Silicone-modified polyurethane resin coating agent composition
The polyurethane resin coating composition modified with siloxane solves the problems of membrane shrinkage and low strength of polyurethane resin in gas separation membranes, realizing the preparation of efficient and economical gas separation membranes with excellent air permeability and strength.
Patent Information
- Application Number
- CN202311337854.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2023-09-07
- Filing Date
- 2023-10-17
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-10-17
AI Technical Summary
In the existing technology, polyurethane resin has problems such as membrane shrinkage, low strength, long curing time and high cost when preparing gas separation membranes. In addition, the functional groups containing heteroatoms in the composite material can poison the catalyst, making it difficult to achieve efficient and economical gas separation.
A siloxane-modified polyurethane resin coating composition, comprising a specific composition of siloxane-modified polyurethane resin and volatile organic solvent, forms a transparent, light milky white film through curing, and the curing process is promoted by using a urethane curing catalyst.
It has been achieved that siloxane-modified polyurethane resin membranes with excellent air permeability, strength and flexibility can be formed at low cost through simple drying and solvent removal methods, which are suitable for continuous film formation of gas separation membranes.
Smart Images

Figure CN117903671B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to siloxane-modified polyurethane resin coating compositions, and more specifically to siloxane-modified polyurethane resin coating compositions capable of easily forming siloxane-modified polyurethane resin films with excellent permeability, strength and elongation by simply drying and removing volatile organic solvents. Background Technology
[0002] Polyurethane resin has excellent tensile strength, flexural strength, abrasion resistance and oil resistance, and can be prepared into thermoplastic or thermosetting resins according to its composition, so the resin can be processed into various shapes.
[0003] As is well known, silicone resins have various properties, such as excellent heat resistance, water resistance, slip resistance and electrical insulation, as well as high air permeability.
[0004] In recent years, gas separation membranes for separating and concentrating carbon dioxide gas from exhaust gases or air have been developed using these resins. However, when using the resin alone, gas permeability and selectivity are insufficient. Therefore, composite materials incorporating the resin have been developed.
[0005] As a composite material, various materials are used, such as silica, alumina, zeolite and metal-organic frameworks (MOF).
[0006] On the other hand, resins such as polyvinyl alcohol, polyimide, polysulfone, or polyether have been proposed as adhesive resins for bonding with composite materials (see Patent Documents 1 to 5). In particular, a resin called PIM-1 (a condensate of 5,5',6,6'-tetrahydroxy-3,3,3',3'-tetramethyl-1,1'-spirobisindane and tetrafluoroterephthalonitrile) (see Non-Patent Document 1) is rigid and has high air permeability.
[0007] However, a problem with PIM-1 is that when membranes are prepared from solutions of this polymer, they tend to shrink during solvent evaporation. Furthermore, the reactants are expensive and the purification process is complex, making it difficult to use industrially.
[0008] Silicone resin compositions are also promising adhesive resin compositions. In particular, addition-curable compositions are useful because they readily form films and exhibit increased strength. However, if the composite material to be blended contains heteroatom-containing functional groups (e.g., amino groups), these become platinum catalyst poisons, causing addition-curable compositions to experience curing inhibition.
[0009] To address this issue, Patent Document 3 proposes a gas separation membrane using a condensable curable silicone resin composition. However, its low strength makes it difficult to fabricate the membrane. Furthermore, because it is a wet-curable composition, curing takes a long time, and it is not suitable for cost-effective methods of continuously forming gas separation membranes.
[0010] As described above, there is a need for a resin for adhesives that is readily and inexpensively available, possesses excellent strength and flexibility, is soluble in volatile solvents, and is suitable for continuous film formation. There is also a need for coating agent compositions applicable to continuous film formation.
[0011] Citation List
[0012] Patent Document 1: JP-A 2021-185233
[0013] Patent Document 2: JP-A 2010-222228
[0014] Patent Document 3: JP-A 2012-224777
[0015] Patent Document 4: WO 2017 / 179738
[0016] Patent Document 5: WO 2018 / 038027
[0017] Non-patent literature 1: PMBudd et al., J. Memb. Sci., 325, (2008), 851-860 Summary of the Invention
[0018] The object of the present invention is to provide a siloxane-modified polyurethane resin coating composition containing a resin acting as a starting material, which is easy to synthesize and provides a film with high resin physical properties (e.g., tensile strength and high air permeability), the film being formed in a simple manner by drying and solvent removal, since the resin acting as the starting material is soluble in volatile organic solvents.
[0019] The inventors have discovered that resin-containing coating compositions obtained by curing a siloxane-modified polyurethane resin composition having a specific composition can solve the above-mentioned problems. It is worth noting that, in this invention, the state of "resin soluble in volatile organic solvents" or "resin dissolved" includes a state in which the composition exhibits a transparent, light milky white, or milky white appearance when evaluated by visual observation.
[0020] In one aspect, the present invention provides a siloxane-modified polyurethane resin coating composition comprising the following components (A) and (B):
[0021] (A) Siloxane-modified polyurethane resin; and
[0022] (B) Volatile organic solvents with a boiling point of 180°C or less at 1 atmosphere (atm).
[0023] Component (A) is a cured product of a siloxane-modified polyurethane resin composition, comprising the following components (a) to (c):
[0024] (a) A hydroxyl-containing organosilicon compound having the following formula (1)
[0025] (R 1 3SiO 1 / 2 ) k (R 1 2SiO 2 / 2 ) p (R 1 SiO 3 / 2 ) q (SiO 4 / 2 ) r (1)
[0026] Where R 1 Each is independently a monovalent hydrocarbon group of 1 to 10 carbon atoms or a group selected from formulas (2) and (3) below, provided that all R 1 Two of the groups are groups with the following formula (2) or (3), where k, p, q and r are integers k>0, p≥0, q≥0 and r≥0, respectively, provided that k+p+q is an integer k+p+q≥2, and the arrangement of the siloxane units in parentheses is uncertain.
[0027]
[0028] In equation (2), R 4 It is either hydrogen or methyl, x is an integer from 0 to 4, y is 0 or 1, z is an integer from 0 to 6, when y is 1, x is an integer from 0 to 4, z is an integer from 1 to 6, and x+z is an integer from 1 to 10, and when y is 0, x is an integer from 0 to 4, z is an integer from 0 to 6, and x+z is an integer from 1 to 10.
[0029] In equation (3), R 2 Each is independently hydrogen or a group selected from: a monovalent hydrocarbon group with 1 to 5 carbon atoms and an alkoxy group with 1 to 5 carbon atoms; R 3 For hydrogen or methyl, s is an integer from 0 to 4, t is an integer from 2 to 4, u is a number from 1 to 3, and dashed lines represent valence bonds;
[0030] (b) Diisocyanate compounds having two isocyanate groups per molecule; and
[0031] (c) Organic compounds having two functional groups per molecule that can react with isocyanate groups.
[0032] The amounts of components (a) to (c) are: 1 mole of component (a), m moles of component (c), and (1+m)×(0.9 to 1.2) moles of component (b), where m is greater than 0.2 moles and less than 1.6 moles.
[0033] The content of component (B) is 50 to 98% by weight of the total coating composition.
[0034] Preferably, y in the group of formula (2) is 0.
[0035] Preferably, the group in formula (3) is a group having the following formula (3.1a), (3.2a), or (3.3a):
[0036]
[0037] Where t and u are defined as above, and the dashed line represents the valence bond.
[0038] Furthermore, preferably, component (b) has the following formula (7):
[0039] OCN-Q-NCO (7)
[0040] Q is a divalent hydrocarbon group having 1 to 20 carbon atoms.
[0041] In formula (7), Q is preferably a straight-chain or branched alkylene or an alkylene with an alicyclic structure.
[0042] Component (B) preferably contains oxygen atoms in its molecule and has a boiling point of 120°C or less at 1 atm.
[0043] The siloxane-modified polyurethane resin composition preferably further contains (d) a urethane curing catalyst.
[0044] In another aspect, the present invention provides a coating film formed from the above-described coating agent composition.
[0045] An article comprising the above-described coating is also provided.
[0046] Advantages of the present invention
[0047] The siloxane-modified polyurethane resin coating composition of the present invention can be provided in a low-cost manner using resins that can be synthesized in a simple way as starting materials. Furthermore, the resins serving as starting materials are soluble in volatile organic solvents, thus allowing for the easy and simple acquisition of smooth films with excellent air permeability, strength, and flexibility through drying and solvent removal. Detailed Implementation
[0048] The present invention will now be described in detail.
[0049] The siloxane-modified polyurethane resin coating composition of the present invention comprises the following components (A) and (B).
[0050] (A) Siloxane-modified polyurethane resin
[0051] (B) Volatile organic solvents with a boiling point of 180°C or less at 1 atm
[0052] Component (A):
[0053] Component (A) is a siloxane-modified polyurethane resin obtained by curing a siloxane-modified polyurethane resin composition containing the following components (a) to (c).
[0054] (1-1) Component (a):
[0055] Component (a) is a hydroxyl-containing organosilicon compound having the following formula (1).
[0056] (R 1 3SiO 1 / 2 ) k (R 1 2SiO 2 / 2 ) p (R 1 SiO 3 / 2 ) q (SiO 4 / 2 ) r (1)
[0057] In equation (1), R 1 Each is independently a monovalent hydrocarbon group of 1 to 10 carbon atoms or a group selected from formulas (2) and (3) below, provided that all R 1 Two of the groups are groups having the following formula (2) or (3).
[0058]
[0059] Here, the dashed line represents the price key.
[0060] In equation (1), R 1 The monovalent hydrocarbon group representing 1 to 10 carbon atoms can be straight-chain, branched, or cyclic, and is: an alkyl group with 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, more preferably 1 to 3 carbon atoms; a cycloalkyl group with 5 to 10 carbon atoms, preferably 5 to 8 carbon atoms; an aryl group with 6 to 10 carbon atoms, preferably 6 to 8 carbon atoms; or an aralkyl group with 7 to 10 carbon atoms.
[0061] By R 1Examples of monovalent hydrocarbon groups include: alkyl groups, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl; cycloalkyl groups, such as cyclopentyl and cyclohexyl; aryl groups, such as phenyl and tolyl; and aralkyl groups, such as benzyl and phenethyl.
[0062] Among them, R 1 Preferably, it is methyl, ethyl, or phenyl.
[0063] In equation (2), R 4 It is hydrogen or methyl, x is an integer from 0 to 4, y is 0 or 1, and z is an integer from 0 to 6, and when y is 1, x is an integer from 0 to 4, z is an integer from 1 to 6, x+z is an integer from 1 to 10, and when y is 0, x is an integer from 0 to 4, z is an integer from 0 to 6, and x+z is an integer from 1 to 10. Preferably, y is 0.
[0064] Examples of groups having formula (2) include, but are not limited to, those having the following formula. Among them, groups having formulas (2.2b), (2.4f), (2.4h), and (2.4k) are preferred.
[0065]
[0066] Here, the dashed line represents the price key.
[0067] In equation (3), R 2 Each is independently hydrogen or selected from the following groups: monovalent hydrocarbon groups with 1 to 5 carbon atoms and alkoxy groups with 1 to 5 carbon atoms.
[0068] By R 2 The monovalent hydrocarbon group represented, having 1 to 5 carbon atoms, can be straight-chain or branched, examples of which include those related to R. 1 The examples listed are similar to straight-chain or branched groups having 1 to 5 carbon atoms. Among them, methyl, isopropyl, and tert-butyl are preferred.
[0069] As a result of R 2 The alkoxy group represented has 1 to 5 carbon atoms, with alkoxy groups having 1 to 3 carbon atoms being preferred, and examples include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, and n-pentoxy. Among these, methoxy and ethoxy are preferred.
[0070] R 3 It is either hydrogen or methyl.
[0071] The subscript s is an integer from 0 to 4, preferably an integer from 0 to 2.
[0072] The subscript t is an integer from 2 to 4, preferably 2 or 3.
[0073] The subscript u is a number from 1 to 3. The repeating unit in parentheses with u can be a single chemically repeating unit or a combination of different repeating units, with an average value of 1 to 3. When u is 0, the group has a phenolic hydroxyl group, which leads to reduced reactivity to, for example, isocyanate groups. Therefore, u is defined as a number of 1 or greater. The case of u being 0 is not included when different repeating units are combined. Furthermore, when u is greater than 3, heat resistance decreases, so the case of u being greater than 3 is not included. Therefore, u is a number from 1 to 3. The repeating unit in parentheses with u is even more preferably a single chemically repeating unit.
[0074] Examples of groups having formula (3) include, but are not limited to, groups having the following formula.
[0075]
[0076] Here, t and u are defined as above. Dashed lines represent valence bonds.
[0077] Among them, groups having the following formulas (3.1a), (3.2a) and (3.3a) are preferred.
[0078]
[0079] Here, t and u are defined as above. Dashed lines represent valence bonds.
[0080] Examples of groups having formulas (3.1a), (3.2a), and (3.3a) include, but are not limited to, groups having the following formulas. Among them, groups having formulas (3.1a)-1, (3.2a)-1 to (3.2a)-5 and (3.3a)-1 are preferred.
[0081]
[0082]
[0083] Here, the dashed line represents the price key.
[0084] In equation (1), k, p, q and r are integers where k > 0, p ≥ 0, q ≥ 0 and r ≥ 0, provided that the sum k + p + q is an integer where k + p + q ≥ 2.
[0085] The subscript k is preferably an integer from 2 to 5, and more preferably an integer from 2 to 4.
[0086] The subscript p is preferably an integer from 2 to 100, and more preferably an integer from 5 to 80.
[0087] The subscript q is preferably an integer from 0 to 3, more preferably an integer from 0 to 2, and even more preferably 1 or 2.
[0088] The subscript r is preferably an integer from 0 to 3, more preferably 0 or 1, and even more preferably 0.
[0089] The sum k+p+q is preferably an integer k+p+q≥5, and more preferably an integer k+p+q≥8.
[0090] There are no particular restrictions on the arrangement of the siloxane units in parentheses, and the siloxane units can be randomly bonded or can form a block structure.
[0091] The hydroxyl-containing organosilicon compounds used in this invention preferably have the structure of formula (1), where k is an integer from 2 to 5, p is an integer from 2 to 100, q is an integer from 0 to 3, r is 0, and all R 1 Two of the groups are groups having formula (2) or (3). It is noteworthy that they can be used in all R groups. 1 The group contains three or more hydroxyl-containing organosilicon compounds having formula (2) or (3), provided that the solubility of the siloxane-modified polyurethane resin in volatile organic solvents is not impaired.
[0092] Particularly preferred examples of hydroxyl-containing organosilicon compounds include: all R 1 Organosilicon compounds containing two hydroxyl groups that have the above formula (2) or (3) and are only connected to the end of the molecular chain.
[0093] (1-2) Properties of component (a)
[0094] The weight-average molecular weight of the hydroxyl-containing organosilicon compounds used in this invention is preferably 400 to 15,000, more preferably 600 to 10,000, even more preferably 600 to 8,000, and still more preferably 600 to 6,000. It is worth noting that the weight-average molecular weight is a polystyrene equivalent value obtained by gel permeation chromatography (GPC) under the following conditions.
[0095] [Measurement Conditions]
[0096] Development solvent: Tetrahydrofuran (THF)
[0097] Flow rate: 0.6 mL / min
[0098] Detector: Differential Refractive Index Detector (RI)
[0099] Column: TSK Guard Column SuperH-H
[0100] TSKgel SuperHM-N(6.0mm ID×15cm×1)
[0101] TSKgel SuperH2500(6.0mm ID×15cm×1)
[0102] (All manufactured by Tosoh Corporation)
[0103] Column temperature: 40℃
[0104] Sample injection volume: 50 μL (THF solution, concentration 0.3% by weight)
[0105] The kinematic viscosity of the hydroxyl-containing organosilicon compound used in this invention is preferably 10 to 10,000 mm⁻¹. 2 / s, more preferably 20 to 5000 mm 2 / s. It is worth noting that kinematic viscosity was measured at 25°C using the Cannon Fenske viscometer described in JIS Z 8803:2011.
[0106] The average molecular weight, determined by the hydroxyl value according to JIS K 0070:1992, is preferably 400 to 15,000, more preferably 600 to 10,000, even more preferably 600 to 8,000, and even more preferably 600 to 6,000.
[0107] (1-3) Preparation method of component (a)
[0108] The hydroxyl-containing organosilicon compounds used in this invention can be obtained by hydrosilylating, for example, the following compounds: organohydropolysiloxanes having the following formula (4), and compounds having hydroxyl and aliphatic unsaturated groups having the following general formula (5) or (6).
[0109] (R 5 3SiO 1 / 2 ) k (R 5 2SiO 2 / 2 ) p (R 5 SiO 3 / 2 ) q (SiO 4 / 2 ) r (4)
[0110]
[0111] As an organohydrogen polysiloxane, an organohydrogen polysiloxane having the following formula (4) can be used.
[0112] (R 5 3SiO 1 / 2 ) k (R 5 2SiO 2 / 2 ) p (R5 SiO 3 / 2 ) q (SiO 4 / 2 ) r (4)
[0113] In equation (4), R 5 Each is independently hydrogen or a monovalent hydrocarbon group having 1 to 10 carbon atoms, provided that all R 5 Two of the groups are hydrogen atoms.
[0114] By R 5 Examples of monovalent hydrocarbon groups represented by R 1 As illustrated, and among these, methyl, ethyl and phenyl are preferred.
[0115] The subscripts k, p, q, and r are defined in the same way as above.
[0116] There are no particular restrictions on the arrangement of the siloxane units in parentheses, and the siloxane units can be randomly bonded or can form a block structure.
[0117] The organohydrogen polysiloxane used here preferably has the structure of formula (4), where k is an integer from 2 to 5, p is an integer from 2 to 100, q is an integer from 0 to 3, r is 0, and all R 5 Two of the groups are preferably hydrogens. Particularly preferred examples of organohydrogen polysiloxanes include those that have only two hydrogens attached to the ends of the molecular chain.
[0118] It is worth noting that organohydrogen polysiloxanes containing three or more hydrogen atoms can be used, as long as the solubility of the siloxane-modified polyurethane resin to be obtained in volatile organic solvents is not impaired.
[0119] Examples of organohydropolysiloxanes having formula (4) include: 1,1,3,3-tetramethyldisiloxane; dimethylpolysiloxanes end-capped with dimethylhydrosiloxanes at both ends of the molecular chain; dimethylsiloxane-diphenylsiloxane copolymers end-capped with dimethylhydrosiloxanes at both ends of the molecular chain; methylhydropolysiloxanes end-capped with dimethylhydrosiloxanes at one end of the molecular chain; methylhydrosiloxane-dimethylsiloxane copolymers end-capped with dimethylhydrosiloxanes at one end of the molecular chain; methylhydrosiloxane-diphenylsiloxane copolymers end-capped with dimethylhydrosiloxanes at one end of the molecular chain; methylhydrosiloxane-dimethylsiloxane-diphenylsiloxane copolymers end-capped with dimethylhydrosiloxanes at one end of the molecular chain; and (CH3)3SiO 1 / 2 Unit, (CH3)2HSiO 1 / 2 unit, (CH3)2SiO unit and CH3SiO 3 / 2A copolymer of units; containing (CH3)2HSiO 1 / 2 unit, (CH3)2SiO unit and CH3SiO 3 / 2 A copolymer of units; containing (CH3)2HSiO 1 / 2 unit, (C6H5)2SiO unit, (CH3)2SiO unit and CH3SiO 3 / 2 A copolymer of units; containing (CH3)(C6H5)HSiO 1 / 2 unit, (CH3)2SiO unit and CH3SiO 3 / 2 copolymers containing (CH3)2HSiO 1 / 2 (CH3)2SiO unit and C6H5SiO 3 / 2 Copolymers of units. These can be used alone or in combination of two or more.
[0120] Compounds having hydroxyl and aliphatic unsaturated groups can have the following formula (5) or (6).
[0121]
[0122] In equation (5), R 4 x, y, and z are defined the same as above. In equation (6), R 2 R 3 , s, t and u are the same as defined above.
[0123] Examples of groups having formula (5) include, but are not limited to, those having the following formula. Among them, groups having formulas (5.2b), (5.4f), (5.4h), and (5.4k) are preferred.
[0124]
[0125] Examples of groups having formula (6) include, but are not limited to, groups having the following formula.
[0126]
[0127] Here, t and u are the same as defined above.
[0128] Among them, groups having the following formulas (6.1a), (6.2a) and (6.3a) are preferred.
[0129]
[0130] Here, t and u are the same as those defined above.
[0131] Examples of groups having formulas (6.1a), (6.2a), and (6.3a) include, but are not limited to, groups having the following formulas. Among them, groups having formulas (6.1a)-1, (6.2a)-1 to (6.2a)-5 and (6.3a)-1 are preferred.
[0132]
[0133] Compounds of formula (6) having hydroxyl and aliphatic unsaturated groups can be obtained, for example, by the following methods.
[0134] When using phenolic compounds containing an allyl group in the molecule, such as o-allylphenol or eugenol (2-methoxy-4-allylphenol), which are readily available as commercial products, as starting materials, the compound can be obtained by adding a predetermined amount of ethylene oxide, propylene oxide, butylene oxide, tetrahydrofuran, or a mixture thereof to the phenolic hydroxyl group via methods known in the art.
[0135] Furthermore, for example, when using phenolic compounds such as phenol, 2,6-dimethylphenol, 2,4-di-tert-butylphenol, or 2,6-di-tert-butylphenol as starting materials, firstly, allyl halides such as allyl bromide, allyl chloride, or methyl allyl chloride are reacted with these phenolic compounds under alkaline conditions by methods known in the art to obtain allyl (or methyl allyl) phenyl ethers.
[0136] Subsequently, an allyl thermal rearrangement reaction is carried out to obtain allylated (or methylallylated) phenol, which is then subjected to an addition reaction with a predetermined amount of any one or a mixture of ethylene oxide, propylene oxide, butane oxide, tetrahydrofuran, etc., to obtain the compound in the same manner as described above.
[0137] The thermal rearrangement reaction of allyl groups occurs at the ortho or para position. Therefore, in order to obtain a product of high purity, it is more preferable to use a compound with a vacancy at only one of the ortho or para positions, such as 2,6-dimethylphenol, 2,4-di-tert-butylphenol, or 2,6-di-tert-butylphenol.
[0138] In the reaction between the organohydrogen polysiloxane of formula (4) and the compound having hydroxyl and aliphatic unsaturated groups of formula (5) or (6), although there is no particular limitation on the amount of the compound having hydroxyl and aliphatic unsaturated groups to be reacted, it is preferred that the molar number of the aliphatic unsaturated group (allyl or methylallyl) of the compound having hydroxyl and aliphatic unsaturated groups is in excess relative to the molar number of the hydrosilyl group of the organohydrogen polysiloxane.
[0139] For example, the molar ratio of aliphatic unsaturated groups per mole of hydrosilyl group is preferably 1 to 5 moles, more preferably 1 to 2 moles, and even more preferably 1 to 1.5 moles. If this ratio is less than 1 mole, the number of aliphatic unsaturated groups is insufficient, and dehydrogenation may occur. On the other hand, if this ratio is greater than 5 moles, a large amount of unreacted material of the compound having hydroxyl and aliphatic unsaturated groups remains in the reaction system, which may be uneconomical.
[0140] The hydrosilylation reaction between the organohydropolysiloxane of formula (4) and the compound of formula (5) or (6) having hydroxyl and aliphatic unsaturated groups is preferably carried out in the presence of a catalyst. There are no particular limitations on the catalyst, and conventionally known addition reaction catalysts can be used.
[0141] Examples of catalysts include platinum group metals such as platinum (including platinum black), palladium, rhodium, and ruthenium, as well as metal catalysts containing these platinum group metals, gold, nickel, cobalt, etc. Among them, metal catalysts containing platinum, palladium, or rhodium are preferred.
[0142] Examples of catalysts containing platinum, palladium, or rhodium include: PtCl4, H2PtCl6·6H2O, Pt-ether complexes, Pt-olefin complexes, PdCl2(PPh3)2, PdCl3(PhCN)2, RhCl2(PPh3)3 (in the above formula, Ph is phenyl), and complexes of platinum chloride, chloroplatinic acid, or chloroplatinate with vinyl-containing siloxanes. These catalysts can be used alone or in mixtures of two or more.
[0143] Among them, a metal catalyst containing platinum is preferred, and the Karstedt catalyst (a complex of the sodium bicarbonate neutralization product of 1,1,3,3-tetramethyl-1,3-divinyldisiloxane and chloroplatinic acid) is even more preferred.
[0144] These catalysts can be used after dilution with solvents such as alcohols, aromatic compounds, hydrocarbons or ketones when necessary.
[0145] There is no particular limitation on the amount of catalyst, as long as it is a catalytic amount. Here, catalytic amount refers to an amount sufficient to allow the addition reaction to proceed, and is preferably less than 0.02 parts by weight, more preferably 0.00001 to 0.02 parts by weight, even more preferably 0.0001 to 0.01 parts by weight, and even more preferably 0.0003 to 0.005 parts by weight, relative to 100 parts by weight of organohydrogen polysiloxane based on the atomic weight of the main metal of the metal catalyst.
[0146] The full amount of catalyst can be added at the start of the reaction, or it can be added multiple times during the reaction. Even with a small amount of catalyst, the reaction can proceed sufficiently. However, if the amount of catalyst is too small, the reaction rate may be too slow; therefore, the amount of catalyst is preferably equal to or greater than the lower limit mentioned above. Furthermore, if the amount of catalyst is too large, the reaction rate is not significantly improved, which may be uneconomical.
[0147] The large amount of residual metal catalyst in the hydroxyl-containing organosilicon compound (hydroxyl-containing siloxane) obtained as component (a) can cause discoloration. Therefore, the amount of residual metal catalyst is preferably small. In the preparation method of the present invention, the amount of metal catalyst contained in the hydroxyl-containing siloxane to be obtained is preferably 0.02 parts by weight or less, more preferably 0.01 parts by weight or less, and even more preferably 0.005 parts by weight or less, based on the conversion amount of major metal atoms per 100 parts by weight of siloxane.
[0148] After the addition reaction is complete, the remaining metal catalyst can be adsorbed and removed by activated carbon or other materials.
[0149] In the hydrosilylation reaction between organohydrogen polysiloxanes and compounds having hydroxyl and aliphatic unsaturated groups in this invention, solvents may be used if necessary.
[0150] Examples of solvents include alcohols, such as ethanol and 2-propanol; aromatic hydrocarbons, such as toluene, xylene, and benzene; aliphatic hydrocarbons, such as hexane, cyclohexane, methylcyclohexane, and ethylcyclohexane; halogenated hydrocarbons, such as chloroform, dichloromethane, and carbon tetrachloride; ethers, such as tetrahydrofuran (THF) and diethyl ether; ketones, such as acetone and methyl ethyl ketone; dimethylformamide (DMF); and acetonitrile.
[0151] The reaction temperature for hydrosilylation is preferably 20 to 200°C, more preferably 40 to 180°C, and even more preferably 60 to 150°C. The reaction time is preferably within 20 hours, more preferably within 12 hours, and even more preferably within 8 hours.
[0152] (2) Component (b)
[0153] Component (b) is a diisocyanate compound having two isocyanate groups per molecule. Component (b) is not particularly limited as long as it has two isocyanate groups per molecule, and examples include those having the following formula (7).
[0154] OCN-Q-NCO (7)
[0155] Here, Q is a divalent hydrocarbon group with 1 to 20 carbon atoms.
[0156] Examples of divalent hydrocarbon groups of Q include: linear or branched alkylene groups preferably having 1 to 15 carbon atoms, more preferably 1 to 10 carbon atoms, and even more preferably 1 to 8 carbon atoms; cycloalkylene groups preferably having 3 to 10 carbon atoms, more preferably 3 to 6 carbon atoms; alkylene groups comprising an alicyclic structure preferably having 4 to 15 carbon atoms, more preferably 4 to 13 carbon atoms; arylene groups preferably having 6 to 15 carbon atoms, more preferably 6 to 10 carbon atoms; arylalkylene groups preferably having 7 to 15 carbon atoms, more preferably 7 to 13 carbon atoms; and groups obtained by combining these groups.
[0157] Wherein, Q is preferably a straight-chain or branched alkylene, an alkylene with an alicyclic structure, or an arylalkylene, and more preferably a straight-chain or branched alkylene or an alkylene with an alicyclic structure.
[0158] Examples of alkylene compounds include methylene, ethylene, trimethylene, propylene, tetramethylene, pentamethylene, hexamethylene, heptamethylene, octamethylene, nonamethylene, decamethylene, dodecylene, and tetradecylene.
[0159] Examples of cycloalkylene compounds include cyclopentylene and cyclohexylene.
[0160] The alkylene group having an alicyclic structure is preferably an alkylene group having a saturated alicyclic structure, and examples of such alkylene groups include methylenecyclohexylene, methylene biscyclohexylene, (1,3-cyclohexanediyl)bismethylene and (1,4-cyclohexanediyl)bismethylene.
[0161] Examples of aryl groups include phenylene and naphthylene.
[0162] Examples of arylene alkyl groups include methylene phenylene and methylene diphenylene.
[0163] It also includes the aforementioned groups in which some or all of the hydrogen atoms are replaced by other substituents, examples of which include: alkyl groups with 1 to 3 carbon atoms, such as methyl and ethyl; alkoxy groups with 1 to 3 carbon atoms, such as methoxy and ethoxy; halogen atoms, such as chlorine and bromine; and carboxyl groups.
[0164] Examples of diisocyanate compounds having formula (7) include: diisocyanate compounds such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, m-phenylene diisocyanate, terephthalene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 3,3'-dimethyl-4,4'-biphenyl diisocyanate, 3,3'-dimethoxy-4,4'-biphenyl diisocyanate, 3,3'-dichloro-4,4'-biphenyl diisocyanate, 1,5-naphthalene diisocyanate, 1,5-tetrahydronaphthalene diisocyanate, tetramethylene Diisocyanate, 1,6-hexamethylene diisocyanate, dodecamethyl diisocyanate, trimethylhexamethylene diisocyanate, 1,3-cyclohexene diisocyanate, 1,4-cyclohexene diisocyanate, phenyl dimethyl diisocyanate, tetramethylphenyl dimethyl diisocyanate, hydrogenated phenyl dimethyl diisocyanate, lysine diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 3,3'-dimethyl-4,4'-dicyclohexylmethane diisocyanate, cyclohexane-1,3-dimethylbis(methylene) diisocyanate, and cyclohexane-1,4-dimethylbis(methylene) diisocyanate.
[0165] Component (b) can be used alone or in combination of two or more. Notably, compounds having three or more isocyanate groups per molecule can be included, provided that the solubility of the resulting resin in volatile organic solvents is not impaired.
[0166] Preferred examples include 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 1,6-hexamethylene diisocyanate, phenyl dimethyl diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and cyclohexane-1,4-dimethylbis(methylene) diisocyanate. More preferred examples include 1,6-hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and cyclohexane-1,4-dimethylbis(methylene) diisocyanate.
[0167] Although there is no particular limitation on the amount of component (b) added, it is preferably 1 to 50 parts by weight relative to 100 parts by weight of component (a).
[0168] (3) Component (c)
[0169] Component (c) is an organic compound having two or more functional groups per molecule that are capable of reacting with isocyanate groups. Examples of functional groups capable of reacting with isocyanate groups include hydroxyl, amino, carboxyl, and mercapto groups. Component (c) is not particularly limited, as long as it has two or more functional groups per molecule, but compounds having hydroxyl or amino groups are preferred.
[0170] Examples of component (c) include polyols (diols), such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,2-butanediol, 2,3-butanediol, 1,5-pentanediol, 1,4-pentanediol, 1,3-pentanediol, 1,2-pentanediol, 2,5-pentanediol, 2,4-pentanediol, 2,3-pentanediol, and 1,6-hexanediol. 1,5-hexanediol, 1,4-hexanediol, 1,3-hexanediol, 1,2-hexanediol, 2,6-hexanediol, 2,5-hexanediol, 2,4-hexanediol, 2,3-hexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanediol (1,4-dihydroxymethylcyclohexane), 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, neopentyl glycol, and methylpentyl glycol.
[0171] It is worth noting that, unlike component (a), the polyol described herein is a polyol with a low molecular weight and no silicon atoms, and preferably a polyol with a weight average molecular weight of less than 400.
[0172] In addition, examples include trifunctional alcohols, such as glycerol and trimethylolpropane; tetrafunctional alcohols, such as pentaerythritol and α-methyl glycosides; hexafunctional alcohols, such as sorbitol and sucrose; alkanolamines, such as monoethanolamine, diethanolamine, and triethanolamine; and diamines, such as ethylenediamine, diaminotoluene, diphenylmethanediamine, 4,4'-diaminodiphenylmethane, 3,3'-dichloro-4,4'-diaminodiphenylmethane, and 4,4'-methylenebis(2,6-diphenylmethane). Ethylaniline), 4,4'-methylenebis(2-ethyl-6-methylaniline), diethylmethylphenylenediamine, 4,6-diethyl-2-methyl-1,3-phenylenediamine, 2-methyl-4,6-bis(methylthio)-1,3-phenylenediamine, 4-methyl-2,6-bis(methylthio)-1,3-phenylenediamine, bis(4-amino-2,3-dichlorophenyl)methane (TCDAM), trimethylenebis(4-aminobenzoate) and isophorone diamine.
[0173] It also includes organopolysiloxanes with amino groups at both ends of the molecular chain, such as dimethylpolysiloxane with amino groups at both ends of the molecular chain.
[0174] These can be used individually, or two or more can be used in combination.
[0175] Among them, 1,4-butanediol, 1,9-nonanediol, 1,4-dihydroxymethylcyclohexane, 4,4'-diaminodiphenylmethane and isophorone diamine are preferred.
[0176] It is worth noting that compounds with three or more functional groups per molecule capable of reacting with isocyanate groups can be included, as long as the solubility of the resin to be obtained in volatile organic solvents is not impaired.
[0177] Although there is no particular limitation on the amount of component (c) added, it is preferred to be 0.1 to 10 parts by weight relative to 100 parts by weight of component (a).
[0178] The amounts of components (a) to (c) contained in the siloxane-modified polyurethane resin composition are: 1 mole of a hydroxyl-containing organosilicon compound as component (a), m moles of an organic compound as component (c), and (1+m)×(0.9 to 1.2) moles of a diisocyanate compound as component (b).
[0179] If the molar ratio of component (b) is less than (1+m)×0.9 mol, the molecular weight of the siloxane-modified polyurethane resin decreases, and the strength and elongation of the resin become insufficient. If the molar ratio is greater than (1+m)×1.2 mol, the residual amount of unreacted isocyanate groups increases. This molar ratio is preferably (1+m)×(0.95 to 1.1) mol, more preferably (1+m)×(0.98 to 1.05) mol, and even more preferably (1+m)×(1 to 1.05) mol.
[0180] Typically, to improve the solubility of the desired resin in organic solvents, it is considered preferable to increase the ratio of the hydroxyl-containing organosilicon compound of component (a) to the total amount of components (a) to (c) contained in the siloxane-modified polyurethane resin composition. However, in this invention, it has been found that the resin becomes soluble in organic solvents when the molar ratio (m) of the organic compound as component (c), rather than the molar ratio of component (a), is 0.2 moles or more and less than 1.6 moles. This molar ratio is preferably 1.5 or less, more preferably 1.4 or less.
[0181] The strength and elongation of siloxane-modified polyurethane resin decrease as m decreases. Therefore, the lower limit of m is preferably 0.4 mol or more, and more preferably 0.5 mol or more.
[0182] (4)(d) Carbamate curing catalyst
[0183] In addition to components (a) to (c), the siloxane-modified polyurethane resin composition used in this invention preferably contains (d) a urethane curing catalyst.
[0184] Component (d) promotes the reaction between the isocyanate group of component (b) and the hydroxyl group of component (a) and the isocyanate reactive group of component (c).
[0185] Examples of urethane curing catalysts include amine compounds such as triethylamine, N,N-dimethylcyclohexylamine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethylhexamethylenediamine, N,N,N',N",N"-pentamethyldiethylenetriamine, N,N,N',N",N"-pentamethyldipropylenetriamine, triethylenediamine, N-methyl-N'-(2-dimethylaminoethyl)piperazine, N-ethylmorpholine, 1,2-dimethylimidazolium, dimethylethanolamine, dimethylaminoethoxyethanol, N,N,N'- Trimethylaminoethylethanolamine, N-methyl-N'-(2-hydroxyethyl)piperazine, bis(2-dimethylaminoethyl) ether; organotitanium compounds, such as tetraisopropoxytitanium, tetra-n-butoxytitanium, tetra-tert-butoxytitanium, diisopropoxybisacetylacetone titanium complex; tetra-2-ethylhexanoltitanium, diisopropoxybis(ethylacetoacetate)phthalide; organozirconium compounds, such as tetrabutoxyzirconium, tetrapropoxyzirconium, tetra(2,4-pentanedione)zirconium, dibutoxybis(ethylacetoacetate)zirconium; and organotin compounds, such as dibutyltin diacetate and dibutyltin dilaurate.
[0186] Organozzirconium compounds are preferred, and tetra(2,4-pentanedione)zirconium is more preferred.
[0187] When mixing component (d), although there is no particular limitation on the amount added and it is typically within the range used to prepare polyurethane resins, it is preferably 1 to 1000 ppm, more preferably 10 to 500 ppm, relative to the total weight of components (a) to (c).
[0188] (5) Other components
[0189] In the siloxane-modified polyurethane resin composition of the present invention, other components may be mixed in addition to components (a) to (c) and optional component (d), as long as the advantageous effects of the present invention are not impaired. Examples of other components include polyols, antioxidants, ultraviolet absorbers, and light stabilizers other than component (c).
[0190] Examples of polyols include, for example, hydroxyl-containing polymer components, such as polyether polyols, polyester polyols, and polycarbonate polyols. Examples include polyethylene glycol, polypropylene glycol, polyethylene glycol-tetramethylene glycol, polytetramethylene ether glycol, polytetramethylene glycol, and polyhexamethylene glycol, which are obtained by polymerizing or copolymerizing alkylene oxides or cyclic ethers. It is noteworthy that, unlike component (a), the polyols mentioned herein do not contain silicon atoms and, unlike the polyols exemplified in component (c), preferably have a weight-average molecular weight of 400 to 15,000.
[0191] Examples of antioxidants include hindered phenolic antioxidants, amine antioxidants, phosphorus antioxidants, and sulfur antioxidants.
[0192] Examples of ultraviolet absorbers include benzotriazole-type ultraviolet absorbers, triazine-type ultraviolet absorbers, benzophenone-type ultraviolet absorbers, and benzoic acid ester-type ultraviolet absorbers.
[0193] Examples of light stabilizers include hindered amine light stabilizers.
[0194] A siloxane-modified polyurethane resin composition containing the above components (a) to (c), optional component (d), and other components can be obtained by mixing the above components according to conventional methods. Other components may be added at any time.
[0195] (6) Preparation method of component (A)
[0196] The preparation method (synthesis method) of the (A) siloxane-modified polyurethane resin contained in the coating composition of the present invention is not particularly limited, and conventional methods for preparing polyurethane resins can be adopted, including the prepolymer method and the one-step method.
[0197] In the prepolymer method, components (a) and (b) are first reacted. The reaction temperature is preferably 10 to 250°C, more preferably 20 to 150°C, and even more preferably 50 to 120°C. The reaction time is preferably 10 minutes to 10 hours, more preferably 30 minutes to 5 hours. Then, component (c) is further reacted. The reaction temperature and time are the same as described above.
[0198] The one-step process involves reacting components (a), (b), and (c) simultaneously. The reaction temperature is preferably 10 to 250°C, more preferably 20 to 150°C, and even more preferably 50 to 120°C. The reaction time is preferably 10 minutes to 10 hours, more preferably 30 minutes to 5 hours.
[0199] When (d) urethane curing catalyst is added as an optional component, in the case of the prepolymer method, it is preferable to add the urethane curing catalyst in the first stage of reacting components (a) and (b), while in the case of the one-step method, it is preferable to add the urethane curing catalyst when components (a), (b) and (c) react simultaneously.
[0200] The siloxane-modified polyurethane resin composition is preferably a composition that can be cured to form a thermoplastic resin or elastomer.
[0201] While the weight-average molecular weight of the thus obtained component (A) is not particularly limited, it is preferably from 50,000 to 500,000. It is worth noting that the weight-average molecular weight of component (A) is a polystyrene equivalent value obtained by GPC, and the measurement method is the same as that described with respect to component (a).
[0202] While there is no particular limitation on the amount of siloxane in component (A), it is preferably 65 to 98% by weight, more preferably 70 to 97% by weight. It should be noted that in this invention, the amount of siloxane in component (A) is defined as the content ratio of component (a) to the total weight of components (a) to (c) contained in the resin composition before curing.
[0203] While the tensile strength of component (A) is not particularly limited, it is preferably from 0.1 to 30 MPa. While the elongation at break is not particularly limited, it is preferably from 50 to 1000%.
[0204] Furthermore, while there are no particular limitations on the gas permeability coefficient of component (A), in the case of carbon dioxide, it is preferably 500 to 4000 Barrer.
[0205] It is worth noting that the methods used to measure tensile strength, elongation at break, and gas permeability are described in the examples below.
[0206] Component (B)
[0207] Component (B) is a volatile organic solvent having a boiling point of 180°C or lower at 1 atm. Examples of component (B) include ketones, such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ethers, such as tetrahydrofuran and ethylene glycol dimethyl ether; amides, such as dimethylformamide and dimethylacetamide; alcohols, such as ethanol and 2-propanol; aromatics, such as toluene and xylene; aliphatic hydrocarbons, such as cyclohexane and methylcyclohexane; halogenated hydrocarbons, such as chloroform, dichloromethane, and carbon tetrachloride; esters, such as ethyl acetate and butyl acetate; and nitriles, such as acetonitrile.
[0208] Component (B) preferably contains one or more heteroatoms selected from oxygen, nitrogen, and halogens in its molecule. Component (B) is more preferably containing an oxygen atom in its molecule and having a boiling point of 120°C or lower at 1 atm. It is even more preferably an ether, such as tetrahydrofuran and ethylene glycol dimethyl ether, and even more preferably tetrahydrofuran.
[0209] The content of volatile organic solvent in component (B) is 50 to 98% by weight of the total coating composition. If the content is less than 50% by weight, the viscosity of the composition is too high. If the content is greater than 98% by weight, it is uneconomical. The content is preferably 60 to 95% by weight, more preferably 70 to 95% by weight, even more preferably 80 to 95% by weight, and even more preferably 85 to 95% by weight.
[0210] In the coating composition of the present invention, additives typically used in coating compositions and known in the art, such as antioxidants, ultraviolet absorbers and light stabilizers, may be incorporated, provided that the advantageous effects of the present invention are not impaired.
[0211] Preparation method of coating agent composition
[0212] The method for obtaining the coating composition of the present invention, containing a siloxane-modified polyurethane resin as component (A) and a volatile organic solvent as component (B), is not particularly limited, but examples include the following method: wherein components (A) and (B) are mixed, and then the mixture is heated to a temperature equal to or below the boiling point of the component (B) to be dissolved. The heating conditions are, for example, preferably 40 to 100°C, more preferably 50 to 80°C, and preferably 0.5 to 10 hours, and more preferably 1 to 5 hours.
[0213] When synthesizing component (A), component (B) can be mixed and obtained as a solution. However, in order to increase the molecular weight of the resin so that the resin exhibits its original strength and elongation, it is preferable to heat and cure components (a) to (c) to obtain the resin, and then add the volatile organic solvent (B) to dissolve the resin at a predetermined concentration.
[0214] Coated film or resin film
[0215] The siloxane-modified polyurethane resin coating composition of the present invention can provide a film in a simple manner by drying and removing volatile organic solvents, and can form a siloxane-modified polyurethane resin film with excellent air permeability, strength and elongation.
[0216] There are no particular limitations on the substrates on which the coating composition of the present invention is applied, and examples include plastic molded products, wood products, ceramics, glass and metals (such as stainless steel), and composites thereof, as well as substrates whose surfaces are treated with polytetrafluoroethylene or the like.
[0217] The coating method of the coating composition of the present invention can be suitably selected from conventionally known methods, and various coating methods can be used, such as bar coating, brush coating, spraying, dipping, flow coating, roller coating, curtain coating, spin coating and doctor blade coating.
[0218] After coating, drying is preferably carried out at room temperature (25°C) to 100°C for approximately 10 minutes to 20 hours to remove volatile organic solvents, thereby obtaining a siloxane-modified polyurethane resin film. If the temperature is below room temperature, the drying time may be too long, and if the temperature is above 100°C, bubbles may easily form.
[0219] Although there is no particular limitation on the thickness of the resulting film, it can be appropriately selected according to the intended use, and is preferably 1 to 500 μm, more preferably 10 to 200 μm.
[0220] Nevertheless, there are no particular limitations on the tensile strength, elongation at break, and gas permeability of the obtained siloxane-modified polyurethane resin film, but these can be within the same range as the values of the siloxane-modified polyurethane resin as component (A).
[0221] Example
[0222] Examples and comparative examples are given below by way of illustration rather than limitation.
[0223] In the following embodiments, performance evaluation is performed using the following methods.
[0224] Hydroxyl value was measured according to JIS K 0070:1992.
[0225] According to the method defined in JIS K 7312:1996, tensile strength and elongation at break were measured at a speed of 100 mm / min using a specimen obtained by stamping a dumbbell-shaped No. 6 specimen from a 1 mm thick cured product sheet.
[0226] The gas permeability coefficient was measured using a gas permeability measuring device (K-315N-01G) manufactured by Toyo Rika Co., Ltd. at a measurement temperature of 25°C.
[0227] The weight-average molecular weight of component (A) is the polystyrene equivalent value obtained by gel permeation chromatography (GPC) under the following conditions.
[0228] [Measurement Conditions]
[0229] Measuring device: HLC-8320GPC, manufactured by Tosoh Corporation.
[0230] Development solvent: Tetrahydrofuran (THF)
[0231] Flow rate: 0.6 mL / min
[0232] Detector: Differential Refractive Index Detector (RI)
[0233] Column: TSK Guard Column SuperH-H
[0234] TSKgel SuperHM-N(6.0mm ID×15cm×1)
[0235] TSKgel SuperH2500(6.0mm ID×15cm×1)
[0236] (All manufactured by Tosoh Corporation)
[0237] Column temperature: 40℃
[0238] Sample injection volume: 50 μL (THF solution, concentration 0.3% by weight)
[0239] Component (a) was synthesized in the same manner as disclosed in Examples 1 to 12 and Comparative Example 1 of Japanese Patent Application No. 2022-031383.
[0240] [1] Preparation of coating composition
[0241] Examples 1-1 to 1-3 and Comparative Examples 1-1 and 1-2
[0242] After purging the flask with nitrogen, hydroxyl-containing dimethyl polysiloxane (component (a)) and zirconium tetraacetylacetone (component (d)) as shown in Table 1 were added, followed by hexamethylene diisocyanate (component (b)). The mixture was stirred at 80°C for 2 hours. The mixture was cooled to below 35°C, and then 1,4-butanediol (component (c)) was added, followed by stirring for 5 minutes. The contents were then transferred to a polytetrafluoroethylene drum (hereinafter referred to as the drum) and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain siloxane-modified polyurethane resin (A). The weight-average molecular weight of the obtained resin (A) was measured.
[0243] The obtained resin block was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm, and the tensile strength and elongation at break were measured.
[0244] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding in a similar manner, and the permeability coefficient of carbon dioxide gas at 25 °C was measured.
[0245] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. The solubility of the composition was evaluated by visual observation.
[0246] The amount of component (b) is 1.02 times the total number of moles of components (a) and (c).
[0247] The results are shown in Table 1.
[0248] As shown in Table 1, when the amount of component (c) relative to component (a) is 1.6 mol or more, component (c) cannot be completely dissolved in THF at a concentration of 10 wt% (Comparative Examples 1-1 and 1-2).
[0249] Table 1
[0250]
[0251] (a) Polyol component a-3:
[0252] A hydroxyl-containing dimethyl polysiloxane having the following general formula (8) and an average molecular weight of 5343 as determined by the hydroxyl value.
[0253]
[0254] Here, n is a number corresponding to the molecular weight.
[0255] (b) Diisocyanate component HDI: Hexamethylene diisocyanate
[0256] (c) Diol component BD: 1,4-Butanediol
[0257] (d) Catalyst amount (ppm): Amount relative to the total amount of components (a), (b) and (c).
[0258] Amount of siloxane: The proportion (by weight) of component (a) among components (a), (b), and (c) that constitute the resin.
[0259] 1 bahl = 1 × 10 -6 cm 3 (STP)·cm / (cm 2 ·sec·cmHg)
[0260] THF solubility: The resin / tetrahydrofuran was mixed at a weight ratio of 10 / 90, stirred at 65°C for 3 hours, and then cooled to room temperature. The appearance of the composition was evaluated by visual observation according to the following standards.
[0261] ◎:Transparent solution
[0262] ○: Light milky white solution
[0263] ×: Some insoluble resin remains.
[0264] ××: The resin only swells and hardly dissolves.
[0265] *No measurements were taken because insoluble resin could be visually identified even at a concentration of 0.3% by weight.
[0266] Even when the concentration of the composition was reduced to 1% by weight of (A) resin / 99% by weight of (B) tetrahydrofuran, visual observation revealed that Comparative Example 1 was rated "×" and Comparative Example 2 was rated "××" for the solubility of the coating composition. The results indicate that this rating is the same as those at a concentration of 10% by weight, and no change in solubility was observed.
[0267] Examples 1-4 to 1-8
[0268] The components shown in Table 2 were mixed to obtain a siloxane-modified polyurethane resin (A) in the same manner as in Examples 1-1. The resulting resin (A) was then dissolved in THF (B) to obtain a coating composition.
[0269] The formulation standards, catalyst addition standards, and siloxane calculation methods for component (b) are the same as those in Examples 1-1.
[0270] Tensile strength, elongation at break, carbon dioxide gas permeability, and THF solubility were measured and evaluated in the same manner as in Examples 1-1. The results are shown in Table 2.
[0271] When comparing the resin composition and THF solubility, a correlation exists between the amount of siloxane and THF solubility, and it can be understood that solubility improves with increasing siloxane content.
[0272] However, when Comparative Examples 1-1 and 1-2 were compared with Examples 1-6 and 1-7, it was found that there was no correlation between the amount of siloxane and the solubility of THF, and that the solubility of THF depended on the molar ratio of component (c).
[0273] Table 2
[0274]
[0275] Polyol component a-3: Same as defined above. A hydroxyl-containing dimethyl polysiloxane having the general formula (8) and an average molecular weight of 5343 as determined by the hydroxyl value.
[0276] Polyol component a-2: a hydroxyl-containing dimethyl polysiloxane having the general formula (8) and an average molecular weight of 3300 as determined by the hydroxyl value.
[0277] Polyol component a-1: a hydroxyl-containing dimethyl polysiloxane having the general formula (8) and an average molecular weight of 1968 as determined by the hydroxyl value.
[0278] Polyol component a-0: a hydroxyl-containing dimethyl polysiloxane having the general formula (8) and an average molecular weight of 984 as determined by the hydroxyl value.
[0279] Examples 1-9
[0280] After purging the flask with nitrogen, 90.83 g of (a) polyol component a-3, 16.73 g of (a) polyol component a-0, and 0.006 g of (d) tetraacetylacetone zirconium were added, followed by 10.49 g of (b) hexamethylene diisocyanate. The resulting mixture was stirred at 80°C for 2 hours. The mixture was cooled to below 35°C, and then 2.45 g of (c) 1,4-butanediol was added, followed by stirring for 5 minutes. The mixture was then transferred to a vat and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain siloxane-modified polyurethane resin (A). The weight-average molecular weight of the resulting resin (A) was 137,000.
[0281] The resin formulation is as follows: polyol component a-3: polyol component a-0: hexamethylene diisocyanate: 1,4-butanediol = 0.5:0.5:1.836:0.8, in molar ratio. The amount of siloxane is 89.3% by weight.
[0282] The obtained resin was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm. The tensile strength and elongation at break were then measured. The results showed a tensile strength of 2.4 MPa and an elongation at break of 190%.
[0283] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding, and the permeability coefficient of carbon dioxide gas at 25 °C was measured. The resulting permeability coefficient was 2660 lbler.
[0284] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. Solubility was evaluated by visual observation, revealing that the composition exhibited a transparent appearance and that the resin dissolved.
[0285] Examples 1-10
[0286] After purging the flask with nitrogen, 105.60 g of (a) polyol component a-2 and 0.006 g of (d) tetraacetylacetone zirconium were added, followed by 9.87 g of (b) hexamethylene diisocyanate. The resulting mixture was stirred at 80 °C for 2 hours. The mixture was cooled to below 35 °C, and then 3.69 g of (c) 1,4-dihydroxymethylcyclohexane was added, followed by stirring for 5 minutes. The mixture was then transferred to a large container and heated at 120 °C for 24 hours under a nitrogen atmosphere to obtain siloxane-modified polyurethane resin (A). The weight-average molecular weight of the obtained resin (A) was 476,000.
[0287] The resin formulation is as follows: polyol component a-2: hexamethylene diisocyanate: 1,4-dihydroxymethylcyclohexane = 1.0:1.836:0.8, in molar ratio. The amount of siloxane is 88.6% by weight.
[0288] The obtained resin was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm. The tensile strength and elongation at break were then measured. The results showed a tensile strength of 8.9 MPa and an elongation at break of 970%.
[0289] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding, and the permeability coefficient of carbon dioxide gas at 25 °C was measured. The result was a permeability coefficient of 2440 lbler.
[0290] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. Solubility was evaluated by visual observation, revealing that the composition exhibited a transparent appearance and that the resin dissolved.
[0291] Examples 1-11
[0292] After purging the flask with nitrogen, 105.60 g of (a) polyol component a-2 and 0.006 g of (d) tetraacetylacetone zirconium were added, followed by 9.87 g of (b) hexamethylene diisocyanate. The resulting mixture was stirred at 80 °C for 2 hours. The mixture was cooled to below 35 °C, and then 4.10 g of (c) 1,9-nonanediol was added, followed by stirring for 5 minutes. The mixture was then transferred to a large container and heated at 120 °C for 24 hours under a nitrogen atmosphere to obtain siloxane-modified polyurethane resin (A). The weight-average molecular weight of the resulting resin (A) was 515,000.
[0293] The resin formulation is as follows: polyol component a-2: hexamethylene diisocyanate: 1,9-nonanediol = 1.0:1.836:0.8, in molar ratio. The amount of siloxane is 88.3% by weight.
[0294] The obtained resin was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm. The tensile strength and elongation at break were then measured. The results showed a tensile strength of 7.4 MPa and an elongation at break of 680%.
[0295] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding, and the permeability coefficient of carbon dioxide gas at 25 °C was measured. The resulting permeability coefficient was 2330 lbler.
[0296] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. Solubility was evaluated by visual observation, revealing that the composition exhibited a transparent appearance and that the resin dissolved.
[0297] Examples 1-12
[0298] After purging the flask with nitrogen, 102.30 g of (a) polyol component a-2 and 0.006 g of (d) tetraacetylacetone zirconium were added, followed by 14.23 g of (b) 4,4'-diphenylmethane diisocyanate. The mixture was stirred at 80 °C for 2 hours. The contents were cooled to below 35 °C, and then 2.23 g of (c) 1,4-butanediol was added, followed by stirring for 5 minutes. The contents were then transferred to a large container and heated at 120 °C for 24 hours under a nitrogen atmosphere to obtain siloxane-modified polyurethane resin (A). The weight-average molecular weight of the resulting resin (A) was 188,000.
[0299] The resin formulation is as follows: polyol component a-2: 4,4'-diphenylmethane diisocyanate: 1,4-butanediol = 1.0:1.836:0.8, in molar ratio. The amount of siloxane is 86.1% by weight.
[0300] The obtained resin was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm. The tensile strength and elongation at break were then measured. The results showed a tensile strength of 3.3 MPa and an elongation at break of 270%.
[0301] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding, and the permeability coefficient of carbon dioxide gas at 25 °C was measured. The result was a permeability coefficient of 2400 lbler.
[0302] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. Solubility was evaluated by visual inspection, revealing that the composition had a milky white appearance and that the resin dissolved.
[0303] Additionally, 5% by weight of resin (A) and 95% by weight of tetrahydrofuran (B) were mixed to obtain a coating composition. Solubility was evaluated by visual inspection, revealing that the composition exhibited a transparent appearance and that the resin dissolved.
[0304] Examples 1-13
[0305] After purging the flask with nitrogen, 112.20 g of (a) polyol component a-3 and 0.012 g of (d) tetraacetylacetone zirconium were added, followed by 6.48 g of (b) hexamethylene diisocyanate. The resulting mixture was stirred at 80 °C for 2 hours. The mixture was cooled to below 35 °C, and then 0.756 g of (c) 1,4-butanediol and 1.66 g of (c) 4,4'-diaminodiphenylmethane were added. The mixture was stirred for 5 minutes. The mixture was then transferred to a large container and heated at 120 °C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin (A). The weight-average molecular weight of the resulting resin (A) was 154,000.
[0306] The resin formulation is as follows: polyol component a-3: hexamethylene diisocyanate: 1,4-butanediol: 4,4'-diaminodiphenylmethane = 1.0:1.836:0.4:0.4, in molar ratio. The amount of siloxane is 92.7% by weight.
[0307] The obtained resin was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm. Tensile strength and elongation at break were then measured. The results showed a tensile strength of 2.9 MPa and an elongation at break of 740%.
[0308] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding, and the permeability coefficient of carbon dioxide gas at 25 °C was measured. The resulting permeability coefficient was 2890 lbler.
[0309] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. Solubility was evaluated by visual observation, revealing that the composition exhibited a transparent appearance and that the resin dissolved.
[0310] Examples 1-14
[0311] After purging the flask with nitrogen, 63.48 g of a (a) polyol component having the following general formula (9) and an average molecular weight of 1058 determined by the hydroxyl value, and 0.002 g of (d) zirconium tetraacetylacetone were added, along with 18.51 g of (b) hexamethylene diisocyanate. The mixture was stirred at 80°C for 2 hours. The contents were cooled to below 35°C, and then 4.32 g of (c) 1,4-butanediol was added, and the mixture was stirred for 5 minutes. The contents were then transferred to a large container and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin (A). The weight-average molecular weight of the resulting resin (A) was 69,100.
[0312] The resin formulation consists of the following polyol components: hexamethylene diisocyanate: 1,4-butanediol = 1.0:1.836:0.8, in a molar ratio. The amount of siloxane is 73.6% by weight.
[0313]
[0314] Here, n is a number corresponding to the molecular weight.
[0315] The obtained resin was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm. Tensile strength and elongation at break were then measured. The results showed a tensile strength of 16 MPa and an elongation at break of 510%.
[0316] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding, and the permeability coefficient of carbon dioxide gas at 25 °C was measured. The resulting permeability coefficient was 669 lbler.
[0317] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. Solubility was evaluated by visual inspection, revealing that the composition exhibited a light milky white appearance and that the resin dissolved.
[0318] Additionally, 5% by weight of resin (A) and 95% by weight of tetrahydrofuran (B) were mixed to obtain a coating composition. Solubility was evaluated by visual inspection, revealing that the composition exhibited a transparent appearance and that the resin dissolved.
[0319] Examples 1-15
[0320] After purging the flask with nitrogen, 85.71 g of a (a) polyol component having the following general formula (10) and an average molecular weight of 963 determined by the hydroxyl value, and 0.003 g of (d) tetraacetylacetone zirconium, and 27.45 g of (b) hexamethylene diisocyanate were added, and the mixture was stirred at 80°C for 2 hours. The contents were cooled to below 35°C, and then 6.41 g of (c) 1,4-butanediol was added, and the mixture was stirred for 5 minutes. The contents were then transferred to a large container and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin (A). The weight-average molecular weight of the resulting resin (A) was 195,000.
[0321] The resin formulation consists of the following polyol components: hexamethylene diisocyanate: 1,4-butanediol = 1.0:1.836:0.8, in molar ratio. The amount of siloxane is 71.7% by weight.
[0322]
[0323] Here, n is a number corresponding to the molecular weight.
[0324] The obtained resin was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm. Tensile strength and elongation at break were then measured. The results showed a tensile strength of 27 MPa and an elongation at break of 780%.
[0325] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding, and the permeability coefficient of carbon dioxide gas at 25 °C was measured. The result was a permeability coefficient of 711 lbler.
[0326] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. Solubility was evaluated by visual inspection, revealing that the composition exhibited a light milky white appearance and that the resin dissolved.
[0327] In addition, 5% by weight of (A) resin and 95% by weight of (B) tetrahydrofuran were mixed to obtain a coating composition. Solubility was evaluated by visual observation, and the composition was found to be transparent and the resin dissolved.
[0328] Examples 1-16
[0329] After purging the flask with nitrogen, 95.86 g of (a) polyol component a-1, 2.52 g of polyethylene glycol (molecular weight: 200), and 0.006 g of (d) tetraacetylacetone zirconium were added, along with 17.27 g of (b) hexamethylene diisocyanate. The mixture was stirred at 80°C for 2 hours. The contents were cooled to below 35°C, and then 3.40 g of (c) 1,4-butanediol was added, followed by stirring for 5 minutes. The contents were then transferred to a large container and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain siloxane-modified polyurethane resin (A). The weight-average molecular weight of the resulting resin (A) was 563,000.
[0330] The resin formulation is as follows: polyol component a-1: polyethylene glycol: hexamethylene diisocyanate: 1,4-butanediol = 0.8:0.2:1.632:0.6, in molar ratio. The amount of siloxane is 80.5% by weight.
[0331] The obtained resin was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm. Tensile strength and elongation at break were then measured. The results showed a tensile strength of 15 MPa and an elongation at break of 930%.
[0332] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding, and the permeability coefficient of carbon dioxide gas at 25 °C was measured. The resulting permeability coefficient was 1710 lbler.
[0333] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. Solubility was evaluated by visual observation, revealing that the composition exhibited a transparent appearance and that the resin dissolved.
[0334] Examples 1-17
[0335] After purging the flask with nitrogen, 101.64 g of (a) polyol component a-2, 2.67 g of polypropylene glycol (molecular weight: 202), and 0.006 g of (d) tetraacetylacetone zirconium were added, followed by 13.57 g of (b) hexamethylene diisocyanate, and the mixture was stirred at 80 °C for 2 hours. The contents were cooled to below 35 °C, and then 3.17 g of (c) 1,4-butanediol was added, and the mixture was stirred for 5 minutes. The contents were then transferred to a large container and heated at 120 °C for 24 hours under a nitrogen atmosphere to obtain siloxane-modified polyurethane resin (A). The weight-average molecular weight of the resulting resin (A) was 117,000.
[0336] The resin formulation is as follows: polyol component a-2: polypropylene glycol: hexamethylene diisocyanate: 1,4-butanediol = 0.7:0.3:1.836:0.8, in molar ratio. The amount of siloxane is 84.0% by weight.
[0337] The obtained resin was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm. The tensile strength and elongation at break were then measured. The results showed a tensile strength of 6.5 MPa and an elongation at break of 640%.
[0338] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding, and the permeability coefficient of carbon dioxide gas at 25 °C was measured. The resulting permeability coefficient was 2140 lbler.
[0339] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. Solubility was evaluated by visual observation, revealing that the composition exhibited a transparent appearance and that the resin dissolved.
[0340] Examples 1-18
[0341] After purging the flask with nitrogen, 105.92 g of a (a) polyol component having the following general formula (11) and an average molecular weight of 3310 determined by the hydroxyl value, 0.006 g of (d) tetraacetylacetone zirconium, and 9.87 g of (b) hexamethylene diisocyanate were added, and the mixture was stirred at 80°C for 2 hours. The contents were cooled to below 35°C, and then 2.30 g of (c) 1,4-butanediol was added, and the mixture was stirred for 5 minutes. The contents were then transferred to a large container and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin (A). The weight-average molecular weight of the resulting resin (A) was 297,000.
[0342] The resin formulation consists of the following polyol components: hexamethylene diisocyanate: 1,4-butanediol = 1.0:1.836:0.8, in molar ratio. The amount of siloxane is 89.7% by weight.
[0343]
[0344] Here, n is a number corresponding to the molecular weight.
[0345] The obtained resin was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm. The tensile strength and elongation at break were then measured. The results showed a tensile strength of 6.8 MPa and an elongation at break of 620%.
[0346] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding, and the permeability coefficient of carbon dioxide gas at 25 °C was measured. The result was a permeability coefficient of 2270 lbler.
[0347] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. Solubility was evaluated by visual observation, revealing that the composition exhibited a transparent appearance and that the resin dissolved.
[0348] Examples 1-19
[0349] After purging the flask with nitrogen, 98.83 g of (a) polyol component having general formula (11) and an average molecular weight of 3310 determined by hydroxyl value, and 0.006 g of (d) zirconium tetraacetylacetone were added, along with 16.85 g of (b) isophorone diisocyanate, and the mixture was stirred at 80°C for 2 hours. The contents were cooled to below 35°C, and then 6.25 g of (c) 1,4-dihydroxymethylcyclohexane was added, and the mixture was stirred for 5 minutes. The contents were then transferred to a large container and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain siloxane-modified polyurethane resin (A). The weight-average molecular weight of the resulting resin (A) was 491,000.
[0350] The resin formulation consists of polyol components: isophorone diisocyanate: 1,4-dihydroxymethylcyclohexane = 1.0:2.448:1.4, in molar ratio. The amount of siloxane is 81.1% by weight.
[0351] The obtained resin was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm. Tensile strength and elongation at break were then measured. The results showed a tensile strength of 12 MPa and an elongation at break of 740%.
[0352] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding, and the permeability coefficient of carbon dioxide gas at 25 °C was measured. The result was a permeability coefficient of 1750 lbler.
[0353] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. Solubility was evaluated by visual observation, revealing that the composition exhibited a transparent appearance and that the resin dissolved.
[0354] Examples 1-20
[0355] After purging the flask with nitrogen, 105.34 g of (a) polyol component having general formula (12) and an average molecular weight of 4580 determined by hydroxyl value and 0.012 g of (d) tetraacetylacetone zirconium were added, along with 9.37 g of (b) isophorone diisocyanate, and the mixture was stirred at 80 °C for 2 hours. The contents were cooled to below 35 °C, and then 30 mL of tetrahydrofuran and 3.13 g of (c) isophorone diamine were added, and the mixture was stirred for 5 minutes. The contents were then transferred to a large container and heated at 120 °C for 24 hours under a nitrogen atmosphere to obtain siloxane-modified polyurethane resin (A). The weight-average molecular weight of the resulting resin (A) was 59,000.
[0356] The resin formulation is as follows: polyol component: isophorone diisocyanate: isophorone diamine = 1.0:1.836:0.8, in molar ratio. The amount of siloxane is 89.4% by weight.
[0357]
[0358] Here, n is a number corresponding to the molecular weight.
[0359] The obtained resin was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm. Tensile strength and elongation at break were then measured. The results showed a tensile strength of 1.5 MPa and an elongation at break of 100%.
[0360] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding, and the permeability coefficient of carbon dioxide gas at 25 °C was measured. The result was a permeability coefficient of 2370 lbler.
[0361] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. Solubility was evaluated by visual observation, revealing that the composition exhibited a transparent appearance and that the resin dissolved.
[0362] Examples 1-21
[0363] After purging the flask with nitrogen, 99.00 g of (a) polyol component a-2 and 0.012 g of (d) tetraacetylacetone zirconium were added, followed by 19.24 g of (b) 4,4'-dicyclohexylmethane diisocyanate, and the mixture was stirred at 80 °C for 2 hours. The contents were cooled to below 35 °C, and then 3.78 g of (c) 1,4-butanediol was added, and the mixture was stirred for 5 minutes. The contents were then transferred to a large container and heated at 120 °C for 24 hours under a nitrogen atmosphere to obtain siloxane-modified polyurethane resin (A). The weight-average molecular weight of the resulting resin (A) was 124,000.
[0364] The resin formulation is as follows: polyol component a-2: 4,4'-dicyclohexylmethane diisocyanate: 1,4-butanediol = 1.0:2.448:1.4, in molar ratio. The amount of siloxane is 81.1% by weight.
[0365] The obtained resin was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm. The tensile strength and elongation at break were then measured. The results showed a tensile strength of 3.0 MPa and an elongation at break of 140%.
[0366] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding, and the permeability coefficient of carbon dioxide gas at 25 °C was measured. The result was a permeability coefficient of 2200 lbler.
[0367] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. Solubility was evaluated by visual observation, revealing that the composition exhibited a transparent appearance and that the resin dissolved.
[0368] Examples 1-22
[0369] After purging the flask with nitrogen, 106.86 g of (a) polyol component a-3, 5.06 g of polypropylene glycol (molecular weight: 1011), and 0.012 g of (d) tetraacetylacetone zirconium were added. 6.93 g of cyclohexane-1,4-dimethylbis(methylene) diisocyanate (Fortimo, manufactured by Mitsui Chemicals Co., Ltd.) having the following formula (13) and acting as component (b) was added, and the mixture was stirred at 80°C for 2 hours. The contents were cooled to below 35°C, and then 0.90 g of (c) 1,4-butanediol was added, and the mixture was stirred for 5 minutes. The contents were then transferred to a large container and heated at 120°C for 24 hours under a nitrogen atmosphere to obtain a siloxane-modified polyurethane resin (A). The weight-average molecular weight of the resulting resin (A) was 475,000.
[0370] The resin formulation is as follows: polyol component a-3: polypropylene glycol: cyclohexane-1,4-dimethylbis(methylene)diisocyanate: 1,4-butanediol = 0.8:0.2:1.428:0.4, in molar ratio. The amount of siloxane is 89.2% by weight.
[0371] [Cyclohexane-1,4-dimethylbis(methylene)diisocyanate]
[0372]
[0373] The obtained resin was molded at 210°C for 8 minutes under a molding pressure of 10 MPa to obtain a cured sheet with a thickness of 1 mm. The tensile strength and elongation at break were then measured. The results showed a tensile strength of 3.7 MPa and an elongation at break of 900%.
[0374] Similarly, sheets with a film thickness of 500 μm were prepared by compression molding, and the permeability coefficient of carbon dioxide gas at 25 °C was measured. The resulting permeability coefficient was 2460 lbler.
[0375] Furthermore, 10% by weight of resin (A) and 90% by weight of tetrahydrofuran (B) were mixed in this ratio to obtain a coating composition. Solubility was evaluated by visual observation, revealing that the composition exhibited a transparent appearance and that the resin dissolved.
[0376] [2] Preparation of coating film
[0377] Examples 2-1 to 2-22
[0378] Each coating composition obtained in Examples 1-1 to 1-22 was placed in a mold (17cm × 13cm × 0.2cm) with a stainless steel (SUS) surface coated with polytetrafluoroethylene and dried at room temperature (25°C) for 12 hours to obtain a coating film with a thickness of 150μm.
[0379] The tensile strength, elongation at break, and carbon dioxide permeability coefficient of the obtained coating film can be measured using the siloxane-modified polyurethane resins used in Examples 1-1 to 1-22, respectively.
Claims
1. A siloxane-modified polyurethane resin coating composition comprising the following components (A) and (B): (A) Siloxane-modified polyurethane resin; and (B) Volatile organic solvents with a boiling point of 180°C or less at 1 atm. Component (A) is a cured product of a siloxane-modified polyurethane resin composition, said composition comprising the following components (a) to (c): (a) A hydroxyl-containing organosilicon compound having the following formula (1) (R 1 3SiO 1 / 2 ) k (R 1 2SiO 2 / 2 ) p (R 1 SiO 3 / 2 ) q (SiO 4 / 2 ) r (1) Where R 1 Each is independently a monovalent hydrocarbon group of 1 to 10 carbon atoms or a group selected from formulas (2) and (3) below, provided that all R 1 Two of the groups are groups with the following formula (2) or (3), where k, p, q and r are integers k>0, p≥0, q≥0 and r≥0, respectively, provided that k+p+q is an integer k+p+q≥2, and the arrangement of the siloxane units in the parentheses is uncertain. In equation (2), R 4 It is either hydrogen or methyl, x is an integer from 0 to 4, y is 0 or 1, and z is an integer from 0 to 6. When y is 1, x is an integer from 0 to 4, z is an integer from 1 to 6, and x+z is an integer from 1 to 10. Also, when y is 0, x is an integer from 0 to 4, z is an integer from 0 to 6, and x+z is an integer from 1 to 10. In equation (3), R 2 Each is independently hydrogen or a group selected from: a monovalent hydrocarbon group with 1 to 5 carbon atoms and an alkoxy group with 1 to 5 carbon atoms; R 3 For hydrogen or methyl, s is an integer from 0 to 4, t is an integer from 2 to 4, u is a number from 1 to 3, and dashed lines represent valence bonds; (b) Diisocyanate compounds having two isocyanate groups per molecule; and (c) Organic compounds having two functional groups per molecule capable of reacting with isocyanate groups. in, The amounts of components (a) to (c) are: 1 mole of component (a), m moles of component (c), and (1+m)×(0.9 to 1.2) moles of component (b), where m is greater than 0.2 moles and less than 1.6 moles. The content of component (B) is 50 to 98% by weight of the total coating composition.
2. The coating composition according to claim 1, wherein y in the group of formula (2) is 0.
3. The coating composition according to claim 1, wherein the group of formula (3) is a group having the following formula (3.1a), (3.2a) or (3.3a): Where t is an integer from 2 to 4, u is a number from 1 to 3, and the dashed line represents the valence bond.
4. The coating composition according to claim 1, wherein component (b) has the following formula (7): Q is a divalent hydrocarbon group having 1 to 20 carbon atoms.
5. The coating composition according to claim 4, wherein in formula (7), Q is a straight-chain or branched alkylene or an alkylene having an alicyclic structure.
6. The coating composition according to claim 1, wherein component (B) contains oxygen atoms in its molecule and has a boiling point of 120°C or less at 1 atm.
7. The coating composition according to claim 1, wherein the siloxane-modified polyurethane resin composition further comprises (d) a urethane curing catalyst.
8. A coating film formed from the coating agent composition of claim 1.
9. An article comprising the coating of claim 8.
Citation Information
Patent Citations
gaming machines
JP2022031383A
Antithrombogenic elastomer, molded products of the same, and a process for manufacturing the same
US4528343A