Preparation method of anthracite and boron quantum dot composite negative electrode material
By developing a method for preparing anode materials that combine anthracite and boron quantum dots, the problems of low first-cycle coulombic efficiency and specific capacity of anthracite anode materials have been solved, achieving a significant improvement in electrochemical performance, which is suitable for sodium-ion batteries.
Patent Information
- Application Number
- CN202410259451.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-07
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-03-07
AI Technical Summary
When anthracite is used as the anode material in sodium-ion batteries, the first-cycle coulombic efficiency and specific capacity are relatively low, which affects the electrochemical performance.
A method for preparing anode materials using anthracite and boron quantum dots was adopted. The anthracite was pretreated and mixed with a boron quantum dot solution, then freeze-dried and calcined in a tube furnace. The electron-deficient nature of boron quantum dots was used to increase the charge transfer ability between carbon atoms.
It improves the first-cycle coulombic efficiency and specific capacity of anthracite anode materials, enhances electrochemical performance, and is suitable for large-scale production.
Smart Images

Figure CN117913206B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of rechargeable sodium-ion battery technology, and specifically relates to the negative electrode material of sodium-ion batteries, specifically a method for preparing a negative electrode material composed of anthracite and boron quantum dots. Background Technology
[0002] Limited by factors such as lithium resources, rechargeable sodium-ion batteries are considered the most promising large-scale energy storage devices for the future. The anode material plays a crucial role in the energy storage and release of sodium-ion batteries, significantly influencing their electrochemical performance. my country is a major coal-producing country, and using anthracite to prepare hard carbon as an anode material offers advantages such as abundant supply, low cost, and environmental friendliness. Natural graphite is a commonly used anode material; however, its low-temperature and rate performance as a sodium-ion anode is poor, limiting its application in certain specific fields. Compared to soft carbon, hard carbon has a larger interlayer spacing and contains more defects and micropores, providing more active sites for metallic sodium ions when used as an anode material.
[0003] Currently used commercial hard carbon anode materials mainly suffer from problems such as low first-cycle coulombic efficiency and small storage capacity. Anthracite, as a hard carbon anode material, has an internal disordered structure that is more conducive to sodium ion storage. By doping boron with boron quantum dots, boron replaces carbon atoms in the hexagonal plane in the atomic structure. The increased electron deficiency of boron facilitates charge transfer between nearby carbon atoms, thus improving electrochemical performance. Summary of the Invention
[0004] The purpose of this invention is to solve the problem of low coulombic efficiency in the first cycle when anthracite is used as the negative electrode in sodium-ion batteries, and to provide a novel method for preparing a negative electrode material composed of anthracite and boron quantum dots.
[0005] This invention is achieved through the following technical solution: A method for preparing an anode material composed of anthracite and boron quantum dots includes the following steps: S1. Pre-treated anthracite 1) Mix anthracite and NaOH solution to obtain a mixture; 2) Calcine the mixture in an argon atmosphere; 3) At room temperature, add sulfuric acid solution to the mixture and stir with a magnetic stir bar; 4) Add deionized water and ethanol to the stirred solution and wash repeatedly until the pH value is equal to 7, then filter the solution. 5) The obtained solution is dried in a blower drying oven to finally obtain pretreated anthracite.
[0006] S2. Pretreated anthracite combined with boron quantum dot solution Pretreated anthracite and boron quantum dot solution are mixed, first freeze-dried in a freeze dryer, then calcined and kept warm in a tube furnace, and finally the anthracite and boron quantum dot composite anode material is obtained.
[0007] The boron quantum dot solution can be purchased commercially or prepared as follows: 0.05–0.35 g of boron powder is dispersed in 50 mL of organic solvent and stirred until homogeneous, resulting in 50 mL of a mixed solution containing boron particles. After high-energy ultrasonic disruption, 1.0–9.5 mL of hydrogen peroxide solution and 0.01–0.85 g of boric acid powder are added to obtain a primary product solution. Sodium borohydride is added, and the solution is centrifuged to obtain the boron quantum dot solution. The boron powder is amorphous boron powder, nano-boron, or a mixture of both in any proportion. The organic solvent is isopropanol, tetrahydrofuran, dimethylformamide, or a mixture of these three in any proportion. The high-energy ultrasonic disruption uses a power of 200–1200 W, an ultrasonic time of 2–6 s, an interval of 4–15 s, and a duration of 2–12 h.
[0008] As a preferred technical solution, in step 1) of step S1, the mass ratio of anthracite to NaOH solution is 1:5, and the NaOH solution used is a 60% NaOH solution.
[0009] As a preferred technical solution, in step 2) of step S1, the heating rate during calcination is 5 ℃ / min, the temperature is raised to 700 ℃, and the holding time is 2 h.
[0010] As a preferred technical solution, in step 3) of step S1, the amount of sulfuric acid solution added is calculated as 1 g of anthracite added to 200 mL of sulfuric acid solution, and the sulfuric acid solution used has a concentration of 2 mol·L⁻¹. -1 The sulfuric acid solution was stirred for 24 hours.
[0011] As a preferred technical solution, in step 5) of step S1, the drying temperature is 80 ℃ and the drying time is 8 h.
[0012] As a preferred technical solution, in step S2, the mass ratio of pretreated anthracite and boron quantum dot solution is 1:3~10.
[0013] As a preferred technical solution, in step S2, the mass ratio of pretreated anthracite and boron quantum dot solution is 1:10.
[0014] As a preferred technical solution, in step S2, the freeze-drying time in the freeze dryer is 12 hours.
[0015] As a preferred technical solution, in step S2, the heating rate during calcination in the tube furnace is 5 ℃ / min, the temperature is raised to 900 ℃~1200℃, and the holding time is 0.5 h.
[0016] The method of this invention uses high-temperature annealing to combine anthracite with boron quantum dots, and utilizes the electron-deficient properties of zero-dimensional boron quantum dots to increase the adsorption capacity for sodium ions.
[0017] Compared with the prior art, the beneficial effects of the present invention are as follows: 1) The anthracite-boron quantum dot composite anode material prepared by this invention has high first-cycle coulombic efficiency and specific capacity, which completely solves the problem of low first-cycle coulombic efficiency and specific capacity of traditional anthracite anode materials.
[0018] 2) The negative electrode material prepared by the present invention, which is a composite of anthracite and boron quantum dots, has boron replacing carbon atoms in the hexagonal plane in its atomic structure. The electron deficiency of boron increases, which is beneficial to charge transfer between nearby carbon atoms, thereby greatly improving the electrochemical performance.
[0019] 3) The precursor preparation method and material synthesis method in the present invention are relatively simple, the raw material cost is low, and it is conducive to large-scale production. Attached Figure Description
[0020] The accompanying drawings, which are provided to further illustrate the invention and form part of this application, illustrate exemplary embodiments of the invention and are used to explain the invention, but do not constitute an undue limitation of the invention.
[0021] Figure 1 Scanning electron microscope (SEM) images of the anode materials prepared by the method of this invention under different reaction conditions.
[0022] Figure 2 The XRD patterns are shown for the negative electrode materials prepared by the method of the present invention under different reaction conditions.
[0023] Figure 3 This is a transmission electron microscope (TEM) image of the negative electrode material prepared by the method of this invention. Detailed Implementation
[0024] To enable those skilled in the art to better understand the present invention, the present invention will be further described clearly and completely below with reference to the accompanying drawings and embodiments. It should be noted that, unless otherwise specified, the embodiments and features in the embodiments of this application can be combined with each other. Example 1
[0025] A method for preparing an anode material composed of anthracite and boron quantum dots includes the following steps: S1. Pre-treated anthracite 1) Take 1 g of anthracite and 5 g of 60% NaOH solution and mix them to obtain a mixture.
[0026] 2) The mixture was calcined in an argon atmosphere at a heating rate of 5 °C / min until the temperature reached 700 °C. The temperature was then held for 2 h and removed after cooling to room temperature.
[0027] 3) At room temperature, add 200 mL of a 2 mol·L⁻¹ solution to the mixture. -1 The sulfuric acid solution was stirred with a magnetic stir bar for 24 hours.
[0028] 4) Add deionized water and ethanol to the stirred solution and wash repeatedly until the pH value is equal to 7, then filter the solution.
[0029] 5) The obtained solution was dried in a forced-air drying oven at a temperature of 80 ℃ for 8 h to finally obtain pretreated anthracite.
[0030] S2. Preparation of boron quantum dots 1) Disperse 0.05g of amorphous boron powder in 50mL of organic solvent, stir thoroughly, and then crush it with high-energy ultrasound to obtain a mixed solution containing boron particles. The high-energy ultrasound crushing power is 200W, the ultrasound time is 6s, the interval time is 10s, and the high-energy ultrasound crushing lasts for 10h.
[0031] 2) Add 5.0 mL of hydrogen peroxide solution (30%) and 0.01 g of boric acid powder to the mixed solution one after another. Set the power of the probe-type high-energy ultrasonic crusher to 200 W, the ultrasonic time to 4 s, and the interval time to 4 s. Then crush the mixture with high-energy ultrasonic for 4 h to obtain the initial product solution.
[0032] 3) Add 0.05g of sodium borohydride powder to the initial product solution, and then centrifuge at 3500rpm for 15min to obtain a boron quantum dot solution.
[0033] S3. Pretreated anthracite combined with boron quantum dot solution 100 mg of pretreated anthracite and 300 mg of boron quantum dot solution were mixed and freeze-dried in a freeze dryer for 12 h. Then, the mixture was calcined and held at a temperature of 5 ℃ / min in a tube furnace until the temperature reached 900 ℃. The holding time was 0.5 h. Finally, the negative electrode material composed of anthracite and boron quantum dots was obtained. Example 2
[0034] A method for preparing an anode material composed of anthracite and boron quantum dots includes the following steps: S1. Pre-treated anthracite 1) Take 1 g of anthracite and 5 g of 60% NaOH solution and mix them to obtain a mixture.
[0035] 2) The mixture was calcined in an argon atmosphere at a heating rate of 5 °C / min until the temperature reached 700 °C. The temperature was then held for 2 h and removed after cooling to room temperature.
[0036] 3) At room temperature, add 200 mL of a 2 mol·L⁻¹ solution to the mixture. -1 The sulfuric acid solution was stirred with a magnetic stir bar for 24 hours.
[0037] 4) Add deionized water and ethanol to the stirred solution and wash repeatedly until the pH value is equal to 7, then filter the solution.
[0038] 5) The obtained solution was dried in a forced-air drying oven at a temperature of 80 ℃ for 8 h to finally obtain pretreated anthracite.
[0039] S2. Preparation of boron quantum dots 1) Disperse 0.05g of amorphous boron powder in 50mL of organic solvent, stir thoroughly, and then crush it with high-energy ultrasound to obtain a mixed solution containing boron particles. The high-energy ultrasound crushing power is 200W, the ultrasound time is 6s, the interval time is 10s, and the high-energy ultrasound crushing lasts for 10h.
[0040] 2) Add 5.0 mL of hydrogen peroxide solution (30%) and 0.01 g of boric acid powder to the mixed solution one after another. Set the power of the probe-type high-energy ultrasonic crusher to 200 W, the ultrasonic time to 4 s, and the interval time to 4 s. Then crush the mixture with high-energy ultrasonic for 4 h to obtain the initial product solution.
[0041] 3) Add 0.05g of sodium borohydride powder to the initial product solution, and then centrifuge at 3500rpm for 15min to obtain a boron quantum dot solution.
[0042] S3. Pretreated anthracite combined with boron quantum dot solution 100 mg of pretreated anthracite and 300 mg of boron quantum dot solution were mixed and freeze-dried in a freeze dryer for 12 h. Then, the mixture was calcined and held at a temperature of 5 °C / min in a tube furnace until the temperature reached 1200 °C. The holding time was 0.5 h. Finally, the negative electrode material composed of anthracite and boron quantum dots was obtained. Example 3
[0043] A method for preparing an anode material composed of anthracite and boron quantum dots includes the following steps: S1. Pre-treated anthracite 1) Take 1 g of anthracite and 5 g of 60% NaOH solution and mix them to obtain a mixture.
[0044] 2) The mixture was calcined in an argon atmosphere at a heating rate of 5 °C / min until the temperature reached 700 °C. The temperature was then held for 2 h and removed after cooling to room temperature.
[0045] 3) At room temperature, add 200 mL of a 2 mol·L⁻¹ solution to the mixture. -1 The sulfuric acid solution was stirred with a magnetic stir bar for 24 hours.
[0046] 4) Add deionized water and ethanol to the stirred solution and wash repeatedly until the pH value is equal to 7, then filter the solution.
[0047] 5) The obtained solution was dried in a forced-air drying oven at a temperature of 80 ℃ for 8 h to finally obtain pretreated anthracite.
[0048] S2. Preparation of boron quantum dots 1) Disperse 0.05g of amorphous boron powder in 50mL of organic solvent, stir thoroughly, and then crush it with high-energy ultrasound to obtain a mixed solution containing boron particles. The high-energy ultrasound crushing power is 200W, the ultrasound time is 6s, the interval time is 10s, and the high-energy ultrasound crushing lasts for 10h.
[0049] 2) Add 5.0 mL of hydrogen peroxide solution (30%) and 0.01 g of boric acid powder to the mixed solution one after another. Set the power of the probe-type high-energy ultrasonic crusher to 200 W, the ultrasonic time to 4 s, and the interval time to 4 s. Then crush the mixture with high-energy ultrasonic for 4 h to obtain the initial product solution.
[0050] 3) Add 0.05g of sodium borohydride powder to the initial product solution, and then centrifuge at 3500rpm for 15min to obtain a boron quantum dot solution.
[0051] S3. Pretreated anthracite combined with boron quantum dot solution 100 mg of pretreated anthracite and 1 g of boron quantum dot solution were mixed and freeze-dried in a freeze dryer for 12 h. Then, the mixture was calcined and held at a temperature of 5 °C / min in a tube furnace until the temperature reached 1200 °C. The holding time was 0.5 h. Finally, the negative electrode material composed of anthracite and boron quantum dots was obtained. Example 4
[0052] A method for preparing an anode material composed of anthracite and boron quantum dots includes the following steps: S1. Pre-treated anthracite 1) Take 1 g of anthracite and 5 g of 60% NaOH solution and mix them to obtain a mixture.
[0053] 2) The mixture was calcined in an argon atmosphere at a heating rate of 5 °C / min until the temperature reached 700 °C. The temperature was then held for 2 h and removed after cooling to room temperature.
[0054] 3) At room temperature, add 200 mL of a 2 mol·L⁻¹ solution to the mixture. -1 The sulfuric acid solution was stirred with a magnetic stir bar for 24 hours.
[0055] 4) Add deionized water and ethanol to the stirred solution and wash repeatedly until the pH value is equal to 7, then filter the solution.
[0056] 5) The obtained solution was dried in a forced-air drying oven at a temperature of 80 ℃ for 8 h to finally obtain pretreated anthracite.
[0057] S2. Preparation of boron quantum dots 1) Disperse 0.05g of amorphous boron powder in 50mL of organic solvent, stir thoroughly, and then crush it with high-energy ultrasound to obtain a mixed solution containing boron particles. The high-energy ultrasound crushing power is 200W, the ultrasound time is 6s, the interval time is 10s, and the high-energy ultrasound crushing lasts for 10h.
[0058] 2) Add 5.0 mL of hydrogen peroxide solution (30%) and 0.01 g of boric acid powder to the mixed solution one after another. Set the power of the probe-type high-energy ultrasonic crusher to 200 W, the ultrasonic time to 4 s, and the interval time to 4 s. Then crush the mixture with high-energy ultrasonic for 4 h to obtain the initial product solution.
[0059] 3) Add 0.05g of sodium borohydride powder to the initial product solution, and then centrifuge at 3500rpm for 15min to obtain a boron quantum dot solution.
[0060] S3. Pretreated anthracite combined with boron quantum dot solution 100 mg of pretreated anthracite and 2 g of boron quantum dot solution were mixed and freeze-dried in a freeze dryer for 12 h. Then, the mixture was calcined and held at a temperature of 5 °C / min in a tube furnace until the temperature reached 1200 °C. The holding time was 0.5 h. Finally, the negative electrode material composed of anthracite and boron quantum dots was obtained. Example 5
[0061] A method for preparing an anode material composed of anthracite and boron quantum dots includes the following steps: S1. Pre-treated anthracite 1) Take 1 g of anthracite and 5 g of 60% NaOH solution and mix them to obtain a mixture.
[0062] 2) The mixture was calcined in an argon atmosphere at a heating rate of 5 °C / min until the temperature reached 700 °C. The temperature was then held for 2 h and removed after cooling to room temperature.
[0063] 3) At room temperature, add 200 mL of a 2 mol·L⁻¹ solution to the mixture. -1 The sulfuric acid solution was stirred with a magnetic stir bar for 24 hours.
[0064] 4) Add deionized water and ethanol to the stirred solution and wash repeatedly until the pH value is equal to 7, then filter the solution.
[0065] 5) The obtained solution was dried in a forced-air drying oven at a temperature of 80 ℃ for 8 h to finally obtain pretreated anthracite.
[0066] S2. Preparation of boron quantum dots 1) Disperse 0.05g of amorphous boron powder in 50mL of organic solvent, stir thoroughly, and then crush it with high-energy ultrasound to obtain a mixed solution containing boron particles. The high-energy ultrasound crushing power is 200W, the ultrasound time is 6s, the interval time is 10s, and the high-energy ultrasound crushing lasts for 10h.
[0067] 2) Add 5.0 mL of hydrogen peroxide solution (30%) and 0.01 g of boric acid powder to the mixed solution one after another. Set the power of the probe-type high-energy ultrasonic crusher to 200 W, the ultrasonic time to 4 s, and the interval time to 4 s. Then crush the mixture with high-energy ultrasonic for 4 h to obtain the initial product solution.
[0068] 3) Add 0.05g of sodium borohydride powder to the initial product solution, and then centrifuge at 3500rpm for 15min to obtain a boron quantum dot solution.
[0069] S3. Pretreated anthracite combined with boron quantum dot solution 100 mg of pretreated anthracite and 300 mg of boron quantum dot solution were mixed and freeze-dried in a freeze dryer for 12 h. Then, the mixture was calcined and held at a temperature of 5 °C / min in a tube furnace until the temperature reached 1000 °C. The holding time was 0.5 h. Finally, the negative electrode material composed of anthracite and boron quantum dots was obtained.
[0070] Comparative Example 1 A method for preparing an anode material composed of anthracite and boron quantum dots includes the following steps: S1. Pre-treated anthracite 1) Take 1 g of anthracite and 5 g of 60% NaOH solution and mix them to obtain a mixture.
[0071] 2) The mixture was calcined in an argon atmosphere at a heating rate of 5 °C / min until the temperature reached 700 °C. The temperature was then held for 2 h and removed after cooling to room temperature.
[0072] 3) At room temperature, add 200 mL of a 2 mol·L⁻¹ solution to the mixture. -1 The sulfuric acid solution was stirred with a magnetic stir bar for 24 hours.
[0073] 4) Add deionized water and ethanol to the stirred solution and wash repeatedly until the pH value is equal to 7, then filter the solution.
[0074] 5) The obtained solution was dried in a forced-air drying oven at a temperature of 80 ℃ for 8 h to finally obtain pretreated anthracite.
[0075] S2. Pretreatment of anthracite to prepare anode materials Take 100 mg of pretreated anthracite, freeze-dry it in a freeze dryer for 12 h, and then calcine and hold it in a tube furnace. The heating rate during calcine is 5 ℃ / min, the temperature is raised to 900 ℃, and the holding time is 0.5 h. Finally, the negative electrode material composed of anthracite and boron quantum dots is obtained.
[0076] Comparative Example 2 A method for preparing an anode material composed of anthracite and boron quantum dots includes the following steps: S1. Pre-treated anthracite 1) Take 1 g of anthracite and 5 g of 60% NaOH solution and mix them to obtain a mixture.
[0077] 2) The mixture was calcined in an argon atmosphere at a heating rate of 5 °C / min until the temperature reached 700 °C. The temperature was then held for 2 h and removed after cooling to room temperature.
[0078] 3) At room temperature, add 200 mL of a 2 mol·L⁻¹ solution to the mixture. -1 The sulfuric acid solution was stirred with a magnetic stir bar for 24 hours.
[0079] 4) Add deionized water and ethanol to the stirred solution and wash repeatedly until the pH value is equal to 7, then filter the solution.
[0080] 5) The obtained solution was dried in a forced-air drying oven at a temperature of 80 ℃ for 8 h to finally obtain pretreated anthracite.
[0081] S3. Pretreatment of anthracite to prepare anode materials Take 100 mg of pretreated anthracite, freeze-dry it in a freeze dryer for 12 h, and then calcine and hold it in a tube furnace. The heating rate during calcinement is 5 ℃ / min, the temperature is raised to 1200 ℃, and the holding time is 0.5 h. Finally, the negative electrode material composed of anthracite and boron quantum dots is obtained.
[0082] Figure 1 The figures show scanning electron microscope (SEM) images of the negative electrode materials prepared by the method of this invention under different reaction conditions. In the figures, (a) is an SEM image of the negative electrode material prepared by the method of Comparative Example 1, (b) is an SEM image of the negative electrode material prepared by the method of Example 1, (c) is an SEM image of the negative electrode material prepared by the method of Comparative Example 2, and (d) is an SEM image of the negative electrode material prepared by the method of Example 2. As can be seen from the figures, the smoothness of the anthracite surface changes significantly with temperature; as the temperature increases, the smoothness of the anthracite surface increases, indicating that the internal order is increasing.
[0083] Figure 2 The figures show the XRD patterns of the anode materials prepared by the method of the present invention under different reaction conditions. The figures show the XRD patterns of the anode materials prepared by the methods of Example 2 and Comparative Example 2. Two distinct carbon characteristic peaks, 002 and 101, can be seen in the figures.
[0084] Figure 3 The images show transmission electron microscopy (TEM) images of the negative electrode material prepared by the method in Example 2. In the figures, (a) is a TEM image at 10 nm magnification, and (b) is a TEM image at 50 nm magnification. As can be seen from the figures, the anthracite material exhibits obvious lattice fringes with a lattice spacing of approximately 0.27 nm, which is consistent with the results measured by scanning electron microscopy.
[0085] The embodiments described above are merely examples of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention.
Claims
1. A method for preparing a negative electrode material composed of anthracite and boron quantum dots, characterized in that, Includes the following steps: S1. Pre-treated anthracite 1) Mix anthracite and NaOH solution to obtain a mixture; 2) Calcine the mixture in an argon atmosphere; 3) At room temperature, add sulfuric acid solution to the mixture and stir with a magnetic stir bar; 4) Add deionized water and ethanol to the stirred solution and wash repeatedly until the pH value is equal to 7, then filter the solution. 5) The obtained solution is dried in a forced-air drying oven to finally obtain pretreated anthracite; S2. Pretreated anthracite combined with boron quantum dot solution Pretreated anthracite and boron quantum dot solution were mixed, first freeze-dried in a freeze dryer, then calcined and kept warm in a tube furnace, and finally the anthracite and boron quantum dot composite negative electrode material was obtained. The mass ratio of pretreated anthracite to boron quantum dot solution is 1:3~20; The heating rate during calcination in the tube furnace is 5 °C / min, the temperature is raised to 900 °C~1200 °C, and the holding time is 0.5h. The boron quantum dot solution was prepared by the following method: 0.05–0.35 g of boron powder was dispersed in 50 mL of organic solvent and stirred evenly to obtain 50 mL of mixed solution containing boron particles. After high-energy ultrasonic crushing, 1.0–9.5 mL of hydrogen peroxide solution and 0.01–0.85 g of boric acid powder were added to obtain a primary product solution. Sodium borohydride was added, and the solution was centrifuged to obtain the boron quantum dot solution. The boron powder was amorphous boron powder, nano-boron, or a mixture of the two in any proportion. The organic solvent was isopropanol, tetrahydrofuran, dimethylformamide, or a mixture of the three in any proportion. The high-energy ultrasonic crushing power was 200–1200 W, the ultrasonic time was 2–6 s, the interval time was 4–15 s, and the high-energy ultrasonic crushing time was 2–12 h.
2. The method for preparing the negative electrode material composed of anthracite and boron quantum dots according to claim 1, characterized in that: In step S1, step 1), the mass ratio of anthracite to NaOH solution is 1:5, and the NaOH solution used is a 60% NaOH solution.
3. The method for preparing the negative electrode material composed of anthracite and boron quantum dots according to claim 1, characterized in that: In step 2) of step S1, the heating rate during calcination is 5 ℃ / min, the temperature is raised to 700 ℃, and the holding time is 2 h.
4. The method for preparing the negative electrode material composed of anthracite and boron quantum dots according to claim 1, characterized in that: In step S1, step 3), the amount of sulfuric acid solution added is calculated as 1 g of anthracite added to 200 mL of sulfuric acid solution, and the sulfuric acid solution used has a concentration of 2 mol·L⁻¹. -1 The sulfuric acid solution was stirred for 24 hours.
5. The method for preparing the negative electrode material composed of anthracite and boron quantum dots according to claim 1, characterized in that: In step 5 of step S1, the drying temperature is 80 ℃ and the drying time is 8 h.
6. The method for preparing the negative electrode material composed of anthracite and boron quantum dots according to claim 1, characterized in that: In step S2, the mass ratio of pretreated anthracite to boron quantum dot solution is 1:
10.
7. The method for preparing the negative electrode material composed of anthracite and boron quantum dots according to claim 1, characterized in that: In step S2, the freeze-drying time in the freeze dryer is 12 hours.
Citation Information
Patent Citations
Boron quantum dot, and stabilizing treatment method and application thereof
CN111217375A
A preparation method of graphene as well as graphene oxide based on anthracite
US20160347617A1