 25 sets of first mix proportion schemes, preparing a corresponding first mortar sample according to each set of first mix proportion schemes, and conducting performance tests on the 25 first mortar samples to obtain 25 sets of first test results; wherein, the first orthogonal experiment is a six-factor, five-level orthogonal experiment, the six factors include coal gangue, fly ash, silica fume, aerogel, basalt fiber and polypropylene fiber, and the performance tests include compressive strength testing and thermal conductivity testing.
[0036] In some possible implementations, the step of narrowing the level span of each factor based on the preferred mix proportion to design a second orthogonal experiment to obtain several sets of second test results includes: narrowing the level span of each factor based on the preferred mix proportion to design a second orthogonal experiment to obtain 18 sets of second mix proportion schemes, preparing a corresponding second mortar sample according to each set of second mix proportion schemes, and conducting performance tests on the 18 second mortar samples to obtain 18 sets of second test results; wherein, the second orthogonal experiment is the six-factor, three-level orthogonal experiment.
[0037] In some possible implementations, the preparation of high-strength thermal insulation mortar according to the optimal proportion includes: weighing fine aggregate, cementitious material, aerogel, fiber admixture, early-strength agent, water-reducing agent, and water according to the optimal proportion; after weighing, adding the cementitious material, early-strength agent, water-reducing agent, and aerogel to the fine aggregate in sequence, mixing and stirring until the color is uniform to obtain an admixture; dispersing the fiber admixture into the admixture and mixing it; adding the water to the admixture and stirring for 3 minutes to obtain the initial mortar; pouring the initial mortar into a standard cylindrical mold with a diameter of 50 mm and a height of 100 mm, and tamping it evenly from the edge to the center 20 times with a tamping rod in a spiral direction; after molding, smoothing the top surface of the initial mortar 2 hours before the initial setting of the initial mortar; after demolding the initial mortar, placing the initial mortar in a standard curing box for curing for 14 days to obtain the high-strength thermal insulation mortar.
[0038] It should be noted that the high-strength heat-insulating mortar preparation method provided in this embodiment 2 is the same as the high-strength heat-insulating mortar described in this embodiment 1. Its implementation principle and technical concept are exactly the same as those in embodiment 1. Therefore, for the parts not described in detail in this embodiment 2, please refer to embodiment 1. They will not be repeated here.
[0039] To further illustrate the technical solution of this application and support the technical problem to be solved by this application, the preparation method of high-strength heat-insulating mortar is illustrated in detail below, as in Example 3.
[0040] Example 3
[0041] This embodiment three provides a method for preparing high-strength thermal insulation mortar, the preparation method comprising:
[0042] Using M20 cement mortar mix proportion without any admixtures as a control group, the heat insulation and load-bearing capacity enhancement effects of high-strength heat-insulating mortar were compared. To save research and development time, water-reducing agent and early-strength agent were added uniformly in the experiment, and the mortar curing age was shortened to 14 days. The basic data of M20 material mix proportion and 14-day curing are shown in Table 1 below. After curing, the thermal conductivity, uniaxial compressive strength and porosity of M20 cement mortar were tested.
[0043] Table 1. Material Proportioning and Performance Parameters of M20 Cement Mortar
[0044]
[0045] The first orthogonal experiment was designed to obtain several sets of experimental results. Specifically, this embodiment designed a six-factor, five-level orthogonal experiment, as shown in Table 2. In the table, basalt fiber and polypropylene fiber are volumetric admixtures, while the others are mass admixtures. Through orthogonal design, 25 formulation schemes were obtained, as shown in Table 3. In each formulation scheme, the mass concentration of water is 310 kg / m³. 3 The mass concentration of the fine aggregate is 1600 kg / m³. 3 The mass concentration of the cementitious material is 340 kg / m³. 3 Based on the unchanged, coal gangue replaced part of the fine aggregate, silica fume and fly ash replaced part of the ordinary silicate cement, and aerogel, fiber admixture, early strength agent and water-reducing agent were directly added as admixtures. The amount of early strength agent and water-reducing agent added in each group was the same. Six cylindrical standard specimens (φ50×100mm) were poured for each group of mix proportions and cured for 14 days according to the curing process specified in the specification (GB / T50081-2019). One first mortar specimen was prepared according to each group of first mix proportions. The performance of 25 first mortar specimens was tested to obtain the results of the 25 first tests, as shown in Table 4.
[0046] Table 2. Factor Levels of the First Orthogonal Experiment
[0047]
[0048] Table 3. First Orthogonal Experimental Design Table (Unit: %)
[0049]
[0050]
[0051] Table 4 Results of the First Test
[0052]
[0053]
[0054] The river sand used in this embodiment has a fineness modulus of 2.8 and a bulk density of 1600 kg / m³. 3 The gradation standard area is Class II; the mesh size of the coal gangue used is 6-8 mesh, and the bulk density of the coal gangue is 1835.4 kg / m³. 3 The density of the aerogel used is 52 kg / m³. 3 The thermal conductivity is less than 0.024; the chemical composition of silica fume, fly ash and ordinary silicate cement is shown in Table 5; the physical and mechanical properties of polypropylene fiber and basalt fiber composite are shown in Table 6.
[0055] Table 5 Chemical composition analysis of cementitious materials (mass fraction %)
[0056]
[0057] Table 6 Physical and Mechanical Properties
[0058]
[0059] Using the strength-to-conductivity ratio, thermal conductivity, and uniaxial compressive strength as performance evaluation indicators, the preferred test result is selected from several groups of first test results as A17. Based on the preferred test result and performing range analysis and variance analysis on the preferred test result, the preferred mix ratio of high-strength thermal insulation mortar is obtained as A1B2C1D3E1F5.
[0060] Based on the optimized ratio, the level range of each factor was narrowed to design a second orthogonal experiment to obtain several sets of second experimental results. Specifically, based on the optimized ratio obtained from the first orthogonal experiment, a six-factor, three-level orthogonal experiment was designed, with the level of each factor fluctuating up and down from the optimized ratio. The factor level table and orthogonal design table are shown in Tables 7 and 8 below. According to the factor level table (Table 7, where basalt fiber and polypropylene fiber are volumetric admixtures and the others are mass admixtures), a detailed experimental ratio scheme was designed (Table 8), totaling 18 groups. In each ratio scheme, the mass concentration of water is 310 kg / m³. 3 The mass concentration of the fine aggregate is 160 kg / m³. 3 The mass concentration of the cementitious material is 340 kg / m³. 3 Based on the unchanged premise, coal gangue replaced part of the fine aggregate, silica fume and fly ash replaced part of the ordinary Portland cement, and aerogel, fiber admixture, early strength agent, and water-reducing agent were directly added as admixtures. The addition amount of early strength agent and water-reducing agent was the same for each group. Six cylindrical standard specimens (φ50×100mm) were poured for each mix design and cured for 14 days according to the curing process specified in the standard (GB / T 50081-2019). The preparation process was strictly carried out in accordance with the relevant specifications. A second mortar specimen was prepared according to each second mix design, and the performance of 18 second mortar specimens was tested to obtain the results of the 18 second tests, as shown in Table 9.
[0061] Table 7. Factor Levels for the Second Orthogonal Experiment
[0062]
[0063] Table 8. Second Orthogonal Experimental Design Table (Unit: %)
[0064]
[0065]
[0066] Table 9 Results of the Second Test
[0067]
[0068]
[0069] Using the strength-to-conductivity ratio, thermal conductivity, and uniaxial compressive strength as performance evaluation indicators, the optimal test result B2 is selected from several groups of second test results. Based on the optimal test result and performing range analysis and variance analysis on the optimal test result, the optimal mix ratio of high-strength thermal insulation mortar is obtained as A1B1C3D2E1F1.
[0070] After determining the optimal mix ratio, verification of the optimal mix ratio was carried out. The core purpose of this stage was to confirm, through repeated experiments, whether the material mix ratio obtained from the previous analysis was the truly optimal mix ratio for the thermal insulation mortar. The mortar was prepared strictly according to the determined mix ratio, and its various properties were comprehensively tested to ensure the reliability of the mix ratio. The test results are shown in Table 7.
[0071] Table 7 Comparison of Experimental Results
[0072]
[0073] The results showed that the strength-to-conductivity ratio of the test group was 21.39, which was less than 5% different from that of the B2 group in the second round of tests, and increased by 60.7% compared with that of plain mortar. It has good thermal insulation and load-bearing capacity, and the test results are relatively stable.
[0074] High-strength thermal insulation mortar is prepared according to the optimal proportions. The high-strength thermal insulation mortar comprises fine aggregate, cementitious material, aerogel, fiber admixture, early-strength agent, water-reducing agent, and water. Specifically, fine aggregate, cementitious material, aerogel, fiber admixture, early-strength agent, water-reducing agent, and water are weighed according to the optimal proportions. After weighing, the cementitious material, early-strength agent, water-reducing agent, and aerogel are added to the fine aggregate sequentially. After each addition, the mixture is stirred for 2 minutes until the color is uniform. The mixture is then stirred until the color is uniform to obtain the admixture. The fiber admixture is dispersed into the admixture and mixed. Water is added to the admixture and stirred for 3 minutes to obtain the initial mortar. The initial mortar is poured into a standard cylindrical mold with a diameter of 50 mm and a height of 100 mm. A tamping rod is used to tamp the mortar evenly from the edge to the center 20 times in a spiral direction. After molding, the top surface of the initial mortar is smoothed 2 hours before the initial mortar sets. After the initial mortar is demolded, it is placed in a standard curing box for 14 days to obtain the high-strength heat-insulating mortar.
[0075] In this embodiment, the high-strength thermal insulation mortar prepared according to the optimal ratio has a thermal conductivity of approximately 0.8 W / m·K, a uniaxial compressive strength of up to 17 MPa, and a strength-to-conductivity ratio increased by 60.7%.
[0076] It should be noted that the preparation steps of M20 cement mortar in the control group, the preparation steps of the first mortar sample in the first orthogonal experiment, and the preparation steps of the second mortar sample in the second orthogonal experiment are all the same as the steps for preparing high-strength heat-insulating mortar according to the optimal mix ratio.
[0077] Finally, it should be noted that the terms “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0078] Although preferred embodiments of the invention have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including both the preferred embodiments and all changes and modifications falling within the scope of the invention.
[0079] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this invention and their equivalents, this invention also intends to include these modifications and variations.
Claims
1. A method for preparing high-strength heat-insulating mortar for long-term support of high-temperature tunnels, characterized in that, The preparation method includes: The first orthogonal experiment was designed to obtain several sets of first test results. The strength-to-conductivity ratio, thermal conductivity and uniaxial compressive strength were used as performance evaluation indicators to select the optimal test results from the several sets of first test results. Based on the optimal test results, the optimal mix ratio of high-strength thermal insulation mortar was obtained. Based on the preferred ratio, the horizontal span of each factor is narrowed to design a second orthogonal experiment to obtain several sets of second test results. The thermal conductivity, thermal conductivity and uniaxial compressive strength are used as performance evaluation indicators to select the optimal test result from several sets of second test results. Based on the optimal test result, the optimal ratio of high-strength thermal insulation mortar is obtained. High-strength thermal insulation mortar is prepared according to the optimal mix ratio; wherein, the high-strength thermal insulation mortar is composed of fine aggregate, cementitious material, aerogel, fiber admixture, early strength agent, water-reducing agent and water; The strong conductivity ratio is set as follows: RST = σ / λ; Where RST is the thermal conductivity ratio, in MPa·m·K / W; σ is the uniaxial compressive strength, in MPa; and λ is the thermal conductivity, in W / m·K. The mass concentration of the water is 310 kg / m³. 3 The mass concentration of the fine aggregate is 1600 kg / m³. 3 The fine aggregate includes river sand and coal gangue, and the cementitious material has a mass concentration of 340 kg / m³. 3 The cementitious material includes ordinary silicate cement, fly ash and silica fume, and the fiber admixture includes basalt fiber and polypropylene fiber; The fineness modulus of the river sand is 2.8, and the bulk density of the river sand is 1600 kg / m³. 3 The gradation standard area is Class II; the mesh size of the coal gangue is 6-8 mesh, and the bulk density of the coal gangue is 1835.4 kg / m³. 3 ; The coal gangue is added at a mass ratio of 30% of the total mass of the high-strength thermal insulation mortar; the fly ash is added at a mass ratio of 7.06% of the total mass of the high-strength thermal insulation mortar; the silica fume is added at a mass ratio of 3.35% of the total mass of the high-strength thermal insulation mortar; the aerogel is added at a mass ratio of 0.26% of the total mass of the high-strength thermal insulation mortar; the basalt fiber is added at a volume ratio of 0.05% of the total volume of the high-strength thermal insulation mortar; and the polypropylene fiber is added at a volume ratio of 0.45% of the total volume of the high-strength thermal insulation mortar. The density of the aerogel used is 52 kg / m³. 3 Thermal conductivity less than 0.024; The preparation of high-strength thermal insulation mortar according to the optimal ratio includes: Weigh out the fine aggregate, cementitious material, aerogel, fiber admixture, early strength agent, water-reducing agent and water according to the optimal proportions; After weighing, the cementitious material, the early strength agent, the water-reducing agent and the aerogel are added to the fine aggregate in sequence. After each addition, the mixture is stirred for 2 minutes until the color is uniform. After stirring until the color is uniform, the admixture is obtained. The fiber admixture is dispersed into the admixture and mixed. Then, the water is added to the admixture and stirred for 3 minutes to obtain the initial mortar. The initial mortar was poured into a standard cylindrical mold with a diameter of 50 mm and a height of 100 mm. The mold was then tamped 20 times in a spiral direction from the edge to the center. After molding, the top surface of the initial mortar was smoothed 2 hours before the initial mortar set. After the initial mortar was demolded, it was placed in a standard curing box for 14 days to obtain the high-strength heat-insulating mortar.
2. The preparation method according to claim 1, characterized in that, The design of the first orthogonal experiment yielded several sets of first experiment results, including: The first orthogonal experiment was designed to obtain 25 sets of first mix proportion schemes. A corresponding first mortar sample was prepared according to each set of first mix proportion schemes. The performance of the 25 first mortar samples was tested to obtain 25 sets of first test results. The first orthogonal experiment is a six-factor, five-level orthogonal experiment. The six factors include coal gangue, fly ash, silica fume, aerogel, basalt fiber, and polypropylene fiber. The performance tests include compressive strength testing and thermal conductivity testing.
3. The preparation method according to claim 2, characterized in that, The process of narrowing the level range of each factor based on the preferred ratio to design a second orthogonal experiment yields several sets of second experimental results, including: Based on the preferred proportions, the horizontal span of each factor was narrowed to design a second orthogonal experiment to obtain 18 sets of second proportion schemes. A corresponding second mortar sample was prepared according to each set of second proportion schemes. The performance of the 18 second mortar samples was tested to obtain 18 sets of second test results. The second orthogonal experiment is the six-factor, three-level orthogonal experiment.
Citation Information
Patent Citations
Coal-gangue lightweight aggregate concrete
CN105174834A
SiO2 aerogel mortar and preparation method thereof
CN105439505A
Thermal-insulation concrete
CN111848213A
Self-heat-preservation anti-freezing lining structure for traffic tunnel in seasonally frozen soil area
CN112983468A