A nitrogen-containing molecule-controlled Ru / RuO2 heterocatalyst, its preparation method and application

By using a Ru/RuO₂ heterocatalyst controlled by nitrogen-containing molecules, the problem of insufficient activity and stability of Ru-based heterojunction catalysts under high current density was solved, achieving high-efficiency water electrolysis for hydrogen production, which is suitable for industrial applications.

CN117904668BActive Publication Date: 2026-11-24SHIHEZI UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311863868.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2026-11-24
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

Existing Ru-based heterojunction catalysts exhibit poor hydrogen evolution activity and stability at high current densities, making them difficult to apply in industrial applications.

Method used

A woven network structure NH₂-Ru/RuO₂-NH₂/NF heterojunction catalytic electrode was prepared by using a nitrogen-containing molecule-controlled Ru/RuO₂ heterocatalyst and through porous nickel foam surface modification and low-temperature reduction. The chelating and strong adhesion properties of nitrogen-containing molecules were utilized to improve the active sites and stability of the catalyst.

Benefits of technology

In the alkaline hydrogen evolution reaction, the catalyst can drive 1000 mA cm⁻² water electrolysis to produce hydrogen at a low overpotential of 121 mV. The preparation method is simple, the raw materials are readily available, and it is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117904668B_ABST
    Figure CN117904668B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of catalyst preparation technology, and discloses a nitrogen-containing molecule-controlled Ru / RuO2 heterojunction catalyst, its preparation method, and its application. Nickel foam is immersed in a nitrogen-containing organic molecule solution and dried to obtain an NH2 / NF electrode. The NH2 / NF electrode is placed in a RuCl3·3H2O aqueous solution and reacted at 30–120°C, then dried to obtain a Ru / RuO2-NH2 / NF electrode. The Ru / RuO2-NH2 / NF electrode is then immersed in a nitrogen-containing organic molecule solution at room temperature and dried to obtain a nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst. This catalyst utilizes the chelating, strong adhesion, and reducing properties of nitrogen-containing molecules to prepare a Ru / RuO2 heterojunction composite catalyst. The heterostructure not only increases the active sites of the catalyst, but the synergistic effect between the two also improves the stability of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of water electrolysis for hydrogen production technology, specifically relating to a nitrogen-containing molecule-controlled Ru / RuO2 heterocatalyst, its preparation method, and its application. Background Technology

[0002] With the depletion of traditional fossil fuels and the increasing severity of ecological and environmental problems, the search for renewable and environmentally friendly alternative energy sources is urgently needed. Hydrogen energy, as a renewable and clean energy carrier, has become one of the most promising next-generation energy sources. Currently, hydrogen has a wide range of applications, mainly concentrated in transportation, fuel cells, hydrogen metallurgy, chemical industry, building heating, and power generation. The main hydrogen production methods include fossil fuel production, industrial by-product production, water electrolysis, biomass production, and others. With the goal of producing "green hydrogen," coupling renewable energy power generation with water electrolysis technology holds promise for achieving zero carbon emissions in the hydrogen production process. Therefore, water electrolysis technology is rapidly moving towards large-scale commercialization. However, some key challenges remain in the basic and applied research of water electrolysis for hydrogen production, such as the high overpotential of hydrogen evolution at the cathode and the high electrolysis voltage, leading to high energy consumption and a lack of economic advantage compared to traditional hydrogen production methods. Currently, industrial alkaline water electrolysis cathode hydrogen evolution catalysts mainly consist of platinum and nickel-based composite electrodes. However, the scarcity and high price of Pt, along with its poor activity and stability at high current densities, prevent its application in large-scale industrial hydrogen production. Meanwhile, nickel-based catalytic electrodes exhibit low intrinsic activity and require large overpotentials. Therefore, there is an urgent need to develop catalytic materials with simple preparation methods and excellent catalytic activity.

[0003] Ruthenium-based catalysts have attracted considerable attention as potential catalysts for the hydrogen evolution reaction (HER) due to their inherent high activity and relatively low cost. However, their high surface energy still poses a challenge during preparation or reaction due to the tendency of metal particles to aggregate, reducing their specific activity. Therefore, developing a Ru-based HER catalyst with high activity and stability at industrial current densities remains a significant challenge. Studies have shown that catalysts with unique heterostructures can expose more active sites, accelerate the diffusion kinetics of electrons and ions, significantly reduce the dissociation energy of water, and optimize the adsorption energy of hydrogen intermediates, thereby promoting HER reaction kinetics.

[0004] Wang et al. (Zexing Wu, Lei Wang, et al. Small, 2022, 18, 2105168) synthesized a RuO2-RuP2 / Ru catalyst material with a unique heterostructure supported by N and P co-doped carbon via HMT complex precursors, achieving highly efficient hydrogen evolution across the entire pH range. However, this catalyst only exhibits excellent hydrogen evolution activity at lower current densities.

[0005] Wu et al. (CN114318411B) prepared bamboo-like carbon nanotubes loaded with cobalt nanoparticles using lysozyme-assisted synthesis, and simultaneously anchored ruthenium nanoclusters on the outer surface of the carbon nanotubes to form a cobalt / carbon nanotube / ruthenium composite material with a three-phase heterostructure. Due to the synergistic effect of the components and the increased exposure of more active sites at the interface, the hydrogen evolution activity was improved in electrolytes with a wide pH range. In 1.0 M KOH, 0.5 M H2SO4, and 1 M PBS, at a current density of 10 mA / cm², the hydrogen evolution activity was significantly enhanced. -2 The required overpotentials are only 10 mV, 32 mV, and 63 mV, respectively. However, the hydrogen evolution activity of Ru-based heterojunction catalysts at high current densities remains low. Summary of the Invention

[0006] To address the problem of poor hydrogen evolution activity and stability of Ru-based heterojunction catalysts under high current densities in existing technologies, the present invention aims to provide a nitrogen-containing molecule-controlled Ru / RuO2 heterocatalyst suitable for high-current water electrolysis hydrogen evolution reaction, along with its preparation method and application. This heterojunction catalyst utilizes organic nitrogen-containing molecule surface modification combined with a low-temperature method, resulting in a simple, controllable, and easily scaled-up preparation method. It exhibits excellent hydrogen evolution activity and stability in high-current hydrogen evolution reactions.

[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0008] A method for preparing a nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst includes the following steps:

[0009] (1) Immerse nickel foam in a nitrogen-containing organic molecule solution and dry to obtain an NH2 / NF electrode;

[0010] (2) The NH2 / NF electrode was placed in RuCl3·3H2O aqueous solution and reacted at 30-120℃. After drying, Ru / RuO2-NH2 / NF electrode was obtained.

[0011] (3) The Ru / RuO2-NH2 / NF electrode was immersed in a nitrogen-containing organic molecule solution at room temperature and dried to obtain a nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst.

[0012] Furthermore, the concentration of the nitrogen-containing organic molecule solution is 1–10 mg / mL.

[0013] Furthermore, in steps (1) and (3), the nitrogen-containing organic molecule is one or two of ethylenediamine, disodium ethylenediaminetetraacetate, 3-aminopropyltriethoxysilane, nucleotide, polyaniline, polydopamine and amide.

[0014] Furthermore, the concentration of the RuCl3·3H2O aqueous solution is 0.1–1.5 mg / mL.

[0015] Furthermore, the reaction time is 2–12 hours.

[0016] Furthermore, in step (3), the concentration of the nitrogen-containing organic molecule solution is 1–5 mg / mL.

[0017] Furthermore, in steps (1) and (3), the immersion time is 2 to 24 hours.

[0018] Furthermore, in steps (1), (2) and (3), the drying is vacuum drying, the temperature is 30-90℃, and the drying time is 2-10h.

[0019] A nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst prepared according to the method described above.

[0020] Application of a nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst prepared according to the method in the field of hydrogen evolution by water electrolysis.

[0021] Compared with the prior art, the beneficial effects of the present invention are:

[0022] This invention uses porous nickel foam as a support and modifies the surface of the nickel foam with nitrogen-containing molecules to improve the loading capacity of ruthenium species. Then, using a low-temperature method and leveraging the weak reducing properties of nitrogen-containing molecules, the ruthenium precursor is converted into Ru / RuO2. Further, the electronic structure and morphology of Ru / RuO2 are controlled using nitrogen-containing molecules to prepare an NH2-Ru / RuO2-NH2 / NF heterojunction catalytic electrode with a woven network structure. This electrode utilizes the chelating, strong adhesion, and reducing properties of nitrogen-containing molecules to prepare a Ru / RuO2 heterojunction composite catalyst. The heterostructure not only increases the active sites of the catalyst, but the synergistic effect between the two also improves the stability of the catalyst.

[0023] The catalytic electrode prepared by this invention can drive 1000 mA cm⁻¹ at a low overpotential of 121 mV in the alkaline hydrogen evolution reaction. -2 Hydrogen production by water electrolysis. The preparation method of this invention is simple, the raw materials are readily available, and it is easy to scale up, making it promising for large-scale industrial application. Attached Figure Description

[0024] To further understand and illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required in the embodiments are briefly described below, and constitute a part of the specification. They are used together with the embodiments of the present invention to explain the present invention, but do not constitute a limitation thereof. In the drawings:

[0025] Figure 1This is a SEM image of the NH2-Ru / RuO2-NH2 / NF catalyst;

[0026] Figure 2 This is the XRD pattern of the NH2-Ru / RuO2-NH2 / NF catalyst;

[0027] Figure 3 This is the Raman diagram of the NH2-Ru / RuO2-NH2 / NF catalyst;

[0028] Figure 4 This is the electrochemical performance graph of the hydrogen evolution reaction (linear sweep polarization curve LSV);

[0029] Figure 5 This is a graph (it) showing the stability test results of the hydrogen evolution reaction of the NH2-Ru / RuO2-NH2 / NF catalyst. Detailed Implementation

[0030] The preferred embodiments of the present invention will be described below with reference to the accompanying drawings. It should be understood that the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0031] The present invention discloses a method for preparing a nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst, comprising the following steps:

[0032] (1) The porous nickel foam was immersed in hydrochloric acid solution (3mol / L) to remove impurities. Then the nickel foam was ultrasonically cleaned with acetone, ethanol and deionized water in sequence. After cleaning, it was dried at 40-90℃ to obtain pretreated nickel foam.

[0033] (2) The pretreated nickel foam is immersed in a nitrogen-containing organic molecule solution for 2 to 24 hours and then rinsed repeatedly with deionized water. After that, it is vacuum dried at 30 to 90°C for 2 to 10 hours to obtain an amino-modified nickel foam (NF) electrode, namely the NH2 / NF electrode.

[0034] The concentration of the nitrogen-containing organic molecule solution is 1–10 mg / mL, and the nitrogen-containing organic molecule is one or two of ethylenediamine, disodium ethylenediaminetetraacetate, 3-aminopropyltriethoxysilane, nucleotide, polyaniline, polydopamine, and amide.

[0035] (3) The NH2 / NF electrode prepared in step (2) is placed in a 0.1-1.5 mg / mL RuCl3·3H2O aqueous solution and reacted at a low temperature of 30-120℃ for 2-12 h. Then it is repeatedly rinsed with deionized water and dried under vacuum at 30-90℃ for 2-10 h to obtain the Ru / RuO2-NH2 / NF electrode.

[0036] (4) The Ru / RuO2-NH2 / NF electrode prepared in step (3) is immersed again in a nitrogen-containing organic molecule solution with a concentration of 1-5 mg / mL in step (2) for 2-24 h at room temperature, rinsed repeatedly with deionized water, and vacuum dried at 30-90 °C for 2-10 h to obtain the NH2-Ru / RuO2-NH2 / NF electrode, which is the Ru / RuO2 composite catalyst regulated by nitrogen molecules.

[0037] The vacuum drying time in steps (1), (2) and (3) is 2 to 10 hours, and the vacuum drying temperature is 30 to 90°C.

[0038] The NH2-Ru / RuO2-NH2 / NF electrode prepared by this invention is a self-supporting Ru / RuO2 heterostructure electrode that can be used in the field of hydrogen production by water electrolysis, and is especially suitable for the field of hydrogen evolution by high-current water electrolysis.

[0039] The pretreated nickel foam in Examples 1-6 below was all pretreated using the following process:

[0040] Porous nickel foam was immersed in hydrochloric acid solution (3 mol / L) to remove impurities. Then, the nickel foam was ultrasonically cleaned in sequence with acetone, ethanol and deionized water. After cleaning, it was dried at 40-90℃ to obtain pretreated nickel foam.

[0041] Example 1

[0042] This application provides a method for preparing a Ru- or RuO2-containing catalyst using polyaniline as a nitrogen source, the main steps of which are:

[0043] (1) The pretreated nickel foam was immersed in 50 mL of polyaniline solution with a concentration of 2 mg / mL and immersed for 12 h at room temperature. After immersion, the nickel foam was vacuum dried at 50 °C for 4 h to obtain amino-modified nickel foam (NH2-NF-1).

[0044] (2) 10 mL of RuCl3·3H2O (1.0 mg / mL) solution was poured into the reactor, and then the nickel foam (NH2-NF-1) prepared in step (1) was placed in the reactor and subjected to hydrothermal reaction at 120 °C for 6 h. After the hydrothermal reaction was completed, the above NH2-NF-1 was dried in a vacuum chamber at 60 °C for 2 h to obtain the Ru / RuO2 / NH2-NF-1 electrode. Subsequently, the Ru / RuO2 / NH2-NF-1 electrode was immersed in ethylenediamine solution at room temperature for 2 h. Finally, the immersed Ru / RuO2 / NH2-NF-1 was dried in a vacuum chamber at 50 °C for 4 h to obtain the NH2 / Ru / RuO2 / NH2-NF-1 electrode.

[0045] The prepared NH2 / Ru / RuO2 / NH2-NF-1 catalyst was analyzed by scanning electron microscopy (SEM). Figure 1 This is a SEM image of the catalyst from Example 1; as shown. Figure 1 As can be seen, the morphology of NH2 / Ru / RuO2 / NH2-NF-1 consists of a woven network structure. This structure facilitates better electrolyte penetration into the electrode, improves conductivity, and provides high strength and stability.

[0046] Furthermore, the prepared NH2 / Ru / RuO2 / NH2-NF-1 catalyst was analyzed by X-ray diffraction (XRD). Figure 2 This is the XRD pattern of the catalyst in Example 1; from Figure 2 The diffraction peak of Ni (JCPDS card number 04-0850) can be clearly seen, and no other diffraction peaks are observed. This indicates that the polyaniline is amorphous and that Ru and RuO2 are uniformly distributed on the polyaniline coating with a small loading.

[0047] Further Raman spectroscopy analysis was performed on the prepared NH2 / Ru / RuO2 / NH2-NF-1 catalyst. Figure 3 This is the Raman plot of the NH2 / Ru / RuO2 / NH2-NF-1 catalyst; by Figure 3 It can be clearly observed at 500cm -1 The presence of stretching vibrations belonging to Ni-O on both sides confirms the presence of Ni(OH)2 in the composite catalyst.

[0048] Comparative Example 1

[0049] Comparative Example 1 provides a polyaniline-modified nickel foam electrode. Compared with Example 1, the difference is that an amino-modified nickel foam electrode was prepared by electrodeposition. The specific preparation process of Comparative Example 1 is as follows:

[0050] 5.2 g of Na₂SO₄ and 2 mL of aniline were added to 50 mL of deionized water to form a precursor solution, which also served as the electrolyte solution. Pretreated nickel foam was selected as the working electrode, and Pt sheet and Ag / AgCl were used as the counter and reference electrodes, respectively. A constant current density of 2 mA / cm² was applied. -2 Electrodeposition was performed under the specified conditions for 1 hour. After electrodeposition, the above-mentioned nickel foam was vacuum dried at 50°C for 4 hours to obtain the NH2-NF-2 electrode.

[0051] Comparative Example 2

[0052] Comparative Example 2 provides a Ru-based catalyst electrode that is modified with polyaniline by electrodeposition and then introduces Ru through a hydrothermal reaction. Compared with Example 1, a different polyaniline modification method is used, and no secondary amine modification is performed. The specific preparation process of Comparative Example 2 is as follows:

[0053] (1) 5.2 g Na2SO4 and 2 mL aniline were poured into 50 mL deionized water to form a precursor solution. Pretreated nickel foam was selected as the working electrode, and Pt sheet and Ag / AgCl were used as the counter electrode and reference electrode, respectively. The constant current density was 2 mA cm⁻¹. -2 Electrodeposition was performed under the specified conditions for 1 hour. After electrodeposition, the product was washed with water and dried to obtain amino-modified nickel foam (NH2-NF-2).

[0054] (2) Pour 10 mL of RuCl3·3H2O (1.0 mg / mL) solution into the reactor, and then place the nickel foam (NH2-NF-2) prepared in step (1) into the reactor and react at 120 °C for 6 h. After the hydrothermal reaction is completed, place the above NH2-NF-2 in a vacuum oven at 60 °C and dry for 2 h to obtain the Ru / RuO2 / NH2-NF-2 electrode.

[0055] Example 2

[0056] This application provides a method for preparing a Ru- or RuO2-containing catalyst using disodium ethylenediaminetetraacetate as the N source. The main steps are as follows:

[0057] (1) The pretreated nickel foam was immersed in 50 mL of disodium ethylenediaminetetraacetate solution with a concentration of 2 mg / mL and immersed for 12 h at room temperature. After immersion, the nickel foam was vacuum dried at 50 °C for 4 h to obtain NH2-NF-3.

[0058] (2) The dried NH2-NF-3 was placed in 10 mL of RuCl3·3H2O (1 mg / mL) solution and hydrothermally reacted at 120 °C for 12 h. After the hydrothermal reaction was completed, the above-mentioned nickel foam was washed with water and vacuum dried (60 °C; 2 h) to obtain Ru / RuO2 / NH2-NF-3. Subsequently, the Ru / RuO2 / NH2-NF-3 electrode was immersed in disodium ethylenediaminetetraacetate solution at room temperature for 2 h. Finally, the immersed Ru / RuO2 / NH2-NF-3 was placed in a vacuum chamber at 50 °C and dried for 4 h to obtain the NH2 / Ru / RuO2 / NH2-NF-3 electrode.

[0059] Example 3

[0060] (1) The pretreated nickel foam was immersed in a 1 mg / mL solution of 3-aminopropyltriethoxysilane for 24 h and then rinsed repeatedly with deionized water. After that, it was vacuum dried at 70 °C for 4 h to obtain the amino-modified nickel foam (NF) electrode, namely the NH2 / NF-4 electrode.

[0061] (2) The NH2 / NF-4 electrode prepared in step (1) was placed in a 1.5 mg / mL RuCl3·3H2O aqueous solution and reacted at a low temperature of 30 °C for 12 h. Then it was repeatedly rinsed with deionized water and dried under vacuum at 70 °C for 4 h to obtain the Ru / RuO2-NH2 / NF-4 electrode.

[0062] (3) The Ru / RuO2-NH2 / NF-4 electrode prepared in step (1) was immersed again in a 1 mg / mL 3-aminopropyltriethoxysilane solution at room temperature for 2 to 24 h, rinsed repeatedly with deionized water, and dried under vacuum at 50 °C for 6 h to obtain the NH2-Ru / RuO2-NH2 / NF-4 electrode.

[0063] Example 4

[0064] (1) The pretreated nickel foam was immersed in 10 mg / mL amide solution for 2 h and then rinsed repeatedly with deionized water. After that, it was vacuum dried at 50 °C for 8 h to obtain the amino-modified nickel foam (NF) electrode, namely NH2 / NF-5 electrode.

[0065] (2) The NH2 / NF-5 electrode prepared in step (1) was placed in a 0.1 mg / mL RuCl3·3H2O aqueous solution and reacted at 120 °C for 2 h. Then it was repeatedly rinsed with deionized water and dried under vacuum at 50 °C for 8 h to obtain the Ru / RuO2-NH2 / NF-5 electrode.

[0066] (3) The Ru / RuO2-NH2 / NF-5 electrode prepared in step (2) was immersed again in an amide solution of 5 mg / mL at room temperature for 2 to 24 h, rinsed repeatedly with deionized water, and dried under vacuum at 40 °C for 9 h to obtain the NH2-Ru / RuO2-NH2 / NF-5 electrode.

[0067] Example 5

[0068] (1) The pretreated nickel foam was immersed in 50 mL of polydopamine solution with a concentration of 2 mg / mL and immersed for 12 h at room temperature. After immersion, the nickel foam was vacuum dried at 50 °C for 4 h to obtain an amino-modified NH2 / NF-6 electrode.

[0069] (2) The NH2 / NF-6 electrode prepared in step (1) was placed in a 0.5 mg / mL RuCl3·3H2O aqueous solution and reacted at a low temperature of 50 °C for 8 h. Then it was repeatedly rinsed with deionized water and dried under vacuum at 30 °C for 10 h to obtain the Ru / RuO2-NH2 / NF-6 electrode.

[0070] (3) The Ru / RuO2-NH2 / NF-6 electrode prepared in step (2) was placed in a 3 mg / mL polydopamine solution at room temperature for 2 to 24 h, rinsed repeatedly with deionized water, and vacuum dried at 30 °C for 10 h to obtain the NH2-Ru / RuO2-NH2 / NF-6 electrode.

[0071] Example 6

[0072] (1) The pretreated nickel foam was immersed in a mixed solution of nucleotides and amides. The concentration of nucleotides was 3 mg / mL and the concentration of amides was 4 mg / mL. After immersion for 18 h, it was repeatedly rinsed with deionized water and then vacuum dried at 90 °C for 10 h to obtain amino-modified nickel foam (NF) electrode, namely NH2 / NF-7 electrode.

[0073] (2) The NH2 / NF-7 electrode prepared in step (1) was placed in a 1 mg / mL RuCl3·3H2O aqueous solution and reacted at 80°C for 5 h. Then it was repeatedly rinsed with deionized water and dried under vacuum at 90°C for 2 h to obtain the Ru / RuO2-NH2 / NF-7 electrode.

[0074] (3) The Ru / RuO2-NH2 / NF-7 electrode prepared in step (2) was immersed again in a mixed solution of nucleotide and amide at room temperature for 2-24 hours. The concentration of nucleotide was 1 mg / mL and the concentration of amide was 2 mg / mL. After rinsing repeatedly with deionized water, the electrode was dried under vacuum at 90°C for 2 hours to obtain the NH2-Ru / RuO2-NH2 / NF-7 electrode.

[0075] Application Example 1

[0076] In this application example, a conventional three-electrode system was selected to determine the performance of the electrocatalysts prepared in the examples in the hydrogen evolution reaction (HER). Using 1 mol / L KOH solution as the electrolyte, the NH2 / Ru / RuO2 / NH2-NF-1 and NH2 / Ru / RuO2 / NH2-NF-3 electrodes prepared in Examples 1 and 2, the catalysts prepared in Comparative Examples 1 and 2, were used as working electrodes, a carbon rod electrode as the counter electrode, and an Hg / HgO electrode as the reference electrode. The electrochemical performance of the materials was determined using the linear sweep polarization curve (LSV) method, and the stability of the materials was tested using the chronoamperometry method.

[0077] The hydrogen evolution reaction of the material was tested in a 1 mol / L KOH solution. Figure 4 This is the electrochemical performance (LSV) graph of the hydrogen evolution reaction. (Example:) Figure 4 As shown, at 500mA cm -2 and 1000mA cm -2 At current densities of 1000 mA / cm², the NH₂ / Ru / RuO₂ / NH₂-NF₁ catalyst prepared in Example 1 requires overpotentials of only 88 mV and 121 mV, respectively. In contrast, the electrode obtained in Comparative Example 1 requires overpotentials of 1000 mA / cm². -2 The required overpotential at the current density was 552 mV, while the overpotential required for the electrode obtained in Comparative Example 2 was 293 mV. As shown in the figure, the electrocatalytic hydrogen evolution performance of Comparative Example 2, after introducing metallic Ru and RuO2 via a hydrothermal method, was significantly better than that of Comparative Example 1. This indicates that the introduction of Ru species plays a crucial role in the preparation of highly active NH2 / Ru / RuO2 / NH2-NF-1 electrocatalytic materials. In particular, the secondary modification with polyaniline provided more active sites for the hydrogen evolution reaction, achieving a synergistic catalytic effect and greatly improving the electrocatalytic hydrogen evolution performance of Example 1.

[0078] Figure 5 This is a graph (it) showing the hydrogen evolution reaction stability of the NH2 / Ru / RuO2 / NH2-NF-1 catalyst; as shown. Figure 5 As shown, in 1M KOH solution, under constant potential conditions, the NH2 / Ru / RuO2 / NH2-NF-1 catalyst can drive 1000 mAcm. -2 The current density remained stable for 250 hours, and good hydrogen evolution stability was maintained.

[0079] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst, characterized in that, Includes the following steps: (1) Immerse nickel foam in a nitrogen-containing organic molecule solution and dry to obtain an NH2 / NF electrode; (2) The NH2 / NF electrode was placed in RuCl3·3H2O aqueous solution and reacted at 30~120℃. After drying, the Ru / RuO2-NH2 / NF electrode was obtained. (3) The Ru / RuO2-NH2 / NF electrode was immersed in a nitrogen-containing organic molecule solution at room temperature and dried to obtain a nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst; In steps (1) and (3), the nitrogen-containing organic molecules are one or two of ethylenediamine, disodium ethylenediaminetetraacetate, 3-aminopropyltriethoxysilane, polyaniline, and polydopamine.

2. The preparation method of the nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst according to claim 1, characterized in that, The concentration of nitrogen-containing organic molecule solutions is 1~10 mg / mL.

3. The method for preparing the nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst according to claim 1, characterized in that, The concentration of RuCl3·3H2O aqueous solution is 0.1~1.5 mg / mL.

4. The method for preparing the nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst according to claim 1, characterized in that, The reaction time is 2 to 12 hours.

5. The method for preparing the nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst according to claim 1, characterized in that, In step (3), the concentration of the nitrogen-containing organic molecule solution is 1~5 mg / mL.

6. The method for preparing the nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst according to claim 1, characterized in that, In steps (1) and (3), the immersion time is 2 to 24 hours.

7. The method for preparing the nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst according to claim 1, characterized in that, In steps (1), (2) and (3), the drying is vacuum drying, the temperature is 30~90℃, and the drying time is 2~10 h.

8. A nitrogen-containing molecule-controlled Ru / RuO2 composite catalyst prepared by the method according to any one of claims 1-7.

9. The application of a nitrogen-containing molecularly regulated Ru / RuO2 composite catalyst prepared by the method according to any one of claims 1-7 in the field of hydrogen evolution by water electrolysis.

Citation Information

Patent Citations

  • A cobalt / carbon nanotube / ruthenium electrocatalyst, its preparation method and application

    CN114318411B

  • Polymer loaded catalyst electrode in fuel cell and its prepn. method

    CN1564355A