Cuw / steel / cu three-phase material electric contact structure and welding process thereof
By using a CuW/steel/Cu three-phase material electrical contact structure and vacuum brazing process, combined with a vertical groove and interlocking block design, the problems of easy oxidation and instability in welding CuW/steel/Cu materials are solved, achieving high-quality and efficient welding results.
Patent Information
- Application Number
- CN202311800563.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-26
AI Technical Summary
The connection of CuW, steel, and Cu materials is mainly carried out through induction brazing technology. However, this technology is prone to oxidation, which leads to a decline in welding quality, and the welding process is unstable and has low production efficiency.
The electrical contact structure adopts a three-phase material design of CuW/steel/Cu, including a first material ring, a second material ring, and a third material ring. It uses AgCu45-AgCu25 welding wire and welding sheet, and is welded by vacuum brazing process. Combined with the design of vertical groove and interlocking block, the gap between the material rings and the welding temperature are controlled to improve the welding strength.
It effectively solved the problems of low welding strength and welding defects, improved product quality and production efficiency, and achieved stable welding results.
Smart Images

Figure CN117912867B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrical contact technology, specifically to an electrical contact structure made of CuW / steel / Cu three-phase materials and its welding process. Background Technology
[0002] CuW alloy is a pseudo-alloy that combines the high electrical and thermal conductivity of copper with the low expansion, wear resistance, corrosion resistance, and arc erosion resistance of tungsten, making it a primary material for high-voltage contacts. Electrical contacts are crucial components of high-voltage circuit breakers, switchgear, disconnectors, and grounding switches; their performance directly affects the quality and service life of these high-voltage electrical appliances. When they make contact, the circuit is connected; their relative movement can open or close the circuit, or they can maintain the circuit's continuity through rotation or sliding. Vacuum brazing refers to heating the workpiece within a vacuum chamber, primarily used for welding products requiring high quality and easily oxidized materials. Many materials are suitable for vacuum brazing, such as aluminum, aluminum alloys, copper, copper alloys, stainless steel, alloy steel, low-carbon steel, titanium, nickel, and Inconei nickel.
[0003] Currently, the connection of CuW / steel / Cu materials is mainly accomplished through ordinary induction brazing. This method is used to simultaneously heat the weld points in the area. The metal workpiece to be welded (usually copper) is placed inside the induction coil, and a high-frequency alternating current is passed through it to generate an induced electromagnetic field. This field couples to generate an induced electromotive force on the workpiece surface, forming induced eddy currents on the metal surface. The eddy currents generated on the metal surface generate heat, and brazing filler metal is placed at the welding point. Welding is completed when the workpiece reaches the melting temperature of the brazing filler metal.
[0004] Currently, the induction brazing technology used for CuW, steel, and Cu materials is carried out in the atmosphere. The welding process is very prone to oxidation, which leads to a decline in welding quality and the generation of more weld defects. Secondly, the welding process is greatly affected by human factors, resulting in unstable welding quality and low production efficiency. Summary of the Invention
[0005] To address the aforementioned technical problems, this invention provides a CuW / steel / Cu three-phase material electrical contact structure and its welding process.
[0006] The technical solution of the present invention is: a CuW / steel / Cu three-phase material electrical contact structure, including a first material ring, and a second material ring and a third material ring nested on the first material ring from the inside to the outside;
[0007] The first material ring is a copper part; the second material ring is a steel part; the third material ring is a CuW alloy part that has been fully melted and infiltrated, and the welded part of the third material ring has a copper layer left by the melt infiltration.
[0008] The second and third material rings each have annular grooves that are connected to each other and used to place welding wires. The joints of the first, second, and third material rings are filled with welding sheets.
[0009] Furthermore, the thickness of the copper layer is 1 mm.
[0010] Note: Leaving a 1mm thick copper layer will not affect the assembly relationship between the third material ring and the first and second material rings, while improving the welding strength of the welding joints between the third material ring and the first material ring, and between the third material ring and the second material ring.
[0011] Furthermore, the welding wire and welding sheet are selected from AgCu45-AgCu25, and the welding sheet is made into annular shapes with corresponding gaps between the various material rings.
[0012] Note: The welding wire and welding sheet made from the above materials can well meet the welding requirements of the welding parts between the first material ring, the second material ring, and the third material ring. They are made from silver and copper as base materials and processed into wires, strips, or powders of different shapes and specifications. They have excellent process performance, suitable melting point, good wetting and gap-filling ability, and excellent strength, conductivity, and corrosion resistance of the brazing filler metal and brazing seam. They are also easy to process into different shapes, thus meeting the welding requirements of CuW / steel / Cu three-phase material electrical contact structures.
[0013] Furthermore, the fitting clearance between the first material ring, the second material ring, and the third material ring is controlled between 0.05 and 1 mm; the first material ring has a first ring groove that engages with the second material ring and a second ring groove that engages with the third material ring.
[0014] Explanation: Controlling the fit gap between the first material ring, the second material ring, and the third material ring to the above-mentioned range can ensure the welding strength between each material ring, avoid excessive gaps affecting the overall strength of the CuW / steel / Cu three-phase material electrical contact structure, and avoid excessive gaps affecting the welding strength between each material ring, thus preventing incomplete welding and detachment between the material rings.
[0015] Furthermore, the inner welded portion of the second material ring is provided with at least one vertical groove;
[0016] The vertical sink is provided with a plurality of horizontally arranged first grooves at equal intervals; each of the first grooves is provided with a corresponding biting block, and the biting block has a second groove that rotates and engages with the first groove, and adjacent biting blocks are staggered and overlapped with each other.
[0017] The upper end of the bite block located at the annular sink has a triangular protrusion, and a silver pad is provided between the upper end of the bite block and the vertical sink. The triangular protrusion transmits the swing of each bite block through the downward pressure of the welding wire.
[0018] Explanation: By setting up vertical sinkers and interlocking blocks, the weight and pressure of the second material rings can be used to make the interlocking blocks move together. This causes the welding sheet to be pushed by the welding wire, which then enters the gap left after being squeezed. The welding sheet melts and fills the gap between the material rings. Finally, the interlocking blocks are melted from bottom to top. This structural design can greatly improve the welding strength between the material rings. Furthermore, the temperature can be controlled by the melting temperature difference of the interlocking blocks, welding sheets, and welding wires, which can effectively meet our process requirements. It is also easy to operate and can be used for large-scale mass production.
[0019] Furthermore, the width of the vertical sink is 1 / 20 to 1 / 30 of the circumference of the second material ring, and the depth of the vertical sink is 1 / 3 to 1 / 6 of the width of the vertical sink.
[0020] The width of the biting block is equal to the width of the vertical groove, the thickness of the biting block is equal to the depth of the vertical groove, and the length of the biting block is 1 / 5 to 1 / 8 of the height of the second material ring.
[0021] Note: The introduction of vertical grooves and interlocking blocks has a certain impact on the assembly and fit between the second material ring and the first and third material rings. If the vertical groove is too wide, it will increase the internal voids of the weld, while if the width is too narrow, the welding effect will be poor. Similarly, the depth of the vertical groove and the thickness of the interlocking blocks are also affected. If the thickness is too large, it will affect the linkage effect of each interlocking block and easily generate internal voids in the weld, while if the thickness is too small, the welding effect of the vertical groove and interlocking blocks will be poor.
[0022] Furthermore, the length and number of interlocking blocks affect the overall welding effect. If the number of interlocking blocks is too small, the length of each individual interlocking block will be too long, which can easily cause gaps inside the weld. On the other hand, if the number of interlocking blocks is too large, the operation will be cumbersome and difficult, making it unsuitable for mass production. In addition, it will not be conducive to the linkage effect of each interlocking block.
[0023] Furthermore, both the upper and lower ends of the biting block are provided with grooves for interlocking and overlapping with adjacent biting blocks.
[0024] Explanation: The design of the grooves and countersunk holes can improve the linkage efficiency between two adjacent interlocking blocks, thereby facilitating the swing of each interlocking block and enhancing its role in the welding process.
[0025] Furthermore, the interlocking block is selected from AgCu70-AgCu25, and the copper content of the interlocking block is higher than that of the welding wire and welding sheet.
[0026] Note: Generally speaking, the melting point of silver-copper alloys is between 779-1090℃, and the melting point of silver-copper alloys increases with the increase of copper content. Therefore, by adjusting the selection of materials with different silver and copper contents to prepare interlocking blocks, welding wires and welding sheets, we can achieve the welding process of this structure by controlling the temperature in the welding furnace.
[0027] This invention also provides a welding process for a CuW / steel / Cu three-phase material electrical contact structure, which includes the following steps based on the above-mentioned CuW / steel / Cu three-phase material electrical contact structure:
[0028] S1. Prepare the first material ring, the second material ring, and the third material ring. Clean the surfaces and welding surfaces of the first material ring, the second material ring, and the third material ring. Galvanize the welding surface of the second material ring. Prepare welding wire and welding sheet, and make the welding wire and welding sheet into ring shapes with corresponding gaps between each material ring.
[0029] S2. Place the welding pieces in the gaps between the second material ring and the first material ring, the third material ring, and the third material ring, respectively, with the gaps controlled between 0.05-1mm. Place the welding wire in the annular groove formed by the second and third material rings to form a combined workpiece.
[0030] S3. Fix the assembled workpiece with tooling, place it in the welding furnace, and gradually increase the temperature from room temperature to about 750℃. Weld the workpiece at a temperature between 750-850℃.
[0031] Note: The above welding process can effectively solve common problems such as low welding strength and welding defects in the connection process of CuW, steel and Cu three-phase electrical contacts, and can significantly improve the product quality and production efficiency of CuW / steel / Cu three-phase electrical contacts.
[0032] This invention also provides another welding process for a CuW / steel / Cu three-phase material electrical contact structure, based on the above-mentioned CuW / steel / Cu three-phase material electrical contact structure, including the following steps:
[0033] S1. Prepare the first material ring, the second material ring, and the third material ring. Clean the surfaces and welding surfaces of the first material ring, the second material ring, and the third material ring. Galvanize the welding surface of the second material ring. Prepare welding wire and welding sheet, and make the welding wire and welding sheet into ring shapes with corresponding gaps between each material ring.
[0034] S2. A welding piece is attached to the welding surface of the second material ring to assist in fixing the interlocking block. Then the second material ring is placed on the first ring groove, and then the third material ring is placed on the second ring groove. Another welding piece is placed in the gap between the third material ring and the first material ring. Then the welding wire is placed in the annular groove formed by the second material ring and the third material ring to form a combined workpiece.
[0035] S3. Fix the assembled workpiece with tooling, place it in the welding furnace, and pressurize the second material ring. Gradually increase the temperature from room temperature to about 750°C. Then, set the welding temperature according to the melting point of the materials selected for the welding wire, welding sheet and interlocking block, and perform variable temperature welding. The welding temperature setting requirements for the variable temperature welding process are: first melt the welding wire, then melt the welding sheet, and then melt the interlocking block from bottom to top.
[0036] Note: The above welding process can effectively solve common problems such as low welding strength and welding defects in the connection process of CuW, steel and Cu three-phase electrical contacts, and can further enhance the welding strength between the three materials, thereby further improving the product quality of CuW / steel / Cu three-phase electrical contacts.
[0037] The beneficial effects of this invention are:
[0038] (1) The welding structure design of CuW / steel / Cu three-phase material electrical contact provided by the present invention can effectively realize the vacuum brazing process, thereby replacing the ordinary induction brazing, thus solving the problems of low welding strength and welding defects in the connection process of CuW, steel and Cu three-material integrated electrical contacts.
[0039] (2) The present invention provides a welding process for CuW / steel / Cu three-phase electrical contacts. Based on the provided CuW / steel / Cu three-phase electrical contact structure, the welding of the three materials can be achieved through simple process processing, and the product quality and production efficiency are greatly improved. Attached Figure Description
[0040] Figure 1 This is a schematic diagram of the CuW / steel / Cu three-phase material electrical contact structure of the present invention;
[0041] Figure 2 This is a cross-sectional view of the CuW / steel / Cu three-phase material electrical contact structure of the present invention;
[0042] Figure 3 This is a schematic diagram of the assembly structure of the second material ring and the welding sheet in Embodiment 5 of the present invention;
[0043] Figure 4 This is a schematic diagram of the assembly structure of the second material ring and the interlocking block in Embodiment 5 of the present invention;
[0044] Figure 5 This is a schematic diagram of the second material ring structure in Embodiment 5 of the present invention;
[0045] Figure 6 This is a schematic diagram of the bite block assembly structure of Embodiment 5 of the present invention;
[0046] Figure 7 This is a schematic diagram of the bite block structure in Embodiment 5 of the present invention. Figure 1 ;
[0047] Figure 8 This is a schematic diagram of the bite block structure in Embodiment 5 of the present invention. Figure 2 ;
[0048] Figure 9 This is a schematic diagram of the bite block structure in Embodiment 5 of the present invention. Figure 3 ;
[0049] Among them, 1-first material ring, 11-first annular groove, 12-second annular groove, 2-second material ring, 21-vertical sink groove, 22-first locking groove, 3-third material ring, 4-annular sink groove, 5-welding wire, 6-welding sheet, 7-clamping block, 71-second locking groove, 72-triangular protrusion, 73-concave-convex groove. Detailed Implementation
[0050] The present invention will now be described in more detail with reference to specific embodiments, so as to better demonstrate the advantages of the present invention.
[0051] Example 1:
[0052] like Figure 1 and Figure 2 As shown, a CuW / steel / Cu three-phase material electrical contact structure includes a first material ring 1, and a second material ring 2 and a third material ring 3 nested on the first material ring 1 from the inside to the outside;
[0053] The first material ring 1 is a copper part; the second material ring 2 is a steel part; the third material ring 3 is a CuW alloy part that has been completely infiltrated, and the welded part of the third material ring 3 has a copper layer left by infiltration, the thickness of which is 1mm.
[0054] The second material ring 2 and the third material ring 3 each have annular grooves 4 that are connected to each other and used to place welding wire 5. Welding sheets 6 are filled at the joints of the first material ring 1, the second material ring 2 and the third material ring 3.
[0055] The fitting gap between the first material ring 1, the second material ring 2, and the third material ring 3 is controlled at 0.05-1mm; the first material ring 1 has a first ring groove 11 that engages with the second material ring 2 and a second ring groove 12 that engages with the third material ring; the welding wire 5 and the welding sheet 6 are selected from AgCu30, that is, the copper content is 30%, and the welding sheet 6 is made into an annular shape with a corresponding gap between each material ring.
[0056] Example 2:
[0057] This embodiment discloses a welding process for a CuW / steel / Cu three-phase material electrical contact structure, based on the CuW / steel / Cu three-phase material electrical contact structure of Embodiment 1, including the following steps:
[0058] S1. Prepare the first material ring 1, the second material ring 2, and the third material ring 3. Clean the surfaces and welding surfaces of the first material ring 1, the second material ring 2, and the third material ring 3, and galvanize the welding surface of the second material ring 2. Prepare the welding wire 5 and the welding sheet 6, and make the welding wire 5 and the welding sheet 6 into ring shapes with corresponding gaps between each material ring.
[0059] S2. Place the welding sheet 6 in the gap between the second material ring 2 and the first material ring 1 and the third material ring 3, and in the gap between the third material ring 3 and the first material ring 1, respectively. The gap is controlled at 0.05-1mm. Place the welding wire 5 in the annular groove 4 formed by the second material ring 2 and the third material ring 3 to form a combined workpiece.
[0060] S3. Fix the assembled workpiece with tooling, place it in the welding furnace, gradually increase the temperature from room temperature to 750℃, and then weld it at a welding temperature of 830℃.
[0061] Example 3:
[0062] The difference between this embodiment and embodiment 1 is that the welding sheet 6 located in the gap between the second material ring 2 and the first material ring 1 and the third material ring 3 melts sequentially from bottom to top. Specifically, the welding sheet 6 is divided into 3 layers of equal height from bottom to top: AgCu25, AgCu30, and AgCu35; and the welding wire 5 is AgCu45, while the other welding sheet 6 is AgCu30.
[0063] Example 4:
[0064] This embodiment discloses a welding process for a CuW / steel / Cu three-phase material electrical contact structure, based on the CuW / steel / Cu three-phase material electrical contact structure of Embodiment 3, which differs from Embodiment 2 in that:
[0065] In step S3, the assembled workpiece is fixed with tooling, placed in the welding furnace, and the welding wire 5 is pressurized and heated from room temperature to about 750°C. Then, the welding temperature is set according to the melting point of the materials selected for the welding wire 5 and the welding sheet 6, and variable temperature welding is performed. First, the welding sheet is melted at 825°C, 835°C and 850°C in sequence, and then the temperature is raised to 880°C to melt the welding wire 5 for welding.
[0066] Example 5:
[0067] The difference between this embodiment and Embodiment 1 is that, Figures 3-9 As shown, the inner welding portion of the second material ring 2 is provided with three vertical grooves 21;
[0068] The vertical groove 21 is provided with a plurality of horizontally arranged first grooves 22 at equal intervals; each of the first grooves 22 is provided with a corresponding biting block 7, and the biting block 7 has a second groove 71 that rotates and engages with the first groove 22, and two adjacent biting blocks 7 are staggered and overlapped with each other; both the upper and lower ends of the biting block 7 are provided with concave and convex grooves 73 for staggered and overlapped with adjacent biting blocks 7.
[0069] The upper end of the bite block 7 located at the annular sink 4 has a triangular protrusion 72, and a silver pad is provided between the upper end of the bite block 7 and the vertical sink 21. The triangular protrusion 72 transmits the swing of each bite block 7 through the downward pressure of the welding wire 5.
[0070] The width of the vertical sink 21 is 1 / 25 of the circumference of the second material ring 2, and the depth of the vertical sink 21 is 1 / 4 of the width of the vertical sink 21.
[0071] The width of the biting block 7 is equal to the width of the vertical groove 21, the thickness of the biting block 7 is equal to the depth of the vertical groove 21, and the length of the biting block 7 is 1 / 6 of the height of the second material ring 2, that is, there are 6 biting blocks 7; the biting blocks 7 are selected sequentially from AgCu70, AgCu65, AgCu60, AgCu55, AgCu50, and AgCu45, and the welding wire 5 is AgCu25 and the welding sheet 6 is AgCu30.
[0072] Example 6:
[0073] This embodiment discloses a welding process for a CuW / steel / Cu three-phase material electrical contact structure, based on the CuW / steel / Cu three-phase material electrical contact structure of Embodiment 5, which differs from Embodiment 2 in that:
[0074] In step S2, a welding piece 6 is attached to the welding surface of the second material ring 2 to assist in fixing the interlocking block 7. Then, the second material ring 2 is placed on the first annular groove 11, and then the third material ring 3 is placed on the second annular groove 12. Another welding piece is placed in the gap between the third material ring 3 and the first material ring 1. Then, the welding wire 5 is placed in the annular groove 4 formed by the second material ring 2 and the third material ring 3 to form a combined workpiece.
[0075] In step S3, the assembled workpiece is fixed with tooling and placed in a welding furnace. The second material ring 2 is pressurized and the temperature is gradually increased from room temperature to about 750°C. Then, the welding temperature is set according to the melting point of the materials selected for the welding wire 5, welding sheet 6 and interlocking block 7, and variable temperature welding is performed. First, the welding wire 5 is melted at 825°C, then the temperature is increased to 835°C to melt the welding sheet 6. After that, the temperature is successively increased to 880°C, 890°C, 900°C, 910°C, 920°C and 930°C to melt the interlocking block 7 from bottom to top, and welding is performed.
[0076] Example 7:
[0077] The difference between this embodiment and embodiment 5 is that the width of the vertical sink 21 is 1 / 20 of the circumference of the second material ring 2, and the depth of the vertical sink 21 is 1 / 6 of the width of the vertical sink 21.
[0078] The width of the interlocking block 7 is equal to the width of the vertical groove 21, the thickness of the interlocking block 7 is equal to the depth of the vertical groove 21, and the length of the interlocking block 7 is 1 / 5 of the height of the second material ring 2. The interlocking blocks 7 are selected sequentially from AgCu70, AgCu65, AgCu60, AgCu55, and AgCu50, and the welding wire 5 is AgCu25 and the welding sheet 6 is AgCu30.
[0079] Example 8:
[0080] The difference between this embodiment and embodiment 5 is that the width of the vertical sink 21 is 1 / 30 of the circumference of the second material ring 2, and the depth of the vertical sink 21 is 1 / 6 of the width of the vertical sink 21.
[0081] The width of the interlocking block 7 is equal to the width of the vertical groove 21, the thickness of the interlocking block 7 is equal to the depth of the vertical groove 21, and the length of the interlocking block 7 is 1 / 8 of the height of the second material ring 2. The interlocking blocks 7 are selected sequentially from AgCu70, AgCu65, AgCu60, AgCu55, AgCu50, AgCu45, AgCu40, and AgCu35, and the welding wire 5 is AgCu25 and the welding piece 6 is AgCu30.
[0082] Experimental example:
[0083] To verify the welding process effect of the CuW / steel / Cu three-phase electrical contacts, the welding strength of the CuW / steel / Cu three-phase electrical contacts welded in each embodiment was tested. The second material ring 2 and the first material ring 1 were pulled respectively to test the critical tensile force value at which they broke.
[0084] Meanwhile, Comparison 1 is set up: It is basically the same as Example 5, except that the inner welding part of the second material ring 2 is provided with a vertical groove 21;
[0085] Setting Comparison 2: It is basically the same as Example 5, except that the inner welding part of the second material ring 2 is provided with six vertical grooves 21;
[0086] The results are shown in Table 1 below:
[0087] Table 1 Welding strength test of CuW / steel / Cu three-phase electrical contacts
[0088] Group Example 1 Example 3 Example 5 Example 7 tensile strength 226MPa 230MPa 247MPa 243MPa Group Example 8 Comparison 1 Comparison 2 / tensile strength 246MPa 239MPa 241MPa /
[0089] As can be seen from Table 1 above, comparing Example 1 and Example 3, the layered melting of the welding sheet can improve the welding strength of the CuW / steel / Cu three-phase electrical contact to a certain extent. Example 3 has better welding strength than Example 1.
[0090] Based on Example 3, we tested Example 5. By setting a certain number of vertical grooves on the second material ring, the welding strength of CuW / steel / Cu three-phase electrical contacts can be greatly improved by the action of the interlocking blocks.
[0091] Meanwhile, through comparisons with Examples 7 and 8, Comparison 1 and Comparison 2, and Example 5, it can be seen that changing the number and size of the vertical groove and the interlocking blocks all have a certain impact on the welding process. Among them, the welding effect is the best when the number and size of the vertical groove and the interlocking blocks in Example 5 are used.
Claims
1. A CuW / steel / Cu three-phase material electrical contact structure, characterized in that, It includes a first material ring (1), and a second material ring (2) and a third material ring (3) nested on the first material ring (1) from the inside out; The first material ring (1) is a copper part; the second material ring (2) is a steel part; the third material ring (3) is a CuW alloy part that has been melted and infiltrated, and the welding part of the third material ring (3) has a copper layer left by the melt infiltration. The second material ring (2) and the third material ring (3) each have annular grooves (4) that are connected to each other and used to place welding wire (5). The joints of the first material ring (1), the second material ring (2) and the third material ring (3) are filled with welding pieces (6). The inner welded portion of the second material ring (2) is provided with at least one vertical groove (21); The vertical sink (21) is provided with a plurality of horizontally arranged first grooves (22) at equal intervals; each of the first grooves (22) is provided with a corresponding biting block (7), and the biting block (7) has a second groove (71) that rotates and engages with the first groove (22), and two adjacent biting blocks (7) are staggered and overlapped with each other; The upper end of the bite block (7) located at the annular sink (4) has a triangular protrusion (72), and a silver pad is provided between the upper end of the bite block (7) and the vertical sink (21). The triangular protrusion (72) transmits the swing of each bite block (7) through the downward pressure of the welding wire (5).
2. The CuW / steel / Cu three-phase material electrical contact structure as described in claim 1, characterized in that, The thickness of the copper layer is 1 mm.
3. The CuW / steel / Cu three-phase material electrical contact structure as described in claim 1, characterized in that, The welding wire (5) and welding sheet (6) are selected from AgCu45-AgCu25, and the welding sheet (6) is made into an annular shape with corresponding gaps between the various material rings.
4. The CuW / steel / Cu three-phase material electrical contact structure as described in claim 1, characterized in that, The fitting clearance between the first material ring (1), the second material ring (2), and the third material ring (3) is controlled between 0.05 and 1 mm; The first material ring (1) has a first ring groove (11) that engages with the second material ring (2) and a second ring groove (12) that engages with the third material ring.
5. The CuW / steel / Cu three-phase material electrical contact structure as described in claim 1, characterized in that, The width of the vertical sinking groove (21) is 1 / 20-1 / 30 of the circumference of the second material ring (2), and the depth of the vertical sinking groove (21) is 1 / 3-1 / 6 of the width of the vertical sinking groove (21). The width of the biting block (7) is equal to the width of the vertical groove (21), the thickness of the biting block (7) is equal to the depth of the vertical groove (21), and the length of the biting block (7) is 1 / 5 to 1 / 8 of the height of the second material ring (2).
6. The CuW / steel / Cu three-phase material electrical contact structure as described in claim 1, characterized in that, Both ends of the bite block (7) are provided with grooves (73) for interlocking with adjacent bite blocks (7), and the upper end of the bite block (7) located in the annular groove (4) has a triangular protrusion (72).
7. The CuW / steel / Cu three-phase material electrical contact structure as described in claim 1, characterized in that, The interlocking block (7) is selected from AgCu70-AgCu25, and the copper content of the interlocking block (7) is higher than that of the welding wire (5) and the welding sheet (6).
8. A welding process for a CuW / steel / Cu three-phase material electrical contact structure, characterized in that, A CuW / steel / Cu three-phase electrical contact structure according to any one of claims 1-4 includes the following steps: S1. Prepare the first material ring (1), the second material ring (2), and the third material ring (3). Clean the surfaces and welding surfaces of the first material ring (1), the second material ring (2), and the third material ring (3), and galvanize the welding surface of the second material ring (2). Prepare the welding wire (5) and welding sheet (6), and make the welding wire (5) and welding sheet (6) into ring shapes with corresponding gaps between each material ring. S2. Place the welding piece (6) in the gap between the second material ring (2) and the first material ring (1), the third material ring (3), and the gap between the third material ring (3) and the first material ring (1), respectively. The gap is controlled between 0.05-1mm. Place the welding wire (5) in the annular groove (4) formed by the second material ring (2) and the third material ring (3) to form a combined workpiece. S3. Fix the assembled workpiece with tooling, place it in the welding furnace, gradually increase the temperature from room temperature to 750℃, and perform welding at a welding temperature between 750-850℃.
9. A welding process for a CuW / steel / Cu three-phase material electrical contact structure, characterized in that, A CuW / steel / Cu three-phase electrical contact structure according to any one of claims 5-7 includes the following steps: S1. Prepare the first material ring (1), the second material ring (2), and the third material ring (3). Clean the surfaces and welding surfaces of the first material ring (1), the second material ring (2), and the third material ring (3), and galvanize the welding surface of the second material ring (2). Prepare the welding wire (5) and welding sheet (6), and make the welding wire (5) and welding sheet (6) into ring shapes with corresponding gaps between each material ring. S2. A welding piece (6) is attached to the welding surface of the second material ring (2) to assist in fixing the interlocking block (7). Then the second material ring (2) is placed on the first ring groove (11). Then the third material ring (3) is placed on the second ring groove (12). Another welding piece is placed in the gap between the third material ring (3) and the first material ring (1). Then the welding wire (5) is placed in the annular groove (4) formed by the second material ring (2) and the third material ring (3) to form a combined workpiece. S3. Fix the assembled workpiece with tooling, place it in the welding furnace, and pressurize the second material ring (2) to gradually increase the temperature from room temperature to 750°C. Then, set the welding temperature according to the melting point of the materials selected for the welding wire (5), welding sheet (6) and interlocking block (7), and perform variable temperature welding treatment. The welding temperature setting requirements for the variable temperature welding treatment are: first melt the welding wire (5), then melt the welding sheet (6), and then melt the interlocking block (7) from bottom to top.
Citation Information
Patent Citations
Contact pin and pipe contact, and method for production
CN106104730A
Gas-insulated switch
JP2000311536A