A > 420 hb high heat damage resistance elastic wheel rim and its heat treatment method and production method

The wheel rim with ≥420HB high heat damage resistance for elastic wheels, prepared by specific chemical composition and heat treatment process, solves the problem of elastic wheels being easily damaged by heat under high axle load and high speed, and achieves high strength, wear resistance and heat damage resistance, thus extending the service life of the wheel.

CN117904535BActive Publication Date: 2026-11-24МААНЬШАНЬ АЙРОН ЭНД СТИЛ КО ЛТД
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410055894.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-15
Publication Date
2026-11-24
Estimated Expiration
2044-01-15

AI Technical Summary

Technical Problem

Existing elastic wheel hub materials are susceptible to heat damage under high axle loads and high speeds, leading to thermal expansion and thermal stress problems, which affect the wear resistance and service life of the wheel.

Method used

High heat-damage resistant elastic wheel rims with a strength of ≥420HB are prepared using specific chemical compositions and heat treatment processes. These processes include alloying of elements such as C, Si, Mn, Cr, Ni, Mo, Co, Zr, La, V, and Nb, combined with stress-relief annealing, austenite homogenization high-temperature normalizing, high-temperature quenching, double-liquid sub-temperature quenching, and multiple tempering treatments to form a fine martensite and lower bainite microstructure.

Benefits of technology

It improves the wheel rim's resistance to heat damage, wear resistance, and strength, reduces the impact of thermal stress, and extends the wheel's service life and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117904535B_ABST
    Figure CN117904535B_ABST
Patent Text Reader

Abstract

This invention discloses a wheel rim with ≥420HB high heat damage resistance and elasticity for wheels, along with its heat treatment and production methods. The wheel rim comprises the following chemical components: C, Si, Mn, Cr, Ni, Mo, Co, Zr, Nb, V, La, [N], and Al. It features high strength, high hardness, high corrosion resistance, and high heat damage resistance, exhibiting excellent strength and toughness properties. Its tensile strength is ≥1300MPa, yield strength is ≥1150MPa, impact energy at -60℃ (KV2) is ≥100J, rim wear limit Brinell hardness is ≥400HBW, the hardness variation of a single wheel rim cross-section is within 15HBW, and the rim fracture toughness at 0℃ is ≥120MPa. 1 / 2 The austenitic grain size of the steel is greater than or equal to 10.0.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of wheel rim technology, specifically relating to a wheel rim with ≥420HB high heat damage resistance and elasticity for wheels, as well as its heat treatment method and production method. Background Technology

[0002] With the development of urban light rail transit, noise generated by light rail vehicles operating on ground or elevated roads in urban areas has become a prominent problem. To address this issue, flexible wheels are widely used in light rail vehicles worldwide. A flexible wheel has an elastic unit installed between the wheel hub and the wheel rim, which elastically supports the wheel, effectively reducing curve noise, minimizing track impact, reducing wheel and rail wear, and extending the service life of the line and vehicles. The use of flexible wheels as an effective measure to reduce curve noise is widely applied in low-floor light rail trams, intercity trains, and subway vehicles.

[0003] From the perspective of transportation systems and the entire life cycle, it is economical. Flexible wheels have been used in trams, urban rail, and high-speed lines both domestically and internationally, and their reliability has been fully verified. As urban rail transit develops towards low noise, the demand for flexible composite wheels is increasing, and the quality requirements for flexible composite wheels are also becoming higher. It is necessary to ensure the shape, size, and assembly accuracy of each component, as well as the internal quality of the wheel rim and wheel core. The heat damage resistance and wear resistance of the wheel rim are particularly important.

[0004] With the increase in axle load and speed of rail transit vehicles, the required braking force increases, leading to a corresponding increase in braking thermal load and aggravating thermal damage caused by wheel braking. Heat generated by friction between the tread and brake shoes is transferred to the wheel and brake shoe interior through the friction contact surface. The problem of thermal damage caused by high thermal stress in the wheels due to increased thermal expansion caused by wheel temperature rise is becoming increasingly prominent.

[0005] Currently, the main materials used for flexible wheel hubs are ER9 and LG61, which are all carbon steels. The final microstructure is pearlite + ferrite. The material's ability to resist thermal damage and the propagation of internal fatigue cracks needs to be further improved. Therefore, there is an urgent need to develop a wheel hub with high resistance to thermal damage for flexible wheels. Summary of the Invention

[0006] To solve the above-mentioned technical problems, the present invention provides a wheel rim with high heat damage resistance (≥420HB) for elastic wheels, which has the characteristics of high strength, high hardness, high corrosion resistance and high heat damage resistance, and exhibits good strength and toughness matching performance.

[0007] The present invention also provides a heat treatment method and a production method for wheel rims with high heat damage resistance (≥420HB).

[0008] The technical solution adopted in this invention is as follows:

[0009] This invention provides a high heat-damage resistant elastic wheel rim (≥420HB), comprising the following chemical composition by weight percentage: C: 0.44–0.49%, Si: 0.80–0.90%, Mn: 1.00–1.20%, Cr: 0.55–0.75%, Ni: 0.15–0.30%, Mo: 0.45–0.55%, Co: 0.55–0.75%, Zr: 0.040–0.060%, La: 0.002–0. 0.003%, V: 0.20~0.30%, Nb: 0.055~0.075%, P≤0.010%, S≤0.008%, T[O]≤0.0010%, [N]: 0.0080~0.010%, [H]≤0.0001%, Al: 0.025~0.045%, with the remainder being Fe and other unavoidable impurities, of which 5.0≤F≤9.9, F=(2.0Mo+1.2Cr) / (V+1.3Nb).

[0010] The preferred chemical composition includes the following weight percentages: C: 0.45–0.48%, Si: 0.82–0.88%, Mn: 1.05–1.15%, Cr: 0.60–0.70%, Ni: 0.20–0.28%, Mo: 0.46–0.53%, Co: 0.60–0.70%, Zr: 0.045–0.058%, La: 0.002–0.003%, V: 0.22–0.28%, Nb: 0.060–0.070%, P≤0.008%, S≤0.005%, T[O]≤0.0008%, [N]: 0.0085–0.0095%, [H]≤0.00008%, Al: 0.028–0.040%, with the remainder being Fe and other unavoidable impurities.

[0011] The composition of the ≥420HB high heat damage resistant elastic wheel rim satisfies the critical quenching diameter DI≥8.0, DI=(0.54C)×(1.00+3.3333Mn)×(1.00+0.7Si)×(1.00+0.363Ni)×(1.00+2.16Cr)×(1.00+3.00Mo)×(1.00+1.73V).

[0012] The composition of the ≥420HB high heat-damage resistant elastic wheel rim meets the following requirements: A value ≥11, A=20(0.21Cr+0.19Si) 2 +0.27Mo +0.51Zr +0.35Co).

[0013] The composition of the ≥420HB high heat damage resistant elastic wheel rim meets the wear limit Brinell hardness Y value ≥420, Y=3.3×(100C-100(C-0.4) / 3+10Si+25Mo+30Mn+6Ni+20Cr+60(V+Nb)).

[0014] The metallographic structure of the ≥420HB high heat damage resistant elastic wheel rim is a tempered martensitic structure and a lower bainitic structure.

[0015] The wheel rims for high heat-damage resistant elastic wheels (≥420HB) have a rim tensile strength ≥1300MPa, yield strength ≥1150MPa, impact energy (KV2) ≥100J at -60℃, rim wear limit Brinell hardness ≥400HBW, hardness variation of a single wheel rim section within 15HBW, and rim fracture toughness ≥120MPa at 0℃. 1 / 2 The austenitic grain size of the steel is greater than or equal to 10.0.

[0016] The present invention also provides a heat treatment method for the ≥420HB high heat damage resistance elastic wheel rim, the heat treatment method comprising the following steps:

[0017] 1) Preliminary heat treatment, including stress-relieving annealing and austenite homogenization high-temperature normalizing;

[0018] 2) Performance heat treatment, including high-temperature quenching, dual-liquid sub-temperature quenching, high-temperature tempering, and low-temperature tempering.

[0019] In step 1), the stress-relief annealing specifically involves heating the blank wheel rim to a temperature of 580–640°C at a heating rate of 180–210°C / h. The holding time within this temperature range is based on the greater of the maximum height and maximum thickness of the blank wheel rim, calculated at 2.8–3.2 min / mm, followed by furnace cooling. During the cooling process after forging, the temperature difference between the surface and the core creates residual internal stress. This internal stress, combined with the internal attraction generated by subsequent process factors, leads to distortion or cracking during subsequent performance heat treatment. To eliminate this internal stress, stress-relief annealing is necessary. Stress-relief annealing also reduces hardness and improves dimensional stability.

[0020] In step 1), the austenite homogenization high-temperature normalizing specifically involves heating the blank hoop to 960–990°C at a heating rate of 200–230°C / h. The holding time within this temperature range is based on the greater of the maximum height and maximum thickness of the blank hoop, calculated at 0.9–1.3 min / mm, followed by air cooling. For steels containing carbide-forming elements such as V, Cr, Nb, and Zr, a higher heating temperature is necessary to ensure complete carbide dissolution during normalizing; therefore, the normalizing temperature is set at 960–990°C. Normalizing not only refines the grains but also improves the inhomogeneity of the microstructure, preparing the microstructure for subsequent final performance heat treatment.

[0021] In step 2), the high-temperature quenching specifically involves heating the blank wheel hoop to a temperature of 1050–1080°C at a heating rate of 150–180°C / h. The heating and holding time within this temperature range is calculated at 0.8–1.2 min / mm, based on the larger of the maximum height and maximum thickness of the blank wheel hoop. Subsequently, oil cooling is performed at 0.35–0.55 s / mm, based on the smaller of the maximum height and maximum thickness of the blank wheel hoop, followed by air cooling to room temperature below 150°C. After high-temperature heating to 1050–1080°C, the insoluble alloy carbides can fully dissolve into the high-temperature austenite, thus obtaining austenite with a homogeneous composition. After subsequent quenching and tempering, the carbides are distributed in a fine, spherical pattern. This carbide distribution, on the one hand, plays a role in dispersion strengthening in the matrix; on the other hand, it makes the crack propagation path tortuous, preventing crack propagation, thereby improving the strength, plasticity, and toughness of the steel.

[0022] In step 2), the dual-liquid sub-critical quenching specifically involves heating the blank wheel rim to 830-860°C at a heating rate of 170-200°C / h. The heating and holding time within this temperature range is calculated at 0.9-1.1 min / mm, based on the greater of the maximum height and maximum thickness of the blank wheel rim. Subsequently, based on the lesser of the maximum height and maximum thickness, the blank wheel rim is cooled in a 5% Na₂CO₃ aqueous solution at 0.15-0.25 s / mm. When cooled to 400°C, it is transferred to an oil bath for further cooling, and finally air-cooled to room temperature below 100°C. This process ensures that the wheel rim cools to near its maximum cooling rate in the high-temperature region, rapidly cooling in the most unstable austenite regions such as the pearlite and bainite transformation zones to prevent decomposition, and slowly cooling during the martensitic transformation to reduce the structural stress during the austenite-to-martensite transformation, thus preventing distortion and cracking of the wheel rim. Simultaneously, it ensures the formation of a fine lath-like martensite structure.

[0023] The mass concentration of the Na2CO3 aqueous solution is 5%.

[0024] In step 2), the high-temperature tempering specifically involves heating the blank wheel rim to a temperature of 600–630°C at a heating rate of 120–150°C / h. The holding time within this temperature range is based on the greater of the maximum height and maximum thickness of the blank wheel rim, calculated at 1.5–1.8 min / mm. Subsequently, it is water-cooled to room temperature to avoid secondary temper brittleness in the steel. After tempering, a uniform and fine martensitic tempered metallographic structure is obtained, resulting in good toughness, plasticity, and suitable strength properties.

[0025] In step 2), the low-temperature tempering specifically involves heating the blank wheel rim to a temperature of 160–190°C at a heating rate of 50–80°C / h. The heating and holding time within this temperature range is based on the greater of the maximum height and maximum thickness of the blank wheel rim, calculated at 1.3–1.5 min / mm. Subsequently, it is air-cooled to room temperature. This low-temperature tempering reduces the brittleness and internal stress generated in the wheel rim during the high-temperature tempering and water-cooling process, thus improving its stability.

[0026] This invention also provides a method for producing wheel rims with ≥420HB high heat damage resistance elasticity, the method comprising the following steps: smelting in an electric arc furnace or converter → refining in an LF furnace → vacuum degassing in an RH or VD furnace → continuous casting → heating in a billet heating furnace → hot rolling of round steel → forging of wheel rim blanks → heat treatment → rough turning → finish turning → flaw detection; wherein, the heat treatment is performed using the heat treatment method described in this invention.

[0027] The function and control of each component in the ≥420HB high heat-damage resistant elastic wheel rim provided by this invention are as follows:

[0028] Carbon (C): Carbon is essential for steel to achieve high strength and hardness. Traditional wheel rim steel has a relatively high C content. While a high C content is beneficial to the strength and hardness of steel, it is extremely detrimental to its plasticity and toughness, reducing the yield strength ratio, increasing decarburization sensitivity, and worsening the steel's fatigue resistance and machinability. Therefore, appropriately reducing the C content in steel improves its plasticity and toughness. However, excessively low C content will affect the steel's strength. Considering the requirements for the dilution ratio (DI) and the addition of other elements, the C content is controlled between 0.44% and 0.49%, with a further preferred range of 0.45% to 0.48%.

[0029] Si: Si is the main deoxidizing element in steel and has a strong solid solution strengthening effect. It can also increase the phase transformation point of steel and improve the heat damage resistance of wheel rims. Therefore, the Si content is controlled at 0.80-0.90%, and more preferably 0.82-0.88%.

[0030] Mn: Mn is a major alloying element in steel and an effective element for deoxidation and desulfurization. Mn can improve the stability of austenite in steel, as well as its hardenability and strength. However, during the tempering of quenched steel, Mn and P have a strong tendency to co-segregate at grain boundaries, which promotes temper brittleness and deteriorates the toughness of the steel. Therefore, the Mn content is controlled at 1.00-1.20%, and more preferably 1.05-1.15%.

[0031] Cr: Cr can effectively improve the hardenability and tempering resistance of steel to obtain the required high strength; at the same time, Cr can reduce the activity of C, which can reduce the tendency of steel surface decarburization during heating, rolling and heat treatment, and is conducive to obtaining high fatigue resistance. However, excessive content will deteriorate the toughness of steel, so the Cr content is controlled at 0.55-0.75%, and more preferably 0.60-0.70%.

[0032] Ni: A major alloying element in steel. Ni can improve the strength and toughness of steel, strengthen grain boundaries at low temperatures, and is an essential alloying element for obtaining high toughness and low-temperature toughness. It also lowers the impact toughness transition temperature. Ni can improve the hardenability and corrosion resistance of steel and ensure its toughness at low temperatures. The Ni content should be controlled at 0.15-0.30%, and more preferably 0.20-0.28%.

[0033] Mo: Mo is a substitutional solid solution alloying element. When dissolved in austenite, it improves the hardenability of steel, enhances tempering resistance, and prevents temper brittleness. If the Mo content is too low, these effects are limited; if the Mo content is too high, these effects are saturated, and the cost of the steel increases. Therefore, the Mo content is controlled at 0.45–0.55%, more preferably 0.46–0.53%.

[0034] Co: Co is a non-carbide-forming element that strengthens ferrite in steel. Co also possesses antioxidant properties, significantly improving the thermal stability and heat resistance of steel. Excessive Co addition leads to decreased toughness and increases the steel's decarburization susceptibility. The Co content is controlled between 0.55% and 0.75%, more preferably between 0.60% and 0.70%.

[0035] Zr: Zr is a strong carbide-forming element, producing fine, dispersed carbides that coherently pin dislocations in the matrix, hindering dendrite growth and grain boundary migration, thus generating whiskers and refining grains. Furthermore, Zr can dissolve in austenite, significantly increasing hardenability. Like Mo, Zr readily precipitates at grain boundaries, exhibiting significant grain boundary strengthening at high temperatures. However, excessive Zr can lead to the formation of brittle inclusions. The Zr content is controlled between 0.040% and 0.060%, with a further preferred range of 0.045% to 0.058%.

[0036] La (La): Adding an appropriate amount of La to steel can transform inclusions such as MnS and Al2O3 into rare earth inclusions, resulting in good deoxidation and desulfurization effects. Tiny solid particles of La provide heterogeneous crystal nuclei or segregate at the crystallization interface, hindering cell growth and improving the room-temperature mechanical properties of the steel. Excessive La has no significant effect. The La content should be controlled between 0.002% and 0.003%.

[0037] The strengthening and toughening effect of vanadium (V) on steel is mainly manifested in precipitation strengthening. Firstly, V(C,N) precipitates during forging and rolling to refine austenite grains. Secondly, during reheating after heat treatment, a large amount of V(CN) nano-second phase precipitates, refining the grain size of the reheated austenite. Excessive V content leads to excessively high V(CN) precipitation temperature, excessive precipitation amount, and coarse particle size, which is detrimental to austenite grain refinement and negatively impacts the steel's strength and toughness. Too low a V content results in negligible overall effects. Therefore, the V content is controlled at 0.20–0.30%, and more preferably 0.22–0.28%.

[0038] Nitrogen b (Nb) primarily strengthens and toughens axle steel through grain refinement, precipitation strengthening, and transformation strengthening. Nb exists in steel as a substitute solute atom. Nb atoms are larger than iron atoms and tend to cluster along dislocation lines, strongly dragging dislocation climb and inhibiting recrystallization nucleation. This significantly raises the recrystallization temperature of austenite, thus refining the austenite grains. Grain refinement not only improves the strength and toughness of the steel but also enhances its low-temperature performance. However, Nb is expensive. Considering all factors, the Nb content can be controlled within the range of 0.055% to 0.075%, with a further preferred range of 0.060% to 0.070%.

[0039] P: P can form micro-segregation when molten steel solidifies, and then agglomerates at the grain boundaries when heated to the austenitizing temperature, which significantly increases the brittleness of the steel. Therefore, the content of P should be controlled below 0.010, and more preferably below 0.008%.

[0040] S: An unavoidable impurity in steel, which forms MnS inclusions and deteriorates the toughness and fatigue resistance of steel by segregation at grain boundaries. Therefore, its content is controlled to be below 0.008%, and more preferably below 0.005%.

[0041] Oxygen (T[O]): Oxygen forms various oxide inclusions in steel. Under stress, stress concentration easily occurs at these oxide inclusions, leading to the initiation of microcracks and thus deteriorating the mechanical properties of the steel, especially its toughness and fatigue resistance. Therefore, measures must be taken in metallurgical production to reduce its content as much as possible. Considering economic efficiency, its content is controlled below 0.0010%, and more preferably below 0.0008%.

[0042] [N]: Nitrogen (N) forms carbonitrides with V and Al in steel, which can effectively inhibit austenite grain growth. However, excessive N content can lead to a deterioration in the toughness and fatigue resistance of steel. Therefore, the N content should be controlled within the range of 0.0080–0.010%, and more preferably 0.0085–0.0095%. Al: In addition to reducing dissolved oxygen in molten steel, aluminum can also refine grains. However, excessive Al content can reduce harmful elements such as Ti in steel and easily cause secondary oxidation and contamination of molten steel during continuous casting. Therefore, the Al content should be controlled within the range of 0.025–0.045%, and more preferably 0.028–0.040%.

[0043] Compared with LG61, the wheel rim with ≥420HB high heat damage resistance provided by this invention: (1) appropriately reduces the C element content to improve the plasticity and toughness of the steel; (2) appropriately increases the Si element content to increase the Ac1 / Ac3 phase transformation point of the steel and improve the heat damage problem that occurs during service; (3) adds trace amounts of V, N and other elements to exert the precipitation strengthening effect of V(CN), refine the grains, improve the toughness and yield strength of the steel, thereby improving the fatigue resistance and anti-peeling performance of the steel; (4) adds appropriate Ni element to the steel, Ni can improve the strength and toughness of the steel, strengthen the grain boundaries under low temperature conditions, obtain high low temperature toughness, and reduce the impact toughness transformation temperature, further improving the safety of the wheel rim under low temperature conditions; (5) adds trace amounts of Nb, Cr and Mo strong carbide forming elements, which not only refine the original austenite grain size, but also maintain the relatively small size of the second phase precipitate M(C,N) during tempering, which can act as a hydrogen trap to inhibit hydrogen-induced delayed fracture. (6) Adding trace amounts of Zr and Co enhances the heat resistance of steel and improves its resistance to heat damage. (7) Strictly control the content of impurity elements such as T[O], P, and S in steel to further improve its fatigue resistance.

[0044] In order to obtain a tempered microstructure of martensite composed of uniform fine-grained cementite and polygonal ferrite matrix, plus a small amount of lower bainite, after heat treatment of the entire cross section of the wheel rim, and considering the effective cross-sectional dimensions of the wheel rim (maximum height of 200 mm (7.87 in) and maximum thickness of 170 mm (6.69 in)) and performance requirements, in order to give the wheel rim suitable hardenability, the critical quenching diameter DI of the steel is set to be ≥8.0, DI=(0.54C)×(1.00+3.3333Mn)×(1.00+0.7Si)×(1.00+0.363Ni)×(1.00+2.16Cr)×(1.00+3.00Mo)×(1.00+1.73V).

[0045] To ensure the wheel rim exhibits high resistance to heat damage, this invention controls the A value to be ≥11, where A = 20(0.21Cr + 0.19Si). 2+0.27Mo+0.51Zr+0.35Co). The A value is an index that evaluates the degree of influence of Cr, Si, Mo, Zr and Co on the heat resistance of steel and the influence of each element by weighting and adding them together. Cr, Si, Mo, Zr and Co are the main elements that improve the heat resistance of the steel grade of this invention.

[0046] To achieve high strength and toughness in wheel rims under appropriate heat treatment processes and meet the requirements for high resistance to thermal damage during service, this invention, based on the role of alloying elements in steel, sets the wear limit Brinell hardness of the wheel rim to a Y value ≥ 420, where Y = 3.3 × (100C - 100(C - 0.4) / 3 + 10Si + 25Mo + 30Mn + 6Ni + 20Cr + 60(V + Nb)). Y is an index used to evaluate the weighted summation of the influence of each element on the Brinell hardness of the quenched and tempered steel.

[0047] The high heat-damage resistant elastic wheel rim provided by this invention has a tensile strength ≥1300MPa and a yield strength ≥1150MPa, belonging to high-strength steel. As the strength of the steel increases, the problem of hydrogen-induced delayed fracture becomes increasingly prominent. This invention employs a design using strong carbide-forming elements such as V, Nb, Cr, and Mo in a coupled manner. This composite microalloying not only refines the original austenite grain size, but also ensures that the second-phase precipitate M(C,N) phase maintains a relatively small size during tempering, acting as a hydrogen trap to suppress hydrogen-induced delayed fracture. The required parameters are (2.0Mo+1.2Cr) / (V+1.3Nb)=F, 5.0≤F≤9.9.

[0048] In the above formula, the value of each element is the content of the corresponding element in the above component × 100;

[0049] The heat treatment method for wheel rims with ≥420HB high resistance to heat damage provided by this invention adopts an overall tempering heat treatment of "preliminary heat treatment (stress-relieving annealing + high-temperature normalizing) + high-temperature quenching + double-liquid sub-temperature quenching + high-temperature tempering + low-temperature tempering". This gives the entire cross-section of the wheel rim a martensitic tempered structure composed of uniform fine-grained cementite and polygonal ferrite matrix, plus a small amount of lower bainite traces. This results in high hardness and high strength, as well as strong toughness and yield strength ratio, further improving the wheel rim's resistance to rolling contact fatigue, heat damage, and wear resistance.

[0050] The key to this invention lies in the organic combination of composition optimization and heat treatment process optimization. Compared with traditional surface-sprayed carbon steel wheel rims, it achieves high strength and high hardness while obtaining excellent heat damage resistance and wear resistance, reducing peeling and detachment phenomena, further improving the service stability of the wheel rim throughout its entire service life, and also has the performance to serve under low temperature conditions.

[0051] Compared with the prior art, the present invention has the following beneficial effects:

[0052] The elastic wheel rims produced using the chemical composition, process flow, and heat treatment parameters of this invention exhibit the following properties: rim tensile strength (Rm) ≥ 1300 MPa, yield strength ≥ 1150 MPa, -60℃ impact energy KV2 ≥ 100 J, rim wear limit Brinell hardness ≥ 400 HBW (50 / 750), hardness variation of a single wheel rim section within 15 HBW, and rim fracture toughness ≥ 120 MPa. 1 / 2 The austenite grain size of the steel is greater than or equal to grade 10.0; the microstructure of the steel after heat treatment is a fine martensitic tempered microstructure with a small amount of lower bainite traces; among which, the content of near-surface martensitic tempered microstructure is 100% or more, and near-surface refers to 0 to 40 mm below the tread surface.

[0053] (1) Compared with the traditional “pearlite + ferrite” wheel rim, it has the characteristics of high strength, high hardness, high corrosion resistance and high heat damage resistance, and exhibits good strength and toughness combination performance.

[0054] (2) The rim tensile strength is ≥1300MPa, yield strength is ≥1150MPa, impact energy at -60℃ (KV2) is ≥100J, the rim wear limit Brinell hardness is ≥400HBW (50 / 750), the variation in hardness value of a single wheel rim section is within 15HBW, and the rim fracture toughness is ≥120MPa. 1 / 2 The austenitic grain size of the steel is greater than or equal to 10.0.

[0055] (3) The microstructure of the steel after heat treatment of the wheel rim is a fine martensitic tempered structure with a small amount of lower bainite traces; among which, the content of near-surface martensitic tempered structure is 100%, and near-surface refers to 0 to 40 mm below the tread surface. It has better heat damage resistance and wear resistance, thereby reducing anti-peeling and detachment phenomena, and further improving the service stability of the wheel rim throughout its entire service life. Attached Figure Description

[0056] Figure 1 The metallographic structure 50mm below the rim tread surface in Example 1 is a tempered structure of 100% martensite.

[0057] Figure 2 The metallographic structure 50 mm below the rim tread in Comparative Example 1 is pearlite + ferrite. Detailed Implementation

[0058] This invention provides a wheel rim with ≥420HB high heat damage resistance and elasticity, comprising the following chemical composition by weight percentage: C: 0.44–0.49%, Si: 0.80–0.90%, Mn: 1.00–1.20%, Cr: 0.55–0.75%, Ni: 0.15–0.30%, Mo: 0.45–0.55%, Co: 0.55–0.75%, Zr: 0.040–0.060%, La: 0.002–0. 0.003%, V: 0.20~0.30%, Nb: 0.055~0.075%, P≤0.010%, S≤0.008%, T[O]≤0.0010%, [N]: 0.0080~0.010%, [H]≤0.0001%, Al: 0.025~0.045%, with the remainder being Fe and other unavoidable impurities, of which 5.0≤F≤9.9, F=(2.0Mo+1.2Cr) / (V+1.3Nb).

[0059] The preferred chemical composition includes the following weight percentages: C: 0.45–0.48%, Si: 0.82–0.88%, Mn: 1.05–1.15%, Cr: 0.60–0.70%, Ni: 0.20–0.28%, Mo: 0.46–0.53%, Co: 0.60–0.70%, Zr: 0.045–0.058%, La: 0.002–0.003%, V: 0.22–0.28%, Nb: 0.060–0.070%, P≤0.008%, S≤0.005%, T[O]≤0.0008%, [N]: 0.0085–0.0095%, [H]≤0.00008%, Al: 0.028–0.040%, with the remainder being Fe and other unavoidable impurities.

[0060] The composition of the ≥420HB high heat damage resistant elastic wheel rim satisfies the critical quenching diameter DI≥8.0, DI=(0.54C)×(1.00+3.3333Mn)×(1.00+0.7Si)×(1.00+0.363Ni)×(1.00+2.16Cr)×(1.00+3.00Mo)×(1.00+1.73V).

[0061] The composition of the ≥420HB high heat-damage resistant elastic wheel rim meets the following requirements: A value ≥11, A=20(0.21Cr+0.19Si) 2 +0.27Mo +0.51Zr +0.35Co).

[0062] The composition of the ≥420HB high heat damage resistant elastic wheel rim meets the wear limit Brinell hardness Y value ≥420, Y=3.3×(100C-100(C-0.4) / 3+10Si+25Mo+30Mn+6Ni+20Cr+60(V+Nb)).

[0063] The metallographic structure of the ≥420HB high heat damage resistant elastic wheel rim is a tempered martensitic structure and a lower bainitic structure.

[0064] The wheel rims for high heat-damage resistant elastic wheels (≥420HB) have a rim tensile strength ≥1300MPa, yield strength ≥1150MPa, impact energy (KV2) at -60℃ ≥100J, rim wear limit Brinell hardness ≥400HBW, hardness variation of a single wheel rim section within 15HBW, and rim fracture toughness ≥120MPa. 1 / 2 The austenitic grain size of the steel is greater than or equal to 10.0.

[0065] The heat treatment method for the wheel rim with ≥420HB high heat damage resistance includes the following steps:

[0066] 1) Preliminary heat treatment, including stress-relieving annealing and austenite homogenization high-temperature normalizing;

[0067] 2) Performance heat treatment, including high-temperature quenching, dual-liquid sub-temperature quenching, high-temperature tempering, and low-temperature tempering.

[0068] In step 1), the stress-relief annealing specifically involves heating the blank wheel hoop to a temperature of 580-640℃ at a heating rate of 180-210℃ / h. The heating and holding time in this temperature range is based on the larger of the maximum height and maximum thickness of the blank wheel hoop, and the holding time is calculated at 2.8-3.2 min / mm, followed by furnace cooling.

[0069] In step 1), the austenite homogenization high-temperature normalizing specifically involves heating the blank wheel hoop to a temperature of 960-990℃ at a heating rate of 200-230℃ / h. The heating and holding time in this temperature range is based on the larger of the maximum height and maximum thickness of the blank wheel hoop, and the holding time is calculated at 0.9-1.3 min / mm, followed by air cooling.

[0070] In step 2), the high-temperature quenching specifically involves heating the blank wheel rim to a temperature of 1050–1080°C at a heating rate of 150–180°C / h. The heating and holding time in this temperature range is calculated at 0.8–1.2 min / mm, based on the larger of the maximum height and maximum thickness of the blank wheel rim. Subsequently, oil cooling is performed at 0.35–0.55 s / mm, based on the smaller of the maximum height and maximum thickness of the blank wheel rim, until the temperature drops below 150°C and then air cooling is performed to room temperature.

[0071] In step 2), the dual-liquid sub-temperature quenching specifically involves heating the blank wheel rim to a temperature of 830–860°C at a heating rate of 170–200°C / h. The heating and holding time in this temperature range is calculated at 0.9–1.1 min / mm, based on the larger of the maximum height and maximum thickness of the blank wheel rim. Subsequently, based on the smaller of the maximum height and maximum thickness of the blank wheel rim, it is cooled in a 5% Na2CO3 aqueous solution at a rate of 0.15–0.25 s / mm. When cooled to 400°C, it is transferred to an oil bath for further cooling. When cooled to below 100°C, it is air-cooled to room temperature.

[0072] The mass concentration of the Na2CO3 aqueous solution is 5%.

[0073] In step 2), the high-temperature tempering specifically involves heating the blank wheel rim to a temperature of 600-630°C at a heating rate of 120-150°C / h. The heating and holding time in this temperature range is based on the larger of the maximum height and maximum thickness of the blank wheel rim, and the holding time is calculated at 1.5-1.8 min / mm. Then, it is water-cooled to room temperature.

[0074] In step 2), the low-temperature tempering specifically involves heating the blank wheel rim to a temperature of 160-190°C at a heating rate of 50-80°C / h. The heating and holding time in this temperature range is based on the larger of the maximum height and maximum thickness of the blank wheel rim, and the holding time is calculated at 1.3-1.5 min / mm. Then, it is air-cooled to room temperature.

[0075] The production method of the ≥420HB high heat damage resistance elastic wheel rim includes the following steps: electric arc furnace or converter smelting → LF furnace refining → RH or VD vacuum degassing → continuous casting → billet heating furnace heating → hot rolling of round steel → wheel rim blank forging → heat treatment → rough turning → finish turning → flaw detection; wherein, the heat treatment is carried out using the heat treatment method described in this invention.

[0076] The present invention will now be described in detail with reference to the embodiments.

[0077] Example 1

[0078] A wheel rim with good fatigue resistance and high resistance to heat damage (≥420HB) is provided. Its chemical composition and weight percentage are shown in Example 1 in Table 1. The balance not shown in Table 1 is Fe and unavoidable impurities.

[0079] The production method of the ≥420HB high heat-damage resistant elastic wheel rim is as follows: electric arc furnace or converter smelting → LF furnace refining → RH or VD vacuum degassing → continuous casting → billet heating furnace heating → hot rolling of round steel → wheel rim blank forging, forging into a blank wheel rim with a height of 200mm, a thickness of 160mm, and an outer diameter of 690mm → heat treatment → rough turning → finish turning → flaw detection; wherein, the heat treatment is carried out using the following heat treatment method:

[0080] Stress-relief annealing: Heat at 180℃ / h to 640℃, hold for 600min, and furnace cool to below 100℃.

[0081] High-temperature normalizing for austenite homogenization: Heat to 960℃ at 230℃ / h, hold for 180min, and air cool to below 200℃.

[0082] High-temperature quenching: Heat to 1050℃ at 170℃ / h, hold for 200min, cool in quenching oil for 70s to below 150℃, and air cool to room temperature.

[0083] Dual-liquid sub-temperature quenching: Heat to 860℃ at 170℃ / h, hold for 210min, cool in 5% Na2CO3 aqueous solution for 26s, transfer to oil bath for further cooling when cooled to 400℃, and air cool to room temperature when cooled to below 100℃.

[0084] High-temperature tempering: Heat to 620℃ at 130℃ / h, hold for 300min, and then cool to room temperature with water.

[0085] Low-temperature tempering: Heat at 60℃ / h to 160℃, hold at that temperature for 270min, and then air cool to room temperature.

[0086] Example 2

[0087] A wheel rim with good fatigue resistance and high heat damage resistance (≥420HB) is provided. Its chemical composition and weight percentage are shown in Example 2 in Table 1. The balance not shown in Table 1 is Fe and unavoidable impurities.

[0088] The production method of the ≥420HB high heat-damage resistant elastic wheel rim is as follows: electric arc furnace or converter smelting → LF furnace refining → RH or VD vacuum degassing → continuous casting → billet heating furnace heating → hot rolling of round steel → wheel rim blank forging, forging into a blank wheel rim with a height of 200mm, a thickness of 170mm, and an outer diameter of 650mm → heat treatment → rough turning → finish turning → flaw detection; wherein, the heat treatment is carried out using the following heat treatment method:

[0089] Stress-relief annealing: Heat at 190℃ / h to 630℃, hold for 620min, and furnace cool to below 100℃.

[0090] High-temperature normalizing for austenite homogenization: Heat to 970℃ at 220℃ / h, hold for 200min, and air cool to below 200℃.

[0091] High-temperature quenching: Heat to 1080℃ at 180℃ / h, hold for 190min, cool in quenching oil for 60s to below 150℃, and air cool to room temperature.

[0092] Dual-liquid sub-temperature quenching: Heat to 850℃ at 180℃ / h, hold for 220min, cool in 5% Na2CO3 aqueous solution for 30s, transfer to oil bath for further cooling when cooled to 400℃, and air cool to room temperature when cooled to below 100℃.

[0093] High-temperature tempering: Heat to 600℃ at 120℃ / h, hold for 360min, and then cool to room temperature with water.

[0094] Low-temperature tempering: Heat at 50℃ / h to 170℃, hold for 260min, and air cool to room temperature.

[0095] Example 3

[0096] A wheel rim with good fatigue resistance and high heat damage resistance (≥420HB) is provided. Its chemical composition and weight percentage are shown in Example 3 in Table 1. The balance not shown in Table 1 is Fe and unavoidable impurities.

[0097] The production method of the ≥420HB high heat-damage resistant elastic wheel rim is as follows: electric arc furnace or converter smelting → LF furnace refining → RH or VD vacuum degassing → continuous casting → billet heating furnace heating → hot rolling of round steel → wheel rim blank forging, forging into a blank wheel rim with a height of 200mm, a thickness of 165mm, and an outer diameter of 690mm → heat treatment → rough turning → finish turning → flaw detection; wherein, the heat treatment is carried out using the following heat treatment method:

[0098] Stress-relief annealing: Heat at 210℃ / h to 580℃, hold for 640min, and furnace cool to below 100℃.

[0099] High-temperature normalizing for austenite homogenization: Heat at 200℃ / h to 990℃, hold for 260min, and air cool to below 200℃.

[0100] High-temperature quenching: Heat to 1070℃ at 160℃ / h, hold for 200min, cool in quenching oil for 80s to below 150℃, and air cool to room temperature.

[0101] Dual-liquid sub-temperature quenching: Heat to 830℃ at 200℃ / h, hold for 190min, cool in 5% Na2CO3 aqueous solution for 41s, transfer to oil bath for further cooling when cooled to 400℃, and air cool to room temperature when cooled to below 100℃.

[0102] High-temperature tempering: Heat to 630℃ at 140℃ / h, hold for 340min, and then cool to room temperature with water.

[0103] Low-temperature tempering: Heat at 80℃ / h to 180℃, hold at that temperature for 300min, and then air cool to room temperature.

[0104] Example 4

[0105] A wheel rim with good fatigue resistance and high resistance to heat damage (≥420HB) is provided. Its chemical composition and weight percentage are shown in Example 4 of Table 1. The balance not shown in Table 1 is Fe and unavoidable impurities.

[0106] The production method of the ≥420HB high heat-damage resistant elastic wheel rim is as follows: electric arc furnace or converter smelting → LF furnace refining → RH or VD vacuum degassing → continuous casting → billet heating furnace heating → hot rolling of round steel → wheel rim blank forging, forging into a blank wheel rim with a height of 200mm, a thickness of 169mm, and an outer diameter of 695mm → heat treatment → rough turning → finish turning → flaw detection; wherein, the heat treatment is carried out using the following heat treatment method:

[0107] Stress-relief annealing: Heat at 200℃ / h to 610℃, hold for 630min, and furnace cool to below 100℃.

[0108] High-temperature normalizing for austenite homogenization: Heat to 980℃ at 210℃ / h, hold for 220min, and air cool to below 200℃.

[0109] High-temperature quenching: Heat to 1060℃ at 150℃ / h, hold for 220min, cool in quenching oil for 90s to below 150℃, and air cool to room temperature.

[0110] Dual-liquid sub-temperature quenching: Heat to 840℃ at 190℃ / h, hold for 180min, cool in 5% Na2CO3 aqueous solution for 38s, transfer to oil bath for further cooling when cooled to 400℃, and air cool to room temperature when cooled to below 100℃.

[0111] High-temperature tempering: Heat to 610℃ at 150℃ / h, hold for 330 minutes, and then cool to room temperature with water.

[0112] Low-temperature tempering: Heat at 70℃ / h to 190℃, hold for 280min, and air cool to room temperature.

[0113] Comparative Example 1

[0114] A type of flexible wheel rim, the chemical composition and weight percentage of which are shown in Comparative Example 1 in Table 1, with the balance not shown in Table 1 being Fe and unavoidable impurities.

[0115] The production method of the elastic wheel rim is as follows: smelting in an electric arc furnace or converter → refining in an LF furnace → RH or VD vacuum degassing → continuous casting → heating in a billet heating furnace → hot rolling of round steel → forging of the wheel rim blank, forging into a blank wheel rim with a height of 200mm, a thickness of 168mm, and an outer diameter of 690mm → heat treatment → rough turning → finish turning → flaw detection; wherein, the heat treatment is carried out using the following heat treatment method:

[0116] Quenching: Heat at 200℃ / h to 865℃, hold for 200min, and cool to room temperature with water.

[0117] Tempering: Heat at 210℃ / h to 610℃, hold for 300min, and air cool to room temperature.

[0118] Comparative Example 2

[0119] A flexible wheel rim, the chemical composition and weight percentage of which are shown in Comparative Example 2 in Table 1, with the balance not shown in Table 1 being Fe and unavoidable impurities.

[0120] The production method of the elastic wheel rim is as follows: smelting in an electric arc furnace or converter → refining in an LF furnace → RH or VD vacuum degassing → continuous casting → heating in a billet heating furnace → hot rolling of round steel → forging of the wheel rim blank into a blank wheel rim with a height of 200mm, a thickness of 165mm, and an outer diameter of 700mm → heat treatment → rough turning → finish turning → flaw detection; wherein, the heat treatment is carried out using the following heat treatment method:

[0121] Quenching: Heat to 855℃ at 220℃ / h, hold for 210min, and then cool to room temperature with water.

[0122] Tempering: Heat at 200℃ / h to 620℃, hold for 310 minutes, and air cool to room temperature.

[0123] Comparative Example 3

[0124] A flexible wheel rim, the chemical composition and weight percentage of which are shown in Comparative Example 3 in Table 1, with the balance not shown in Table 1 being Fe and unavoidable impurities.

[0125] The production method of the elastic wheel rim is as follows: smelting in an electric arc furnace or converter → refining in an LF furnace → vacuum degassing in an RH or VD furnace → continuous casting → heating in a billet heating furnace → hot rolling of round steel → forging of the wheel rim blank, forging into a blank wheel rim with a height of 200mm, a thickness of 170mm, and an outer diameter of 650mm → heat treatment → rough turning → finish turning → flaw detection; wherein, the heat treatment adopts the following heat treatment method for stress relief annealing: heating at 210℃ / h to a temperature of 580℃, holding at that temperature for 640min, and furnace cooling to below 100℃.

[0126] High-temperature normalizing for austenite homogenization: Heat at 200℃ / h to 990℃, hold for 260min, and air cool to below 200℃.

[0127] High-temperature quenching: Heat to 1070℃ at 160℃ / h, hold for 200min, cool in quenching oil for 80s to below 150℃, and air cool to room temperature.

[0128] Dual-liquid sub-temperature quenching: Heat to 830℃ at 200℃ / h, hold for 190min, cool in 5% Na2CO3 aqueous solution for 41s, transfer to oil bath for further cooling when cooled to 400℃, and air cool to room temperature when cooled to below 100℃.

[0129] High-temperature tempering: Heat to 660℃ at 140℃ / h, hold for 340min, and cool to room temperature with water to avoid brittleness from secondary tempering.

[0130] Low-temperature tempering: Heat at 80℃ / h to 180℃, hold at that temperature for 300min, and then air cool to room temperature.

[0131] Comparative Example 4

[0132] A type of flexible wheel rim, the chemical composition and weight percentage of which are shown in Comparative Example 4 in Table 1, with the balance not shown in Table 1 being Fe and unavoidable impurities.

[0133] The production method of the wheel rim for the elastic wheel is the same as in Example 2.

[0134] Table 1

[0135]

[0136]

[0137] The mechanical properties of the wheel rims in each embodiment and comparative example are shown in Table 2.

[0138] Table 2 Mechanical properties of the examples and comparative examples

[0139]

[0140] The metallographic structure of the wheel rims and the hardness values ​​and deviations of the rim sections in each embodiment and comparative example are shown in Table 3.

[0141] Table 3. Metallographic structure and hardness values ​​and deviations of the rim cross-section in the examples and comparative examples.

[0142]

[0143]

[0144] The contact fatigue resistance of the wheel rims in each embodiment and comparative example is shown in Table 4.

[0145] Table 4. Contact fatigue resistance of wheels in the examples and comparative cases.

[0146] Contact stress / MPa Number of loops (times) Rotational speed (r / min) Lubrication conditions Is fatigue causing blockage? Example 1 2000 <![CDATA[6×10 6 ]]> 1500 Oil lubrication no Example 2 2000 <![CDATA[6×10 6 ]]> 1500 Oil lubrication no Example 3 2000 <![CDATA[6×10 6 ]]> 1500 Oil lubrication no Example 4 2000 <![CDATA[6×10 6 ]]> 1500 Oil lubrication no Comparative Example 1 1200 <![CDATA[7.0×10 5 ]]> 1500 Oil lubrication yes Comparative Example 2 1200 <![CDATA[7.0×10 5 ]]> 1500 Oil lubrication yes Comparative Example 3 2000 <![CDATA[4.5×10 6 ]]> 1500 Oil lubrication yes Comparative Example 4 2000 <![CDATA[4.0×10 6 ]]> 1500 Oil lubrication yes

[0147] The above-mentioned organizational and performance testing methods are as follows:

[0148] Performance tests were conducted in accordance with GB / T 13299, GB / T 6394, GB / T 228, GB / T 229, GB / T231, GB / T 21143, and GB / T19746.

[0149] The chemical composition and production methods of the steels in Examples 1-4 were appropriately controlled, ensuring that the chemical composition met the following requirements: DI ≥ 8.0 in, N ≥ 11, B ≥ 420, and 5.0 ≤ F ≤ 9.9. The steel exhibited good strength, plasticity, toughness, contact fatigue resistance, and heat damage resistance. Comparative Examples 1 and 2 had unsuitable chemical compositions and heat treatment processes; Comparative Example 3 had an unsuitable heat treatment process; and Comparative Example 4 had an unsuitable Y-value design. The improper control of chemical composition and heat treatment processes in Comparative Examples 1 and 2 resulted in excessively low strength, cross-sectional hardness, low low-temperature impact toughness, and low heat damage resistance. Although Comparative Example 3 had the same chemical composition as Example 3, its heat treatment process was unreasonable, with an excessively high tempering temperature leading to lower strength and cross-sectional hardness, ultimately resulting in poor heat damage resistance. Comparative Example 4 had the same heat treatment process as Example 2, and its chemical composition design met the requirements, but its Y-value design did not conform to the set formula requirements, resulting in lower strength and cross-sectional hardness, ultimately leading to poor contact fatigue resistance.

[0150] The above detailed description of a wheel rim with ≥420HB high heat damage resistance and elasticity for wheels, its heat treatment method, and its production method, with reference to the embodiments, is illustrative rather than limiting. Several embodiments can be listed according to the defined scope. Therefore, changes and modifications without departing from the overall concept of the present invention should be within the protection scope of the present invention.

Claims

1. A wheel rim with ≥420HB high heat damage resistance and elasticity for wheels, characterized in that, The chemical composition includes the following weight percentages: C: 0.44–0.49%, Si: 0.80–0.90%, Mn: 1.00–1.20%, Cr: 0.55–0.75%, Ni: 0.15–0.30%, Mo: 0.45–0.55%, Co: 0.55–0.75%, Zr: 0.040–0.060%, La: 0.002–0.003%, V: 0.20–0. 0.30%, Nb: 0.055~0.075%, P≤0.010%, S≤0.008%, T[O]≤0.0010%, [N]: 0.0080~0.010%, [H]≤0.0001%, Al: 0.025~0.045%, the remainder being Fe and other unavoidable impurities, of which 5.0≤F≤9.9, F=(2.0Mo+1.2Cr) / (V+1.3Nb); The heat treatment method for the wheel rim with ≥420HB high heat damage resistance includes the following steps: 1) Preliminary heat treatment, including stress-relieving annealing and austenite homogenization high-temperature normalizing; 2) Performance heat treatment, including high-temperature quenching, dual-liquid sub-temperature quenching, high-temperature tempering, and low-temperature tempering; In step 1), the stress-relief annealing specifically involves heating the blank wheel rim to a temperature of 580-640℃ at a heating rate of 180-210℃ / h and holding it at that temperature. In step 1), the austenite homogenization high-temperature normalizing specifically involves heating the blank wheel hoop to a temperature of 960-990℃ at a heating rate of 200-230℃ / h and holding it at that temperature. In step 2), the high-temperature quenching specifically involves heating the blank wheel rim to a temperature of 1050-1080℃ at a heating rate of 150-180℃ / h for high-temperature quenching. In step 2), the dual-liquid sub-temperature quenching specifically involves heating the blank wheel rim to a temperature of 830-860℃ at a heating rate of 170-200℃ / h for dual-liquid sub-temperature quenching. In step 2), the high-temperature tempering specifically involves heating the blank wheel rim to a temperature of 600-630℃ at a heating rate of 120-150℃ / h and holding it at that temperature. In step 2), the low-temperature tempering specifically involves heating the blank wheel rim to a temperature of 160-190℃ at a heating rate of 50-80℃ / h and holding it at that temperature.

2. The wheel rim for a wheel with ≥420HB high heat damage resistance as described in claim 1, characterized in that, The chemical composition includes the following weight percentages: C: 0.45–0.48%, Si: 0.82–0.88%, Mn: 1.05–1.15%, Cr: 0.60–0.70%, Ni: 0.20–0.28%, Mo: 0.46–0.53%, Co: 0.60–0.70%, Zr: 0.045–0.058%, La: 0.002–0.003%, V: 0.22–0.28%, Nb: 0.060–0.070%, P≤0.008%, S≤0.005%, T[O]≤0.0008%, [N]: 0.0085–0.0095%, [H]≤0.00008%, Al: 0.028–0.040%, with the remainder being Fe and other unavoidable impurities.

3. The wheel rim for a high-heat-damage-resistant elastic wheel as described in claim 1, characterized in that, The composition of the ≥420HB high heat damage resistant elastic wheel rim satisfies the critical quenching diameter DI≥8.0, DI=(0.54C)×(1.00+3.3333Mn)×(1.00+0.7Si)×(1.00+0.363Ni)×(1.00+2.16Cr)×(1.00+3.00Mo)×(1.00+0.365Cu)×(1.00+1.73V).

4. The wheel rim for a high-heat-damage-resistant elastic wheel with ≥420HB as described in claim 1, characterized in that, The composition of the ≥420HB high heat-damage resistant elastic wheel rim meets the following requirements: A value ≥11, A = 20 (0.21Cr + 0.19Si). 2 +0.27Mo +0.51Zr +0.35Co).

5. The wheel rim for a wheel with ≥420HB high heat damage resistance as described in claim 1, characterized in that, The composition of the ≥420HB high heat damage resistant elastic wheel rim meets the wear limit Brinell hardness Y value ≥420, Y=3.3×(100C-100(C-0.4) / 3+10Si+25Mo+30Mn+6Ni+20Cr+60(V+Nb)).

6. The wheel rim with ≥420HB high heat damage resistance and elasticity for wheels according to any one of claims 1-5, characterized in that, The metallographic structure of the ≥420HB high heat damage resistant elastic wheel rim is a tempered martensitic structure and a lower bainitic structure.

7. The wheel rim for a high heat-damage resistant elastic wheel with ≥420HB as described in any one of claims 1-5, characterized in that, The wheel rims for high heat-damage resistant elastic wheels (≥420HB) have a rim tensile strength ≥1300MPa, yield strength ≥1150MPa, impact energy (KV2) ≥100J at -60℃, rim wear limit Brinell hardness ≥400HBW, hardness variation of a single wheel rim section within 15HBW, and rim fracture toughness ≥120MPa at 0℃. 1 / 2 The austenitic grain size of the steel is greater than or equal to 10.

0.

8. The heat treatment method for wheel rims with ≥420HB high heat damage resistance as described in any one of claims 1-7, characterized in that, The heat treatment method includes the following steps: 1) Preliminary heat treatment, including stress-relieving annealing and austenite homogenization high-temperature normalizing; 2) Performance heat treatment, including high-temperature quenching, dual-liquid sub-temperature quenching, high-temperature tempering, and low-temperature tempering.

9. The heat treatment method according to claim 8, characterized in that, In step 1), the stress-relief annealing specifically involves heating the blank wheel hoop to a temperature of 580-640℃ at a heating rate of 180-210℃ / h. The heating and holding time in this temperature range is based on the larger of the maximum height and maximum thickness of the blank wheel hoop, and the holding time is calculated at 2.8-3.2 min / mm, followed by furnace cooling.

10. The heat treatment method according to claim 8, characterized in that, In step 1), the austenite homogenization high-temperature normalizing specifically involves heating the blank wheel hoop to a temperature of 960-990℃ at a heating rate of 200-230℃ / h. The heating and holding time in this temperature range is based on the larger of the maximum height and maximum thickness of the blank wheel hoop, and the holding time is calculated at 0.9-1.3 min / mm, followed by air cooling.

11. The heat treatment method according to claim 8, characterized in that, In step 2), the high-temperature quenching specifically involves heating the blank wheel rim to a temperature of 1050-1080℃ at a heating rate of 150-180℃ / h. The heating and holding time in this temperature range is calculated at 0.8-1.2 min / mm, based on the larger of the maximum height and maximum thickness of the blank wheel rim. Then, based on the smaller of the maximum height and maximum thickness of the blank wheel rim, oil cooling is performed at 0.35-0.55 s / mm, followed by air cooling to room temperature below 150℃.

12. The heat treatment method according to claim 8, characterized in that, In step 2), the dual-liquid sub-temperature quenching specifically involves heating the blank wheel rim to a temperature of 830-860°C at a heating rate of 170-200°C / h. The heating and holding time in this temperature range is calculated at 0.9-1.1 min / mm, based on the larger of the maximum height and maximum thickness of the blank wheel rim. Then, based on the smaller of the maximum height and maximum thickness of the blank wheel rim, it is cooled in a Na2CO3 aqueous solution at a rate of 0.15-0.25 s / mm. When cooled to 400°C, it is transferred to an oil bath for further cooling. Finally, it is air-cooled to room temperature when cooled to below 100°C.

13. The heat treatment method according to claim 8, characterized in that, In step 2), the high-temperature tempering specifically involves heating the blank wheel rim to a temperature of 600-630℃ at a heating rate of 120-150℃ / h. The heating and holding time in this temperature range is based on the larger of the maximum height and maximum thickness of the blank wheel rim, and the holding time is calculated at 1.5-1.8 min / mm. Then, it is water-cooled to room temperature.

14. The heat treatment method according to claim 8, characterized in that, In step 2), the low-temperature tempering specifically involves heating the blank wheel rim to a temperature of 160-190°C at a heating rate of 50-80°C / h. The heating and holding time in this temperature range is based on the larger of the maximum height and maximum thickness of the blank wheel rim, and the holding time is calculated at 1.3-1.5 min / mm. Then, it is air-cooled to room temperature.

15. The method for producing wheel rims with ≥420HB high heat damage resistance as described in any one of claims 1-7, characterized in that, The production method includes the following steps: smelting in an electric arc furnace or converter → refining in an LF furnace → vacuum degassing in an RH or VD furnace → continuous casting → heating in a billet heating furnace → hot rolling of round steel → forging of wheel rim blanks → heat treatment → rough turning → finish turning → flaw detection; wherein, the heat treatment is carried out using the heat treatment method described in any one of claims 8-14.

Citation Information

Patent Citations

  • Medium-carbon wheel steel and heat treatment method thereof as well as preparation method of wheel

    CN110284069A

  • Steel for wear-resistant elastic wheel rim and heat treatment method and production method of steel

    CN113699451A